Deepwater shallow layer low-temperature wall protecting agent, drilling fluid and application thereof
Through the development of deep-water shallow low-temperature wall protection agent, the cross-linking reaction of low-molecular-weight actives and polyetheramine salts was used to solve the problem of poor stability of shallow well walls in the deep-water oil and natural gas drilling, and the significant improvement of well wall cementation strength was achieved. and mudstone hydration inhibits, reducing the risk of well wall breakage.
Patent Information
- Application Number
- CN202410977601.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
The shallow well walls of marine deep-water oil and natural gas drilling are prone to shattering in low temperature environments. The existing drilling fluid wall protection agent materials lack applicability, resulting in poor stability of the well wall and risk of overflow and blockage.
Develop deep-water shallow low-temperature wall protection agent, through the combination of low-molecular-weight actives, polyetheramine salts and oligosaccharides, the polymerization reaction under alkaline conditions is used to generate cross-linked structures, improve the cementation strength of rocks and inhibit mudstone hydration.
It significantly improves the cementing strength and stability of the well wall, reduces the risk of well wall crushing, and maintains the influence of drilling fluid density and rheology under low temperature conditions.
Smart Images

Figure BDA0004960629730000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of deepwater marine oil and gas drilling, in particular to a deepwater shallow layer low-temperature wall protecting agent, drilling fluid and application thereof. Background Art
[0002] During the drilling operation of deepwater oil and gas exploration and development, two representative strata will be encountered in the shallow strata: sandstone and mudstone. Since the shallow strata are generally under-compacted and weakly cemented, the safe density window for drilling is very narrow, and the rock of the well wall strata is easily broken under the action of external forces. Under the environmental conditions of deepwater shallow gas and deepwater low temperature (deep water usually refers to a water depth of more than 900 meters and a mudline temperature of 2 to 4°C), once the stratum breaks and leaks occur, the shallow gas invasion will bring the risk of overflow blowout and hydrate formation blocking the pipeline, thus bringing great safety hazards to offshore deepwater drilling operations.
[0003] At present, the following measures are usually taken to prevent the instability of the wellbore wall in deep-water shallow formations: (1) strictly control the density of the drilling fluid to avoid excessive density and fracturing the formation; (2) use drilling plugging materials, such as plant fibers and mineral powders, to strengthen the plugging; (3) use some inorganic salts, polymers (such as polyacrylamide) and other inhibitor materials for mudstone hydration. The above technical measures mainly have the following problems: (1) In order to play an effective plugging role, it is necessary to add a sufficient amount of materials (such as calcium carbonate), which will significantly affect the density of the drilling fluid; (2) In addition, drilling plugging agents are mostly inert materials. The plugging layer formed on the wellbore wall is mainly the mechanical accumulation and filling of materials on the pores and cracks on the rock surface. The drilling fluid scouring and drilling up and down can easily destroy the formed plugging layer, and the plugging layer has poor stability; (3) Inorganic salts and polymer inhibitors are mainly used to prevent mudstone hydration, and have limited effect on improving the cementation quality of the plugging layer. The existing chemical wall protective agent materials for drilling fluid are also mainly used for medium and deep formations (formation temperature 80-150°C). From the above, it can be seen that there is currently a lack of wall-stabilizing materials suitable for deep-water shallow formations (low-temperature environments).
[0004] In summary, in order to solve the problem of shallow wellbore stability in deepwater oil and gas drilling in the ocean, it is urgent to develop a deepwater shallow low-temperature wall protective agent material. Summary of the invention
[0005] The invention provides a deep-water shallow-layer low-temperature wall protecting agent, a drilling fluid and applications thereof, which are used to solve the problem of shallow-layer wellbore stability in deep-water petroleum and natural gas drilling in the ocean.
