Manufacturing method of nanometer SWCNT / PAatSiO2 phase change nanocapsule

By using nano SWCNT/PA@SiO2 phase change nanocapsules manufacturing method in phase change microcapsules, the phase change microcapsules are used to generate an inorganic silica shell material and coated with carbon nanotubes. The phase change microcapsules in the prior art are solved The problem of insufficient heat resistance and thermal conductivity of capsules in the field of thermal management has achieved the improvement of high enthalpy and thermal conductivity.

CN118931499AActive Publication Date: 2024-11-12SOUTH CHINA UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410981457.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The application of existing phase-change microcapsules in the fields of thermal management and thermal interfaces is limited by their inability to heat resistance, insufficient thermal conductivity and complex manufacturing processes, and inorganic nanoparticles are difficult to exert nano-domaining effects, resulting in enthalpy and thermal conductivity. decline.

Method used

Using nano SWCNT/PA@SiO2 phase change nanocapsules, the nanoscale inorganic silica shell material is generated through ultrasonic mixing and hydrolysis reaction, and the carbon nanotubes are coated to form a nanoscale where the inorganic shell material and carbon nanotube die work together. Phase change capsules, enhance enthalpy and thermal conductivity.

Benefits of technology

The preparation of nano-scale phase change capsules for inorganic shell materials is realized, the thermal conductivity and enthalpy value are enhanced, the problem of the reduction of enthalpy value after the addition of inorganic materials in the prior art is overcome, and it is suitable for the fields of thermal management and heat storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931499A_ABST
    Figure CN118931499A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a nano SWCNT / PA (polyamide) SiO2 phase change nano capsule. The method comprises the following steps: carrying out ultrasonic uniform mixing treatment on tetraethoxysilane and carbon nanotubes by using an ultrasonic cell crusher to obtain a dispersion liquid A, and carrying out ultrasonic uniform mixing treatment on n-docosane and the dispersion liquid A by using the ultrasonic cell crusher to obtain an oil phase B formed by mixing a shell material prepolymer, a core material phase change material and the carbon nanotubes; uniformly mixing deionized water, absolute ethyl alcohol and a surfactant to obtain a water phase C, adding the oil phase B into the water phase C, and homogenizing to obtain O / W emulsion; and transferring the O / W emulsion into a three-necked flask, adding ammonia water into the three-necked flask, and stirring the solution in the three-necked flask to obtain the WCNT / PA coated SiO2 phase change nanocapsule emulsion. And filtering, washing and drying to obtain the SWCNT / PA coated SiO2 phase change nanocapsule. The invention provides the carbon nanotube core material modified inorganic shell nano phase change capsule, and the capsule has the capacity of increasing the enthalpy value under the action of intermolecular nano confinement due to the nanoscale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of phase change materials, and in particular to a nano SWCNT / PA@SiO 2 Method for manufacturing phase-change nanocapsules. Background Art

[0002] Phase change material is a new type of energy storage material that allows a large amount of latent heat to be stored during the phase change process. Due to this characteristic of phase change materials, phase change materials are widely used in various fields, such as textiles, solar energy, and thermal management. Among various types of phase change materials, solid-liquid phase change materials are widely studied because of their high latent heat. However, since phase change materials will undergo a phase change from solid to liquid during the phase change process, the phase change material will flow, which is prone to leakage and pollution, which limits the application of phase change materials.

[0003] The use of microencapsulation technology to encapsulate solid-liquid phase change materials in a shell to obtain microcapsule-type composite phase change materials can not only more thoroughly avoid the occurrence of liquid phase leakage, but also make the application of solid-liquid phase change materials more flexible. Phase change capsules are divided into large capsules, microcapsules and nanocapsules according to their size, and smaller capsules have a larger specific surface area, which can improve heat transfer. In order to make phase change capsules used in various fields, there are currently various modifications to phase change capsules. The modification method is to add thermal conductive fillers such as nanoparticles, carbon nanotubes and graphene to the shell material or core material. The modification of phase change capsules can further improve the stability and thermal conductivity of phase change microcapsules.

[0004] Currently, the prior art provides a microcapsule phase change material (MPCM) with a carbon nanotube reinforced filler core material modification and a binary core. The MPCM has improved thermal conductivity and an adjustable operating temperature range, which is suitable for various thermal energy storage applications.

