UV-irradiation-resistant PDLC (Polymer Dispersed Liquid Crystal) composition as well as preparation method and application thereof
A PDLC composition was prepared by using a specific ratio of nematic liquid crystal and photocurable adhesive to form a UV-resistant PDLC film. This solved the yellowing problem of PDLC films when used outdoors and achieved stability and high haze under ultraviolet light, making it suitable for the construction and automotive industries.
Patent Information
- Application Number
- CN202411049982.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-12
AI Technical Summary
Existing polymer-dispersed liquid crystal (PDLC) films cannot withstand strong sunlight and ultraviolet light when used outdoors, and are prone to yellowing, failing to meet the requirements for UV resistance.
A UV-resistant PDLC composition was prepared by using a specific ratio of nematic liquid crystal, photocurable adhesive and spacers, and a PDLC film was formed by photocuring. PET conductive film was used as the substrate to ensure stability under ultraviolet light.
It achieves excellent UV radiation resistance of PDLC film for outdoor use, avoids yellowing, extends service life, and maintains high haze properties, making it suitable for applications such as building glass curtain walls and automotive sunroofs.
Smart Images

Figure BDA0004974635680000011 
Figure BDA0004974635680000021 
Figure BDA0004974635680000022
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional materials and relates to a UV-resistant PDLC composition and a preparation method and application thereof. Background Art
[0002] Polymer dispersed liquid crystals (PDLC) film is a liquid crystal / polymer composite optoelectronic material, and is a functional film material whose optical properties such as transmittance, reflectance or color can be adjusted by electric field, temperature, magnetic field, etc. By adjusting the external electric field and utilizing the different arrangement states of the liquid crystal droplets dispersed inside the polymer, the PDLC film can be switched between the transparent state and the scattering state. It has the advantages of energy saving, environmental protection, privacy protection, safety, sound insulation, and convenient regulation. It can be widely used in partitions, doors, windows, ceilings, and other places such as high-end buildings, banks, insurance companies, hospitals, hotels, restaurants, gold shops, cultural relics showrooms, museums, churches, command centers, etc., and can also be used in car sunroofs.
[0003] PDLC used outdoors needs to be able to withstand strong exposure to sunlight and ultraviolet light to prevent yellowing of PDLC. Currently, many PDLCs cannot meet this requirement.
[0004] Based on this, it is urgent to study a PDLC composition that is resistant to UV radiation. Summary of the invention
[0005] The present invention provides a UV radiation resistant PDLC composition, which has excellent UV radiation resistance and high haze in a foggy state, and provides a method for preparing the PDLC composition, which can be widely used in the fields of building glass curtain walls, automobile skylights or automobile side windows.
[0006] The technical solution of the present invention is achieved in this way:
[0007] In a first aspect, a UV-resistant PDLC composition is provided, wherein the PDLC composition is composed of 35 to 60 parts of a photocurable glue, 40 to 65 parts of a nematic liquid crystal, and 0.1 to 3 parts of a spacer, in parts by mass, wherein the photocurable glue and the nematic liquid crystal total 100 parts;
[0008] The nematic liquid crystal comprises, by mass percentage, 40-60% of component I, 5-20% of component II, 0.5-20% of component III and 5-20% of component IV;
[0009] The structures of components Ⅰ to Ⅳ are as follows:
[0010]
[0011]
[0012] Wherein, R1 to R5 are independently alkyl-C n H 2n+1 or alkoxy-OC n H 2n+1 , wherein n is any integer between 1 and 9; Z1, Z2, and Z3 independently represent a single bond or a -COO-ester bond; A1 to A3 independently represent 1,4-phenylene or 1,4-cyclohexyl; L1 represents -F or alkyl-C n H 2n+1 or -H, wherein n is any integer between 1 and 9; m represents any integer between 0 and 2. Among them, m in components I to IV are independent of each other, and the values of m can be the same or different; similarly, L1 represents an alkyl-C n H 2n+1 When the n value is the same as the alkyl-C n H 2n+1 or alkoxy-OC n H 2n+1 The values of n can be the same or different.
[0013] As an embodiment of the invention, the PDLC composition is composed of 45 to 54 parts of photocurable glue, 46 to 55 parts of nematic liquid crystals and 0.1 to 1 parts of spacers.
[0014] As an embodiment of the invention, the nematic liquid crystal comprises, by mass percentage, 40-60% of component I, 5-20% of component II, 5-20% of component III and 5-20% of component IV.