[0006] In view of this, the scheme of the present invention is:
[0007] The first aspect of the present invention provides a deep-water shallow-layer low-temperature wall protective agent, which includes 70 to 90 parts by mass of a low-molecular-weight active substance and 10 to 30 parts of a polyether amine salt; the low-molecular-weight active substance is obtained by polymerization of bisphenol A, oligosaccharides and excess epichlorohydrin under alkaline conditions, and then drying after removing solvents, water and unreacted light components.
[0008] Furthermore, in the polymerization reaction, the molar ratio of epichlorohydrin to bisphenol A is (4.5-10):1; the mass ratio of epichlorohydrin to oligosaccharide is (1-2):1.
[0009] Preferably, the composition of the deep-water shallow-layer low-temperature wall-protecting agent is specifically selected from any one of the following:
[0010] 1) 80 parts of low molecular weight active substances, bisphenol A, epichlorohydrin, and oligosaccharide in a mass ratio of 10:30:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:7.4), and 20 parts of polyetheramine salt;
[0011] 2) 80 parts of low molecular weight active substances, bisphenol A, epichlorohydrin, and oligosaccharide in a mass ratio of 10:40:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:9.9), and 20 parts of polyetheramine salt;
[0012] 3) 80 parts of low molecular weight active substances, bisphenol A, epichlorohydrin, and oligosaccharide in a mass ratio of 15:30:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:4.9), and 20 parts of polyetheramine salt;
[0013] 4) 70 parts of low molecular weight active substances, bisphenol A, epichlorohydrin, and oligosaccharide in a mass ratio of 10:30:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:7.4), and 30 parts of polyetheramine salt;
[0014] 5) 70 parts of low molecular weight active substances, bisphenol A, epichlorohydrin, and oligosaccharide in a mass ratio of 10:40:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:9.9), and 30 parts of polyetheramine salt;
[0015] 6) 70 parts of low molecular weight active substances, bisphenol A, epichlorohydrin, and oligosaccharide in a mass ratio of 15:30:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:4.9), and 30 parts of polyetheramine salt;
[0016] 7) 90 parts of low molecular weight active substances, bisphenol A, epichlorohydrin, and oligosaccharides in a mass ratio of 10:30:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:7.4), and 10 parts of polyetheramine salt;
[0017] 8) 90 parts of low molecular weight active substances, bisphenol A, epichlorohydrin, and oligosaccharide in a mass ratio of 10:40:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:9.9), and 10 parts of polyetheramine salt;
[0018] 9) 90 parts of low molecular weight active substances, bisphenol A, epichlorohydrin and oligosaccharide in a mass ratio of 15:30:30 (wherein the molar ratio of bisphenol A to epichlorohydrin is 1:4.9), and 10 parts of polyether amine salt.
[0019] Preferably, in the polymerization reaction, the alkaline condition is used as a catalytic reaction condition, and preferably an alkaline solution with a molar concentration of 5 to 7 mol / L and an amount of 10% by mass of epichlorohydrin is added.
[0020] Preferably, in the polymerization reaction, the reaction temperature is 70 to 80° C. and the reaction time is 3 to 5 hours.
[0021] Preferably, the solvent used in the polymerization reaction can be a commonly used organic solvent, preferably toluene.
[0022] Furthermore, the oligosaccharide is selected from one or more of oligofructose, oligoxylose and oligochitosan. The oligosaccharide mentioned above refers to a sugar with a small degree of polymerization, preferably a degree of polymerization below 10, that is, the oligosaccharide is preferably a sugar with a degree of polymerization below 10.
[0023] Furthermore, the polyetheramine salt is obtained by neutralizing polyetheramine with acid; the polyetheramine includes one or more of polyether polyamine T403, polyetheramine FL1000 and polyetheramine D230.
[0024] Preferably, the acid is one or more of hydrochloric acid, sulfuric acid, phosphoric acid, formic acid and acetic acid.
[0025] The second aspect of the present invention is to use the deepwater shallow layer low temperature wall protecting agent described in the first aspect in the preparation of deepwater marine oil and gas drilling fluid. The low molecular weight active substance and the slow-release activator polyetheramine salt are mixed according to mass parts and added to the drilling fluid.