[0005] The disadvantages of the above-mentioned microcapsule phase change material (MPCM) include: MPCM uses organic shells as shell materials, and most organic shells are not heat-resistant and flame-retardant; the improvement in thermal performance is not high, and it is difficult to apply in the field of thermal management and thermal interface. Phase change capsule MPCM is at the micron level, is not heat-resistant and has poor thermal conductivity, and the manufacturing method requires the modification of carbon nanotubes in advance, which is a complex process and changes the structure of carbon nanotubes to a certain extent. The enthalpy value of the capsule decreases to a certain extent due to the addition of thermal conductive material.

[0006] The prior art also provides a carbon nanotube (CNT) loaded paraffin phase change material, and a phase change microcapsule material in a poly (melamine-formaldehyde) shell. The disadvantages of the phase change microcapsule material include: the method uses an organic shell as the shell material, the prepared capsule is at the micron level, the added inorganic nanoparticles are difficult to play the role of nano-confinement, and the simple addition of inorganic nanoparticles reduces the phase change enthalpy value, and it is impossible to obtain an excellent heat-resistant and high thermal conductivity material and to preserve the enthalpy value performance. The manufacturing method introduces other solvents, which makes the process complicated, and the organic shell has low thermal conductivity, so it is impossible to take into account both the enthalpy value and the thermal conductivity performance. Summary of the invention

[0007] The embodiment of the present invention provides a nano SWCNT / PA@SiO 2 The invention discloses a method for manufacturing phase-change nano capsules, so as to realize the effective preparation of nano phase-change nano capsules with nano-scale inorganic shell materials.

[0008] In order to achieve the above object, the present invention adopts the following technical scheme.

[0009] A method for manufacturing nano SWCNT / PA@SiO2 phase change nanocapsules, comprising:

[0010] Selecting tetraethyl orthosilicate as a shell material prepolymer, weighing tetraethyl orthosilicate and ground carbon nanotubes according to a mass ratio of 1: (0.01-0), using an ultrasonic cell disruptor to perform ultrasonic mixing and uniform treatment on the tetraethyl orthosilicate and the ground carbon nanotubes for a certain period of time at a first set temperature, to obtain a dispersion A formed by combining carbon nanotubes and tetraethyl orthosilicate;

[0011] Selecting n-docosane as the core phase change material, weighing n-docosane according to the mass ratio of ethyl orthosilicate to n-docosane of 2:3, using an ultrasonic cell disruptor to perform ultrasonic mixing and homogenizing treatment on n-docosane and the dispersion A for a certain period of time at a second set temperature to obtain an oil phase B mixed with a shell prepolymer, a core phase change material and carbon nanotubes;

[0012] Weigh deionized water, anhydrous ethanol and a surfactant, wherein the mass ratio of the deionized water, anhydrous ethanol and n-docosane is 14:7:3, and mix the deionized water, anhydrous ethanol and the surfactant at a second set temperature to obtain an aqueous phase C;

[0013] adding the oil phase B to the water phase C at a second set temperature and homogenizing to obtain an O / W emulsion;

[0014] The O / W emulsion is placed in a three-necked flask, and ammonia water is added to the three-necked flask at a volume ratio of 1:54 to deionized water. The solution in the three-necked flask is stirred at a second set temperature, so that the ethyl orthosilicate in the solution is hydrolyzed under alkaline conditions and then reacts to generate silicon dioxide. The silicon dioxide coats n-docosane and the carbon nanotubes remaining in the oil phase to form an inorganic silicon dioxide shell material, thereby obtaining a SWCNT / PA@SiO2 phase change nanocapsule emulsion;

[0015] The SWCNT / PA@SiO 2 The phase change nanocapsule emulsion was filtered, washed and dried in sequence to obtain SWCNT / PA@SiO2 phase change nanocapsules.

[0016] Preferably, the process of producing the ground carbon nanotubes in the method comprises:

[0017] Agate balls and carbon nanotubes were weighed in a ratio of 10:1, the agate balls and carbon nanotubes were mixed and put into a ball mill, and ground in the ball mill for 10 hours to obtain carbon nanotubes with shortened length after grinding.

[0018] Preferably, the first set temperature is 80°C, and the second set temperature is 60°C.

[0019] Preferably, the concentration of the surfactant and the deionized water is 0.013 g / mL.

[0020] Preferably, the surfactant is cetyltrimethylammonium bromide.

[0021] Preferably, the three-necked flask is preheated in an oil bath at 60° C. for 10 min, and the rotation speed of the three-necked flask during stirring is 350 rpm.

[0022] Preferably, the washing is performed by washing with petroleum ether, deionized water and ethanol in turn for 3-4 times, and the drying is performed by drying at room temperature for 24 hours using a culture dish.