[0015] The phase transition temperature of the nematic liquid crystal of the present invention is -40 to 150° C., the dielectric anisotropy Δε (20° C., 1 kHz) is ≥5.0, and the optical anisotropy Δn (25° C., 589 nm) is 0.100 to 0.250.
[0016] As an embodiment of the invention, the component I is selected from one or more of the following compounds:
[0017]
[0018]
[0019] As an embodiment of the invention, the component II is selected from one or more of the following compounds:
[0020] As an embodiment of the invention, the component III is selected from one or more of the following compounds:
[0021]
[0022]
[0023] As an embodiment of the invention, the component IV is selected from one or more of the following compounds:
[0024]
[0025] As one embodiment of the invention, the component II is II-7 and / or II-10.
[0026] As an embodiment of the invention, the component III is selected from one or more of III-4, III-5, III-6 and III-8. As an embodiment of the invention, the component IV is selected from one or more of IV-2, IV-7 and IV-10.
[0027] As an embodiment of the invention, the photocurable glue comprises 15-30% acrylate oligomer, 65-80% acrylate diluent, 0.5-5% phosphate modifier and 0.5-3% photoinitiator in terms of mass percentage.
[0028] As an embodiment of the invention, the photocurable glue comprises 20-30% acrylate oligomer, 65-75% acrylate diluent, 0.5-3% phosphate modifier and 0.5-2% photoinitiator in terms of mass percentage.
[0029] As an embodiment of the invention, the particle size of the spacer is 3 to 20 μm, and the material is polystyrene or silicon dioxide;
[0030] As an embodiment of the invention, the particle size of the spacer is 10 to 20 μm.
[0031] As an embodiment of the invention, the acrylate oligomer is selected from one or more of aliphatic urethane acrylate, alicyclic urethane acrylate, aromatic urethane acrylate, polyester acrylate, polyether-modified acrylate and epoxy acrylate;
[0032] As an embodiment of the invention, the acrylate oligomer is aliphatic polyurethane acrylate or alicyclic polyurethane acrylate, wherein the aliphatic polyurethane acrylate is selected from one or more of MU-2305, MU-1204 and MU-2302; the alicyclic polyurethane acrylate is DM9605 and / or DM9603.
[0033] MU-2305, MU-1204 and MU-2302 were purchased from Hemers (Shenzhen) Materials Co., Ltd., and DM9605 and / or DM9603 were purchased from Changzhou Chuangwo New Materials Technology Co., Ltd.
[0034] As an embodiment of the invention, the acrylate diluent is selected from one or more of monofunctional acrylate, monofunctional methacrylate, difunctional acrylate, difunctional methacrylate, multifunctional acrylate and multifunctional methacrylate.
[0035] As an embodiment of the invention, the acrylate diluent is selected from one or more of lauryl acrylate, tetradecyl acrylate, isobornyl acrylate, pentaerythritol tetraacrylate, 1,6-hexanediol diacrylate, hydroxypropyl methacrylate, tetradecyl methacrylate, acryloylmorpholine, dicyclopentenyl acrylate, hexadecyl acrylate, 1,4-butanediol diacrylate, and (ethoxylated) 1,6-hexanediol diacrylate.
[0036] As an embodiment of the invention, the photoinitiator is selected from one or more of photoinitiator TPO, photoinitiator 1173, photoinitiator 651, photoinitiator 907, photoinitiator ITX, photoinitiator MBF, photoinitiator 369, photoinitiator 819, photoinitiator 184, photoinitiator TPO-L, photoinitiator OXE-02, photoinitiator OXE-04 and photoinitiator 2959.
[0037] In a second aspect, a PDLC film prepared from the above-mentioned UV-resistant PDLC composition is provided. The preparation method of the PDLC film comprises: placing the PDLC composition in two PET conductive films, rolling to form a sandwich structure, and then placing it under ultraviolet light for photocuring, wherein the curing temperature is 24-26°C and the curing light intensity is 3-15mw / cm 2 , the curing time is 2-10min; the thickness of the PET conductive film is 188μm, the square resistance is 120-130Ω, the total light transmittance is 80-85%, and the haze is 0.5-1%.
[0038] In a third aspect, there is provided an application of the PDLC film as described in the second aspect in outdoor building curtain walls, automobile skylights or automobile side windows.