[0026] The third aspect of the present invention provides a drilling fluid, comprising the wall protecting agent described in the first aspect above.
[0027] The drilling fluid and its application, the drilling fluid is a deep water synthetic drilling fluid in the art, the main components of which include one or more of water, alkali, weighting agent, coating agent, lubricant, viscosity enhancer, plugging agent and fluid loss reducer.
[0028] In a preferred embodiment, the drilling fluid preparation includes: seawater, Na2CO3, NaOH, filtrate reducer PF-FLOTROL, coating agent PF-PLUS, viscosity enhancer PF-XC, lubricant LUBE168, plugging agent (2000 mesh calcium carbonate), KCl, NaCl and barite.
[0029] The main functions of the main components of the deepwater shallow low-temperature wall protective agent used in the drilling fluid of the present invention are to use bisphenol A, epichlorohydrin and oligosaccharides to prepare low molecular weight active components, wherein bisphenol A and epichlorohydrin are polycondensed under alkaline conditions, the chlorine atoms at the chain ends are combined with the hydrogen atoms on the hydroxyl groups to form HCl and removed, and closed to form new epoxy groups, and the ring opening and closing reactions are repeated, and the new epoxy groups can provide the epoxy groups required for the cross-linking reaction, and the viscosity increasing and steric hindrance effects of the oligosaccharides reduce the reaction activity and speed of bisphenol A and epichlorohydrin, thereby generating low molecular weight active components under experimental conditions. The polyetheramine salt can release amine groups in alkaline drilling fluid, and can react with the active group epoxy group of the low molecular weight active substance LWAS under deep water and low temperature conditions. In this reaction process, the amine group and the epoxy group unite to form an epoxyamine structure, and release a hydroxyl group. The generated epoxyamine structure reacts again with other epoxy groups in the low molecular weight active substance LWAS to form a cross-linked structure. The reaction product contains amine groups, ether bonds, hydroxyl adsorption and electrostatic mutual groups, and also contains a three-dimensional cross-linked structure, thereby achieving the adsorption on the rock surface and the cementation and stabilization of pores. Since the polyetheramine and the reaction product contain amine groups, ether bonds and hydroxyl groups, they also have the function of inhibiting hydration of mudstone. Through the above principles and functions, the deepwater shallow low-temperature wall protective agent composition achieves the purpose of improving the cementation strength of deepwater weakly cemented formation rocks and improving rock stability.
[0030] The fourth aspect of the present invention provides the use of the drilling fluid described in the third aspect in deep-water marine oil and gas drilling.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The wall protecting agent composition provided by the present invention enters into the formation, and because its low molecular weight active substance contains epoxy groups, the activator can release amine groups in the alkaline drilling fluid, and a cross-linking reaction can occur under low temperature conditions, thereby improving the cementing strength of the formation.
[0033] The wall protection agent composition provided by the present invention has a slow-release activator which has a dual effect on well wall stability. On the one hand, the released amine groups react with the epoxy groups in the active substance to generate cross-linking reactions to improve the cementing strength of the formation; on the other hand, the polyetheramine and its salt have multiple amine groups and can be adsorbed on the clay surface at multiple points to effectively prevent the clay from hydrating, thereby solving the well wall stability problem caused by shale hydration.
[0034] The wall protecting agent composition provided by the invention has little influence on the density and rheology of drilling fluid. DETAILED DESCRIPTION
[0035] The technical solution of the present invention will be clearly and completely described below in conjunction with the preferred embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] In the following examples, the oligofructose used was from Jiangsu Tianshun Biotechnology Co., Ltd., the oligoxylose was from Hubei Mingtuo Biotechnology Co., Ltd., and the chitosan was from Henan Lichi Fine Chemical Co., Ltd. The polyetheramines included polyether polyamine T403 from Shandong Pinshang New Materials Co., Ltd., polyetheramine FL1000 from Jinan Jumeihui Chemical Co., Ltd., and polyetheramine D230 from Jinan Shuangying Chemical Co., Ltd.