[0023] It can be seen from the technical solutions provided by the above embodiments of the present invention that the present invention provides an inorganic shell nano phase change capsule modified with a carbon nanotube core material, which not only makes up for the problem that the organic shell is not heat-resistant and difficult to cooperate with the modified inorganic nanoparticles. And because it is at the nano level, it also has the ability to increase the enthalpy value through the effect of intermolecular nanoconfinement, so that while the thermal conductivity is enhanced, the enthalpy value is also improved, and the overall thermal performance is excellent. It can be applied in the fields of heat storage, thermal management, thermal interface, etc.

[0024] Additional aspects and advantages of the present invention will be given in part in the following description, which will become obvious from the following description, or may be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0026] Figure 1 The present invention provides a nano SWCNT / PA@SiO 2 Process flow chart of the method for manufacturing phase change nanocapsules (carbon nanotube-loaded paraffin-silica-coated);

[0027] Figure 2 The SWCNT / PA@SiO synthesized in Example 4 2 (a) SEM of the complete phase-change nanocapsule, (b, c) SEM of the capsule after crushing Example 3, and (d) TEM spectrum. It can be seen that a complete phase-change nanocapsule was synthesized, and the core material contains carbon nanotubes. Figure (e) is the particle size of Example 3 measured by a nanoparticle size analyzer, and it can be seen that all capsules are at the nanometer level;

[0028] Figure 3 The infrared test spectra of all embodiments show that characteristic peaks corresponding to -CH and CH can be seen in the spectra of C22 and capsules, and characteristic peaks of Si-O-Si can be seen in the capsule samples, indicating that there is no chemical interaction between the components, and also indicating that n-docosane is encapsulated by SiO2, and the phase change nanocapsules are successfully synthesized.

[0029] Figure 4 (a) DSC test graphs of all embodiments, and (b) thermal conductivity test graphs, it can be seen that the enthalpy value and thermal conductivity are improved to a certain extent compared with the phase change nanocapsules without carbon nanotubes in Example 2.

[0030] Figure 5 (a) infrared imaging diagram and (b) temperature change diagram of all embodiments. Heat is transferred from the bottom to the top. In the early stage of temperature rise, samples with higher enthalpy values ​​can absorb more heat, so the temperature rises more slowly. Among the samples, the temperature rise of embodiment 3 is the slowest, which matches its enthalpy performance. When the overall temperature exceeds about 45°C, samples with higher thermal conductivity can conduct heat faster, so the temperature rises faster. Figure 5 As shown in , it matches the thermal conductivity;

[0031] Figure 6 This is a statistical diagram of particle sizes obtained by testing with a nanoparticle size analyzer for all embodiments. DETAILED DESCRIPTION

[0032] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention.

[0033] It will be understood by those skilled in the art that, unless expressly stated, the singular forms "one", "said", and "the" used herein may also include plural forms. It should be further understood that the term "comprising" used in the specification of the present invention refers to the presence of the features, integers, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof. It should be understood that when we refer to an element as being "connected" or "coupled" to another element, it may be directly connected or coupled to the other element, or there may be intermediate elements. In addition, the "connection" or "coupling" used herein may include wireless connection or coupling. The term "and / or" used herein includes any unit and all combinations of one or more associated listed items.

[0034] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless defined as herein.

[0035] To facilitate understanding of the embodiments of the present invention, several specific embodiments will be further explained below with reference to the accompanying drawings, and each embodiment does not constitute a limitation on the embodiments of the present invention.

[0036] Embodiment 1

[0037] The embodiment of the present invention provides a nano SWCNT / PA@SiO 2 The process flow of the method for manufacturing phase-change nanocapsules (carbon nanotube-loaded paraffin-silicon dioxide-coated) is as follows: Figure 1 As shown, the steps include:

[0038] Step S1, weighing agate balls and carbon nanotubes according to a ball-to-material ratio of 10:1, wherein the agate balls are used as grinding media, mixing the agate balls and carbon nanotubes and putting them into a ball mill, grinding them in the ball mill for 10 hours, and obtaining carbon nanotubes with shortened lengths after grinding. The amount of carbon nanotubes added is determined by the capacity of the ball mill. The larger the ball-to-material ratio, the better the grinding effect obtained, and the shorter the length of the carbon nanotubes.

[0039] Step S2, selecting tetraethyl orthosilicate as a shell material prepolymer, weighing tetraethyl orthosilicate and ground carbon nanotubes according to a mass ratio of 1: (0.01-0), mixing tetraethyl orthosilicate and ground carbon nanotubes and putting them into an ultrasonic cell disruptor, using the ultrasonic cell disruptor to perform ultrasonic mixing and uniform treatment of tetraethyl orthosilicate and ground carbon nanotubes at 80° C. for a certain time, obtaining a stable dispersion A formed by combining carbon nanotubes and tetraethyl orthosilicate, thereby introducing carbon nanotubes into the oil phase through tetraethyl orthosilicate. The above-mentioned certain time can be several hours, so that the carbon nanotubes and tetraethyl orthosilicate are fully combined and stabilized.

[0040] Step S3, select n-docosane (i.e. paraffin) as the core phase change material. Weigh n-docosane according to the mass ratio of ethyl orthosilicate to n-docosane of 2:3, mix n-docosane with dispersion A and put it into an ultrasonic cell disruptor, perform ultrasonic mixing and uniform treatment on n-docosane and dispersion A at 60°C for a certain period of time, and obtain an oil phase B mixed with shell prepolymer, core phase change material and carbon nanotubes; this step is an important step for the successful synthesis of inorganic shell core modified capsules to tightly combine the modified carbon nanotubes with the oil phase.

[0041] Step S4, weigh deionized water and anhydrous ethanol to n-docosane in a mass ratio of 14:7:3, and also weigh a surfactant and deionized water at a concentration of 0.013 g / mL, and mix the deionized water, anhydrous ethanol and surfactant at 60°C to obtain an aqueous phase C. In this invention, the concentration of the surfactant is about 0.01-0.015 g / ml, and the concentration of surfactant varies with different capsule preparation methods and different types. The more surfactant, the smaller the capsule particle size, but if too much or too little, a stable emulsion cannot be formed.

[0042] The surfactant may be hexadecyltrimethylammonium bromide.

[0043] Step S5, adding the oil phase B to the water phase C at 60° C. and homogenizing to obtain an O / W emulsion;

[0044] Since ethyl orthosilicate is more soluble in ethanol, the ethyl orthosilicate molecules are hydrolyzed and slowly move to the water phase during the process, leaving the carbon nanotubes and paraffin in the oil phase. The homogenization speed of the oil phase B in the water phase C of the method of the present invention is usually 10000 rpm.

[0045] Step S6, transfer the homogenized O / W emulsion to a three-necked flask, use ammonia water as a catalyst, add ammonia water in a volume ratio of 1:54 to deionized water to the three-necked flask, stir the solution in the three-necked flask at 60°C at a speed of 350rpm, and make the solution fully react. The above three-necked flask needs to be preheated in an oil bath at 60°C for 10 minutes to ensure that the emulsion is not destroyed. After adding ammonia water, ethyl orthosilicate is hydrolyzed under alkaline conditions and reacts to form silicon dioxide, which coats n-docosane and carbon nanotubes remaining in the oil phase to form an inorganic silicon dioxide shell material, thereby obtaining a SWCNT / PA@SiO2 phase change nanocapsule emulsion. The shell material of the SWCNT / PA@SiO2 phase change nanocapsule emulsion is silicon dioxide, that is, the SWCNT / PA@SiO2 phase change nanocapsule emulsion has an inorganic shell.

[0046] The carbon nanotubes are interspersed in the core phase change material and contact the silica shell material, forming a heat transfer path inside the capsule to enhance thermal conductivity. At the same time, due to the addition of carbon nanotubes, the structure constrains the activity of the phase change material molecules, making the binding energy of the core phase change material larger, the crystallinity enhanced, and the overall enthalpy value of the capsule increased.

[0047] Step S7, filtering, washing and drying the SWCNT / PA@SiO2 phase change nanocapsule emulsion in sequence to obtain SWCNT / PA@SiO2 phase change nanocapsules.

[0048] The washing is performed by washing with petroleum ether, deionized water and ethanol in turn for 3-4 times. The drying is performed by drying the sample at room temperature for 24 hours using a petri dish.

[0049] The carbon nanotubes added above have hydrophilic groups on their surfaces, and can act as particles in a "Pickering emulsion" to help emulsify the particles, thereby reducing the particle size of the capsules together with the surfactants; however, when there are too many carbon nanotubes, they have the property of agglomeration, which will promote the phase change material to agglomerate with them, forming larger emulsion droplets, resulting in larger capsule size. Therefore, by increasing or decreasing the amount of carbon nanotubes, the SWCNT / PA@SiO 2 The size of phase-change nanocapsules.