[0037] Example 1
[0038] Follow the steps below:
[0039] Step 1: In a reaction kettle, 80 parts of toluene solvent, 30 parts of epichlorohydrin, and 10 parts of bisphenol A are added in sequence, wherein the molar ratio of bisphenol A to epichlorohydrin is 1:7.4, and stirred to dissolve, and then 100 parts of 30% mass concentration of oligofructose aqueous solution are added, and heated to 75°C under stirring, and 4 parts of 6.1 mol / L molar concentration of sodium hydroxide solution are slowly added, and the reaction is carried out for 4 hours. After the reaction is completed, the solvent, water and unreacted light components are removed by vacuum evaporation at a temperature of 105-110°C, and the reaction product is dried to obtain a low molecular weight active substance LWAS-1;
[0040] Step 2: First, add 100 parts of polyether polyamine T403 into the reactor, slowly add 10% hydrochloric acid solution under stirring, and pass cooling water through the coil in the reactor to take away the reaction heat, add acid to neutralize until the pH value of the solution is 6.5, and after the reaction is completed, vacuum evaporate at a temperature of 105-110°C to remove water and unreacted light components to obtain a slow-release activator SRA-1;
[0041] Step 3: Add the low molecular weight active substance LWAS-1 described in step 1 and the slow-release activator SRA-1 described in step 2 into the drilling fluid system at a mass ratio of 80:20.
[0042] Example 2
[0043] Follow the steps below:
[0044] Step 1: In a reaction kettle, 80 parts of toluene solvent, 40 parts of epichlorohydrin, and 10 parts of bisphenol A are added in sequence, wherein the molar ratio of bisphenol A to epichlorohydrin is 1:9.9, and stirred to dissolve, and then 100 parts of a 30% mass concentration of oligoxylose aqueous solution are added, and heated to 70°C under stirring, and 4 parts of a 6.1 mol / L molar concentration of sodium hydroxide solution are slowly added, and the reaction is carried out for 5 hours. After the reaction is completed, the solvent, water and unreacted light components are removed by vacuum evaporation at a temperature of 105-110°C, and the reaction product is dried to obtain a low molecular weight active substance LWAS-2;
[0045] Step 2: First, add 50 parts of polyetheramine FL1000 and 50 parts of polyetheramine D230 into a reactor, slowly add a 10% formic acid solution under stirring, and pass cooling water through the coil in the reactor to remove the reaction heat, add acid to neutralize until the pH value of the solution is 7, and after the reaction is completed, vacuum evaporate at a temperature of 105-110°C to remove water and unreacted light components to obtain a slow-release activator SRA-2;
[0046] Step 3: Add the low molecular weight active substance LWAS-2 described in step 1 and the slow-release activator SRA-2 described in step 2 into the drilling fluid system at a mass ratio of 75:25.
[0047] Example 3
[0048] Follow the steps below:
[0049] Step 1: In a reaction kettle, 80 parts of toluene solvent, 30 parts of epichlorohydrin, and 10 parts of bisphenol A are added in sequence, wherein the molar ratio of bisphenol A to epichlorohydrin is 4.9, and stirred to dissolve, and then 100 parts of chitosan aqueous solution with a mass concentration of 30% are added, and heated to 80° C. under stirring, and 4 parts of sodium hydroxide solution with a molar concentration of 6.1 mol / L are slowly added, and the reaction is carried out for 4 hours. After the reaction is completed, the solvent, water and unreacted light components are removed by vacuum evaporation at a temperature of 105-110° C., and the reaction product is dried to obtain a low molecular weight active substance LWAS-3;
[0050] Step 2: First, add 100 parts of polyetheramine D230 into the reactor, slowly add a 10% phosphoric acid solution under stirring, and pass cooling water through the coil in the reactor to remove the reaction heat, add acid to neutralize until the pH value of the solution is 6.8, and after the reaction is completed, vacuum evaporate at a temperature of 105-110°C to remove water and unreacted light components to obtain a slow-release activator SRA-3;
[0051] Step 3: Add the low molecular weight active substance LWAS-3 described in step 1 and the slow-release activator SRA-3 described in step 2 into the drilling fluid system at a mass ratio of 70:30.