[0050] Of course, the homogenization speed and the amount of surfactant are also the main factors that make the capsule size reach the nanometer level. When the homogenization speed reaches a certain level, sufficient shear force can lead to smaller droplets in the emulsion form of phase change capsules; the concentration of surfactant will also affect the emulsion particle size. The appropriate surfactant concentration can ensure that the emulsification process is sufficient and stable, which helps to form a smaller emulsion particle size.

[0051] The method of the present invention controls the amount of carbon nanotubes, the homogenization speed of the oil phase B in the water phase C, and the amount of the surfactant to regulate the SWCNT / PA@SiO 2 The size of the phase-change nanocapsules makes the prepared SWCNT / PA@SiO 2 The size of the phase-change nanocapsules can reach the nanometer level. For example, the present invention adjusts the size of the phase-change capsules by controlling the content of carbon nanotubes. When the ratio of the carbon nanotube content to ethyl orthosilicate is (0.005-0):1, a nanometer-level phase-change capsule can be obtained.

[0052] Different phase change capsule samples were prepared according to different contents of carbon nanotubes. The particle size and performance of the modified capsules obtained were different (particle size diagram was supplemented). The particle sizes ranged from nanometers to micrometers, and the thermal conductivity and enthalpy values ​​were different, but overall they were improved.

[0053] When used in building materials, large-size phase change capsules can provide a more stable and lasting temperature control effect, and are suitable for temperature regulation over a large area. Small-size phase change capsules are suitable for integration into clothing to provide local heat management and comfort, such as sportswear, thermal insulation clothing, etc. Among them, the samples with the best thermal conductivity and enthalpy values ​​are very suitable for use in the field of heat dissipation.

[0054] Embodiment 2:

[0055] Step 1, weighing n-docosane according to the mass ratio of ethyl orthosilicate to n-docosane of 2:3, mixing n-docosane with dispersion A, and also using an ultrasonic cell disruptor to ultrasonically mix them at 60° C. to obtain an oil phase B mixed with a shell material prepolymer, a core material phase change material and carbon nanotubes;

[0056] Step 2, weighing deionized water and anhydrous ethanol to n-docosane in a mass ratio of 14:7:3, and also weighing a surfactant and deionized water at a concentration of 0.013 g / mL, and mixing the deionized water, anhydrous ethanol and surfactant at 60° C. to obtain an aqueous phase C;

[0057] Step 3, at 60° C., adding the oil phase B into the water phase C and homogenizing to obtain an O / W emulsion;

[0058] Step 4, after the homogenized O / W emulsion is transferred to a three-necked flask, ammonia water is added as a catalyst in a volume ratio of 1:54 to deionized water, and stirred at 60°C and 350rpm to fully react to obtain a PA@SiO2 phase change nanocapsule emulsion;

[0059] Step 5: PA@SiO 2 The phase change nanocapsule emulsion was filtered, washed and dried in sequence to obtain PA@SiO2 phase change nanocapsules as a comparison sample.

[0060] Embodiment three:

[0061] Step 1, weighing agate balls and carbon nanotubes in a ball-to-material ratio of 10:1, mixing them, and ball milling them in a ball mill for 10 hours to obtain carbon nanotubes that are cut to short lengths;

[0062] Step 2, weighing tetraethyl orthosilicate and ground carbon nanotubes in a mass ratio of 1:0.0025, and using an ultrasonic cell disruptor to ultrasonically mix at 80° C. to obtain a dispersion A of carbon nanotubes and prepolymer;

[0063] Step 3, weighing n-docosane according to the mass ratio of ethyl orthosilicate to n-docosane of 2:3, mixing n-docosane with dispersion A, and also using an ultrasonic cell disruptor to ultrasonically mix them at 60° C. to obtain an oil phase B mixed with a shell material prepolymer, a core material phase change material and carbon nanotubes;

[0064] Step 4, weighing deionized water and anhydrous ethanol to n-docosane in a mass ratio of 14:7:3, and also weighing a surfactant and deionized water at a concentration of 0.013 g / mL, and mixing the deionized water, anhydrous ethanol and the surfactant at 60° C. to obtain an aqueous phase C;

[0065] Step 5, at 60° C., adding the oil phase B into the water phase C and homogenizing to obtain an O / W emulsion;

[0066] Step 6, after the homogenized O / W emulsion is transferred to a three-necked flask, ammonia water is added as a catalyst in a volume ratio of 1:54 to deionized water, and stirred at 60°C and 350rpm to fully react to obtain SWCNT / PA@SiO2 phase change nanocapsule emulsion;

[0067] Step 7: SWCNT / PA@SiO 2 The phase change nanocapsule emulsion was filtered, washed and dried in sequence to obtain SWCNT / PA@SiO2 phase change nanocapsules.