[0052] Example 4
[0053] Follow the steps below:
[0054] Step 1: In a reaction kettle, 80 parts of toluene solvent, 30 parts of epichlorohydrin, and 15 parts of bisphenol A are added in sequence, wherein the molar ratio of bisphenol A to epichlorohydrin is 7.4, and stirred to dissolve, and then 100 parts of 30% (mass percentage) oligosaccharide aqueous solution are added, and heated to 72° C. under stirring, and 4 parts of 6.1 mol / L sodium hydroxide solution are slowly added, and the reaction is carried out for 5 hours. After the reaction is completed, the solvent, water and unreacted light components are removed by vacuum evaporation at a temperature of 105-110° C., and the reaction product is dried to obtain a low molecular weight active substance LWAS-4;
[0055] Step 2: In a reactor, first add 40 parts of polyetheramine FL1000, 30 parts of polyetheramine D230, and 30 parts of polyether polyamine T403, slowly add a 10% sulfuric acid solution under stirring, and pass cooling water through the coil in the reactor to take away the reaction heat, add acid to neutralize until the pH value of the solution is 7, and after the reaction is completed, vacuum evaporate at a temperature of 105-110°C to remove water and unreacted light components to obtain a slow-release activator SRA-4;
[0056] Step 3: Add the low molecular weight active substance LWAS-4 described in step 1 and the slow-release activator SRA-4 described in step 2 into the drilling fluid system at a mass ratio of 80:20.
[0057] Comparative Example 1
[0058] The only difference from Example 1 is that bisphenol A is not added in this comparative example.
[0059] Comparative Example 2
[0060] The only difference from Example 1 is that epichlorohydrin is not added in this comparative example.
[0061] Comparative Example 3
[0062] The only difference from Example 1 is that no oligofructose is added in this comparative example.
[0063] Comparative Example 4
[0064] The only difference from Example 1 is that no sustained-release activator is added to this comparative example.
[0065] Experimental example
[0066] The wall protecting agents prepared in each embodiment and the wall protecting agents prepared in the comparative examples are evaluated as follows:
[0067] 1. Instruments for evaluating wall protective agent compositions:
[0068] The instruments used include BC / BD-369GHPT freezer (Haier), GJSS-B12K variable frequency high-speed mixer (Qingdao Haitongda Special Instrument Co., Ltd.), ZNN-D6 six-speed rotational viscometer (Qingdao Haitongda Special Instrument Co., Ltd.), API water loss meter (Qingdao Haitongda Special Instrument Co., Ltd.), GGS71-A high temperature and high pressure water loss meter (Qingdao Haitongda Special Instrument Co., Ltd.), density meter (Qingdao Haitongda Special Instrument Co., Ltd.), bonding strength tester (Hubei Hanke New Technology Co., Ltd.), and precision electronic scale (accuracy 0.01g).
[0069] 2. Formula of base slurry and embodiment:
[0070] Base slurry (blank sample) formula: 400ml seawater + 0.8Na2CO3 + 0.8gNaOH + 4g filtration reducer PF-FLOTROL + 1.2g coating agent PF-PLUS + 0.8g viscosity enhancer PF-XC + 4g lubricant LUBE168 + 10g plugging agent (2000 mesh calcium carbonate) + 20gKCl + 60gNaCl + 58g barite (weighted to 1.200SG).
[0071] Sample slurry formula of the embodiments and comparative examples: base slurry + 20g of wall protecting agent composition.