[0068] Embodiment 4:

[0069] Step 1, weighing agate balls and carbon nanotubes in a ball-to-material ratio of 10:1, mixing them, and ball milling them in a ball mill for 10 hours to obtain carbon nanotubes that are cut to short lengths;

[0070] Step 2, weighing tetraethyl orthosilicate and ground carbon nanotubes in a mass ratio of 1:0.005, and using an ultrasonic cell disruptor to ultrasonically mix at 80° C. to obtain a dispersion A of carbon nanotubes and prepolymers;

[0071] Step 3, weighing n-docosane according to the mass ratio of ethyl orthosilicate to n-docosane of 2:3, mixing it with dispersion A, and also using an ultrasonic cell disruptor to ultrasonically mix them at 60° C. to obtain an oil phase B mixed with a shell material prepolymer, a core material phase change material and carbon nanotubes;

[0072] Step 4, weighing deionized water and anhydrous ethanol to n-docosane in a mass ratio of 14:7:3, and also weighing a surfactant and deionized water at a concentration of 0.013 g / mL, and mixing the deionized water, anhydrous ethanol and surfactant at 60° C. to obtain an aqueous phase C;

[0073] Step 5, at 60° C., adding the oil phase B into the water phase C and homogenizing to obtain an O / W emulsion;

[0074] Step 6, after the homogenized O / W emulsion is transferred to a three-necked flask, ammonia water is added as a catalyst in a volume ratio of 1:54 to deionized water, and stirred at 60°C and 350rpm to fully react to obtain SWCNT / PA@SiO2 phase change nanocapsule emulsion;

[0075] Step 7: SWCNT / PA@SiO 2 The phase change nanocapsule emulsion was filtered, washed and dried in sequence to obtain SWCNT / PA@SiO2 phase change nanocapsules.

[0076] Figure 2 The SWCNT / PA@SiO synthesized in Example 4 2 The (a) SEM of the complete phase-change nanocapsule, and the (b, c) SEM and (d) TEM electron microscope spectra of Example 4 after crushing the capsule show that a complete phase-change nanocapsule has been synthesized, and the core material contains carbon nanotubes. Figure (e) is the particle size of Example 4 measured by a nanoparticle size analyzer, and it can be seen that all capsules are at the nanometer level.

[0077] Embodiment five:

[0078] Step 1, weighing agate balls and carbon nanotubes in a ball-to-material ratio of 10:1, mixing the mixture, and ball milling the mixture in a ball mill for 10 hours to obtain carbon nanotubes that are cut to short lengths;

[0079] Step 2, weighing tetraethyl orthosilicate and ground carbon nanotubes in a mass ratio of 1:0.0075, and using an ultrasonic cell disruptor to ultrasonically mix at 80° C. to obtain a dispersion A of carbon nanotubes and prepolymer;

[0080] Step 3, weighing n-docosane according to the mass ratio of ethyl orthosilicate to n-docosane of 2:3, mixing it with dispersion A, and also using an ultrasonic cell disruptor to ultrasonically mix them at 60° C. to obtain an oil phase B mixed with a shell material prepolymer, a core material phase change material and carbon nanotubes;

[0081] Step 4, weighing deionized water and anhydrous ethanol to n-docosane in a mass ratio of 14:7:3, and also weighing a surfactant and deionized water at a concentration of 0.013 g / mL, and mixing the deionized water, anhydrous ethanol and the surfactant at 60° C. to obtain an aqueous phase C;

[0082] Step 5, at 60° C., adding the oil phase B into the water phase C and homogenizing to obtain an O / W emulsion;

[0083] Step 6, after the homogenized O / W emulsion is transferred to a three-necked flask, ammonia water is added as a catalyst in a volume ratio of 1:54 to deionized water, and stirred at 60°C and 350rpm to fully react to obtain SWCNT / PA@SiO2 phase change nanocapsule emulsion;

[0084] Step 7, filtering, washing and drying the SWCNT / PA@SiO2 phase change nanocapsule emulsion in sequence to obtain SWCNT / PA@SiO2 phase change nanocapsules.

[0085] Embodiment six:

[0086] Step 1, weighing agate balls and carbon nanotubes in a ball-to-material ratio of 10:1, mixing them, and ball milling them in a ball mill for 10 hours to obtain carbon nanotubes that are cut to short lengths;

[0087] Step 2, weighing tetraethyl orthosilicate and ground carbon nanotubes in a mass ratio of 1:0.01, and using an ultrasonic cell disruptor to ultrasonically mix at 80° C. to obtain a dispersion A of carbon nanotubes and prepolymer;

[0088] Step 3, weighing n-docosane according to the mass ratio of ethyl orthosilicate to n-docosane of 2:3, mixing it with dispersion A, and also using an ultrasonic cell disruptor to ultrasonically mix them at 60° C. to obtain an oil phase B mixed with a shell material prepolymer, a core material phase change material and carbon nanotubes;

[0089] Step 4, weighing deionized water and anhydrous ethanol to n-docosane in a mass ratio of 14:7:3, and also weighing a surfactant and deionized water at a concentration of 0.013 g / mL, and mixing the deionized water, anhydrous ethanol and the surfactant at 60° C. to obtain an aqueous phase C;

[0090] Step 5, at 60° C., adding the oil phase B into the water phase C and homogenizing to obtain an O / W emulsion;

[0091] Step 6: After the homogenized O / W emulsion is transferred to a three-necked flask, ammonia water with a volume ratio of 1:54 to deionized water is added as a catalyst, and the mixture is stirred at 60°C and 350 rpm to fully react to obtain SWCNT / PA@SiO 2 Phase change nanocapsule emulsion;

[0092] Step 7, filtering, washing and drying the SWCNT / PA@SiO2 phase change nanocapsule emulsion in sequence to obtain SWCNT / PA@SiO 2 Phase change nanocapsules.

[0093] Those skilled in the art should understand that the above-mentioned values ​​of the ball-to-material ratio and mass ratio are only examples, and other existing or future values ​​of the ball-to-material ratio and mass ratio, if applicable to the embodiments of the present invention, should also be included in the scope of protection of the present invention and are included here by reference.

[0094] Figure 3 For all examples, SWCNT / PA@SiO 2 Infrared test spectrum of phase change nanocapsules, we can see the characteristic peaks corresponding to -CH and CH in the spectra of C22 and capsules, and the characteristic peak of Si-O-Si in the capsule sample, indicating that there is no chemical interaction between the components, and also indicating that n-docosane is SiO 2 The phase change nanocapsules were successfully synthesized.

[0095] Figure 4 (a) DSC test graphs of all embodiments, and (b) thermal conductivity test graphs, it can be seen that the enthalpy value and thermal conductivity are improved to a certain extent compared with the phase change nanocapsules without carbon nanotubes in Example 2.

[0096] Figure 5 (a) infrared imaging diagram and (b) temperature change diagram of all embodiments. Heat is transferred from the bottom to the top. In the early stage of temperature rise, samples with higher enthalpy values ​​can absorb more heat, so the temperature rises more slowly. Among the samples, the temperature of embodiment 4 rises the slowest, which matches its enthalpy performance. When the overall temperature exceeds about 45°C, samples with higher thermal conductivity can conduct heat faster, so the temperature rises faster. Figure 5 As shown in , it matches the thermal conductivity.

[0097] Figure 6 The particle size statistics diagram obtained by the nanoparticle size analyzer of all embodiments are shown. The particle sizes obtained by adding different amounts of carbon nanotubes are different. As the amount of carbon nanotubes increases, the particle size decreases first and then increases (see the specific implementation scheme for the reason), and phase change capsules from nanometer to micrometer levels can be obtained in sequence.

[0098] In summary, the SWCNT / PA@SiO prepared in the embodiment of the present invention 2 Phase change nanocapsules, silica shell materials and modified carbon nanotubes in the core material have a synergistic effect to improve the thermal conductivity and heat transfer performance of the material, and can be well used in fields that require heat storage and heat transfer, such as thermal interfaces and thermal management.

[0099] The core material modified capsule in the present invention is of nanometer level. Currently, there is basically no core material modified phase change capsule of nanometer level, and there is no inorganic shell material modified capsule. The present invention overcomes the difficulty of small material size, which is difficult to modify and difficult to make structure, and combines the carbon nanotube incorporation method into the capsule manufacturing method. The carbon nanotube and shell material prepolymer are ultrasonically improved to improve the compatibility of inorganic nano modified material with oil phase, and other modification reagents and solvents are not introduced, which greatly simplifies the manufacturing method.

[0100] In the present invention, the carbon nanotubes are inserted into the core phase change material and contact the shell material, forming a heat transfer path inside the capsule to enhance thermal conductivity. At the same time, due to the addition of carbon nanotubes, the structure constrains the activity of the phase change material molecules, making their binding energy larger, and the crystallinity enhanced, so that the overall enthalpy value of the capsule is increased. This solves the pain point of the current technology that the addition of inorganic materials actually reduces the enthalpy value, and obtains both excellent thermal conductivity and good enthalpy value.