[0072] 3. Methods for preparing base slurry, sample slurry of embodiments and comparative examples:
[0073] Preparation method of base slurry: measure 400 ml of seawater, pour it into a high-stirring cup, and under stirring at a speed of 10000 r / min, add 0.8 Na2CO3, 0.8 g NaOH, 4 g filtrate reducer PF-FLOTROL, 1.2 g coating agent PF-PLUS, 0.8 g viscosity enhancer PF-XC, 4 g lubricant LUBE168, 10 g plugging agent (2000 mesh calcium carbonate), 20 g KCl, 60 g NaCl, and 58 g barite in sequence, wherein the filtrate reducer, coating agent and viscosity enhancer are all required to be stirred at high speed for 10 minutes after being added before continuing to add other materials. After all the materials are added, stir at high speed for 20 minutes to obtain the base slurry, sample slurry of the embodiment and the comparative example.
[0074] The preparation method of the sample slurry of the embodiment and the comparative example is as follows: 400 ml of seawater is measured and poured into a high-stirring cup, and under the stirring condition of a speed of 10000 r / min, 0.8 Na2CO3, 0.8 g NaOH, 4 g filtrate reducer PF-FLOTROL, 1.2 g coating agent PF-PLUS, 0.8 g viscosity enhancer PF-XC, 4 g lubricant LUBE168, 10 g plugging agent (2000 mesh calcium carbonate), 20 g KCl, 60 g NaCl, 58 g barite, and 20 g wall protective agent composition are added in sequence, wherein after the filtrate reducer, coating agent and viscosity enhancer are added, they are all stirred at high speed for 10 minutes before continuing to add other materials. After all the materials are added, stir at high speed for 20 minutes to obtain the sample slurry of the embodiment and the comparative example.
[0075] 4. Performance test methods of base slurry, sample slurries of embodiments and comparative examples:
[0076] 20 g of the wall protective agent was added to the base slurry of the deepwater drilling fluid system, and stirred for 10 min at a speed of 10000 r / min using a high-speed stirrer. The mixture was fully stirred and mixed to obtain the sample slurries of the embodiment and the comparative example. The apparent viscosity AV and API filtration loss of the sample slurries were measured, and the strength of the simulated rock column was measured.
[0077] Test steps for apparent viscosity AV:
[0078] According to GB / T 16783.1-2014, the evaluation sample was measured at room temperature using a ZNN-D6 six-speed rotation viscometer at 600 rpm, and the reading was multiplied by 0.5 to obtain the apparent viscosity AV value.
[0079] API filtration loss test steps:
[0080] In accordance with GB / T 16783.1-2014, the evaluation sample was tested with an API water loss meter at 0.69 MPa and room temperature for 30 minutes to obtain the API filter loss.
[0081] Density test steps:
[0082] In accordance with GB / T 16783.1-2014, the evaluation sample is tested for density at room temperature using a density meter.
[0083] Bond strength test method:
[0084] ① Take 170g of quartz sand (60-80 mesh) and 30g of low-quality soil, mix them evenly, and use them as simulated rock samples;
[0085] ② Take 40 ml of base slurry or sample slurry of the embodiment and comparative example, mix it thoroughly with the simulated rock sample, put it into the dehydration bucket of the high temperature and high pressure dehydration instrument, stabilize the pressure for 5 minutes under the action of 10 kg pressure, and press it into a rock sample column;
[0086] ③ Pour 300ml of seawater into the water loss bucket of the high-temperature and high-pressure water loss instrument, seal it, install the pressurized pipeline, and slowly pressurize it until liquid flows out of the pressure relief valve at the bottom of the water loss bucket, and immediately close the lower valve stem;
[0087] ④ Pressurize the water loss bucket to 3.5MPa, close the upper valve, and place the water loss bucket with the upper and lower valves sealed in a freezer at a low temperature of 4℃ for 24h;
[0088] ⑤ After the maintenance time is up, carefully depressurize the water loss bucket, disassemble it, and carefully take out the rock sample column;
[0089] ⑥ Use a bond strength tester to measure the bonding strength of the rock sample column and record the experimental data.