[0101] Those skilled in the art can understand that the accompanying drawings are only schematic diagrams of an embodiment, and the modules or processes in the accompanying drawings are not necessarily required to implement the present invention.

[0102] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the device or system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment. The device and system embodiments described above are merely schematic, wherein the units described as separate components may or may not be physically separated, and the components displayed as units may or may not be physical units, that is, they may be located in one place, or they may be distributed on multiple network units. Some or all of the modules may be selected according to actual needs to achieve the purpose of the scheme of this embodiment. Ordinary technicians in this field can understand and implement it without paying creative labor.

[0103] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing nano SWCNT / PA@SiO2 phase change nanocapsules, characterized in that: include: Selecting tetraethyl orthosilicate as a shell material prepolymer, weighing tetraethyl orthosilicate and ground carbon nanotubes according to a mass ratio of 1: (0.01-0), using an ultrasonic cell disruptor to perform ultrasonic mixing and uniform treatment on the tetraethyl orthosilicate and the ground carbon nanotubes for a certain period of time at a first set temperature, to obtain a dispersion A formed by combining carbon nanotubes and tetraethyl orthosilicate; Selecting n-docosane as the core phase change material, weighing n-docosane according to the mass ratio of ethyl orthosilicate to n-docosane of 2:3, using an ultrasonic cell disruptor to perform ultrasonic mixing and homogenizing treatment on n-docosane and the dispersion A for a certain period of time at a second set temperature to obtain an oil phase B mixed with a shell prepolymer, a core phase change material and carbon nanotubes; Weigh deionized water, anhydrous ethanol and a surfactant, wherein the mass ratio of the deionized water, anhydrous ethanol and n-docosane is 14:7:3, and mix the deionized water, anhydrous ethanol and the surfactant at a second set temperature to obtain an aqueous phase C; adding the oil phase B to the water phase C at a second set temperature and homogenizing to obtain an O / W emulsion; The O / W emulsion is placed in a three-necked flask, and ammonia water is added to the three-necked flask at a volume ratio of 1:54 to deionized water. The solution in the three-necked flask is stirred at a second set temperature, so that the ethyl orthosilicate in the solution is hydrolyzed under alkaline conditions and then reacts to generate silicon dioxide. The silicon dioxide coats n-docosane and the carbon nanotubes remaining in the oil phase to form an inorganic silicon dioxide shell material, thereby obtaining a SWCNT / PA@SiO2 phase change nanocapsule emulsion; The SWCNT / PA@SiO2 phase change nanocapsule emulsion is filtered, washed and dried in sequence to obtain SWCNT / PA@SiO2 phase change nanocapsules.

2. The method according to claim 1, characterized in that The process of producing the ground carbon nanotubes in the method includes: Agate balls and carbon nanotubes were weighed in a ratio of 10:1 between balls and materials, and the agate balls and carbon nanotubes were mixed and put into a ball mill, and ground in the ball mill for 10 hours to obtain carbon nanotubes with shortened lengths after grinding.

3. The method according to claim 1, characterized in that The first set temperature is 80°C, and the second set temperature is 60°C.

4. The method according to claim 1, characterized in that: The concentration of the surfactant and the deionized water is 0.013 g / mL.

5. The method according to claim 1, characterized in that The surfactant is hexadecyltrimethylammonium bromide.

6. The method according to claim 1, characterized in that The three-necked flask was preheated in an oil bath at 60° C. for 10 min, and the rotation speed of the three-necked flask during stirring was 350 rpm.

7. The method according to claim 1, characterized in that The washing step is to use petroleum ether, deionized water and ethanol for 3-4 times in turn, and the drying step is to use a culture dish for drying at room temperature for 24 hours.

Citation Information

Patent Citations

  • A graphene-silica composite wall material phase change nanocapsule and its preparation method

    CN108774499B

  • Polystyrene foam plastic containing carbon nanotube / ferroferric oxide modified silicon dioxide coated paraffin phase change microcapsules

    CN116444909A

  • Composite phase change material as well as preparation method and application thereof

    CN116970372A

  • Phase Change Materials Core-Mesoporous Silica Shell Organic Inorganic Hybrid Microcapsules and The Manufacturing Method Thereof

    KR102346473B1

  • Phase change material-carbon nanotube-metal substrate composites for thermal storage and control of heat generating devices

    US20170257974A1