[0090] Calculation of bond strength improvement rate:
[0091] Bond strength improvement rate = [(bonding strength of sample slurry - bonding strength of base slurry) / bonding strength of base slurry] × 100%
[0092] The performance test results of the wall protecting agents prepared in Examples 1-4 and Comparative Examples 1-4 are shown in Table 1.
[0093] Table 1: Performance test results of wall protective agents prepared in Examples 1-4 and Comparative Examples 1-4
[0094]
[0095] It can be seen from the data in Table 1 that compared with the base slurry (blank sample slurry), the apparent viscosity AV and density of the sample slurry of the embodiment do not change much, the filtration loss is reduced, the bonding strength is significantly improved, and the bonding strength improvement rate is greater than 300%.
[0096] The specific analysis is as follows:
[0097] (1) The base slurry is a blank sample slurry without wall protection agent, and the bonding strength is 10100Pa, indicating that the bonding of the rock sample column is weak.
[0098] (2) From the evaluation results of the wall protection agent composition of Examples 1 to 4, it can be seen that the apparent viscosity AV and density of Examples 1 to 4 have no obvious changes, and the API filtration loss is reduced; compared with the base slurry, the bonding strength is increased by 3 to 5 times, indicating that the wall protection agent composition prepared by the invention has a very good effect of improving the bonding strength of the rock formation.
[0099] (3) When the wall protection agent compositions of Comparative Examples 1 to 4 were prepared, bisphenol A, epichlorohydrin, oligosaccharide, and polyetheramine were not used; compared with the base slurry, the bonding strength of the rock sample column was not significantly improved, indicating that bisphenol A, epichlorohydrin, oligosaccharide, and polyetheramine salt all had a significant impact on the bonding performance of the wall protection agent composition. In the absence of bisphenol A and epichlorohydrin, low molecular weight active substances LWAS cannot be formed, and in the absence of polyetheramine salt, amine groups cannot be released in alkaline drilling fluids, that is, the lack of the above components significantly affects the cross-linking effect and hydration inhibition functions under deep water and low temperature conditions, thereby leading to a decrease in wall protection performance.
[0100] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. Deep water shallow layer low temperature wall protective agent, characterized in that: The invention comprises 70 to 90 parts of low molecular weight active substances and 10 to 30 parts of polyether amine salts by weight. The low molecular weight active substances are obtained by polymerization reaction of bisphenol A, oligosaccharides and excess epichlorohydrin under alkaline conditions, and then drying after removing solvent, water and unreacted light components.
2. The wall protecting agent according to claim 1, characterized in that In the polymerization reaction, the molar ratio of epichlorohydrin to bisphenol A is (4.5-10):1; the mass ratio of epichlorohydrin to oligosaccharide is (1-2):
1.
3. The wall protecting agent according to claim 2, characterized in that In the polymerization reaction, the alkaline condition is: adding an alkaline solution with a molar concentration of 5 to 7 mol / L and an amount of 10% by mass of epichlorohydrin.
4. The wall protecting agent according to claim 2, characterized in that: In the polymerization reaction, the reaction temperature is 70 to 80° C. and the reaction time is 3 to 5 hours.
5. The wall protecting agent according to claim 1, characterized in that: The oligosaccharide is selected from one or more of fructooligosaccharide, xylooligosaccharide and chitosan.
6. The wall protecting agent according to claim 1, characterized in that: The polyetheramine salt is obtained by neutralizing polyetheramine with acid; the polyetheramine includes one or more of polyether polyamine T403, polyetheramine FL1000 and polyetheramine D230.
7. The wall protecting agent according to claim 6, characterized in that: The acid is one or more of hydrochloric acid, sulfuric acid, phosphoric acid, formic acid and acetic acid.
8. Use of the deepwater shallow layer low-temperature wall protecting agent according to any one of claims 1 to 6 in the preparation of deepwater marine oil and gas drilling fluid.
9. A drilling fluid, characterized in that: The invention comprises the wall protecting agent according to any one of claims 1 to 6.
10. Use of the drilling fluid according to claim 9 in deep-water marine oil and gas drilling.