[0039] The working principle and beneficial effects of the present invention are:
[0040] The present invention provides a UV-resistant PDLC composition, wherein compounds represented by component I, component II, component III and component IV are added to the nematic liquid crystal used in the composition, thereby synergistically improving the anti-aging performance and effectively extending the application life of the PDLC. The PDLC film is prepared by using the PDLC composition of the present invention, and the obtained product has excellent UV-resistant properties and can be widely used in the fields of building glass curtain walls, automobile sunroofs, automobile side windows, etc. DETAILED DESCRIPTION
[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Preparation Example 1
[0043] The specific formula of the LC1 liquid crystal composition is shown in Table 1.
[0044] Table 1
[0045] Serial number Nematic liquid crystal components content% 1 Ⅰ-1 12.0 2 Ⅰ-8 15.0 3 Ⅰ-7 10.0 4 Ⅳ-7 15.0 5 Ⅱ-7 10.0 6 Ⅰ-4 9.0 7 Ⅰ-6 10.0 9 Ⅱ-10 5.0 10 Ⅲ-5 4.0 11 Ⅲ-6 6.0 12 Ⅲ-8 4.0
[0046] Preparation Example 2
[0047] The specific formula of the LC2 liquid crystal composition is shown in Table 2.
[0048] Table 2
[0049]
[0050]
[0051] Preparation Example 3
[0052] The specific formula of the LC3 liquid crystal composition is shown in Table 3.
[0053] Table 3
[0054] Serial number Nematic liquid crystal components content% 1 Ⅰ-2 15.0 2 Ⅳ-1 10.0 3 Ⅰ-6 15.0 4 Ⅰ-7 10.0 5 Ⅱ-9 5.0 6 Ⅱ-4 10.0 7 Ⅳ-3 10.0 8 Ⅱ-5 5.0 9 Ⅲ-1 5.0 10 Ⅲ-3 5.0 11 Ⅲ-7 10.0
[0055] Preparation Example 4
[0056] The specific formula of the LC4 liquid crystal composition is shown in Table 4.
[0057] Table 4
[0058] Serial number Nematic liquid crystal components content% 1 Ⅱ-6 5 2 Ⅰ-10 15 3 Ⅰ-2 15 4 Ⅲ-3 7 5 Ⅲ-7 8 6 Ⅳ-4 6 7 Ⅰ-8 20 8 Ⅲ-9 5 9 Ⅳ-9 5 10 Ⅰ-4 10 11 Ⅳ-6 4
[0059] Preparation Example 5
[0060] The specific formula of the LC5 liquid crystal composition is shown in Table 5.
[0061] Table 5
[0062]
[0063]
[0064] Preparation Example 6
[0065] The specific formula of the LC6 liquid crystal composition is shown in Table 6.
[0066] Table 6
[0067] Serial number Nematic liquid crystal components content% 1 Ⅰ-1 12.0 2 Ⅰ-8 15.0 3 Ⅰ-7 10.0 4 Ⅳ-7 15.0 5 Ⅱ-7 10.0 6 Ⅰ-4 9.0 7 Ⅰ-6 10.0 9 Ⅱ-10 5.0 10 Ⅲ-3 8.0 11 Ⅲ-7 6.0
[0068] Preparation Example 7
[0069] The specific formula of the LC7 liquid crystal composition is shown in Table 7.
[0070] Table 7
[0071] Serial number Nematic liquid crystal components content% 1 Ⅰ-1 12.0 2 Ⅰ-8 15.0 3 Ⅰ-7 10.0 4 Ⅳ-7 30.0 5 Ⅰ-4 9.0 6 Ⅰ-6 10.0 7 Ⅲ-5 4.0 8 Ⅲ-6 6.0 9 Ⅲ-8 4.0
[0072] Preparation Example 8
[0073] The specific formula of LC8 liquid crystal composition is shown in Table 8.
[0074] Table 8
[0075]
[0076] Preparation Example 9
[0077] The specific formula of the LC9 liquid crystal composition is shown in Table 9.
[0078] Table 9
[0079] Serial number Nematic liquid crystal components content% 1 Ⅰ-1 12.0 2 Ⅰ-8 15.0 3 Ⅰ-7 10.0 4 Ⅳ-7 22.0 5 Ⅱ-7 15.0 6 Ⅰ-4 9.0 7 Ⅰ-6 10.0 9 Ⅱ-10 7.0
[0080] The performance parameters of the above LC1-LC9 liquid crystal compositions are shown in Table 10.
[0081] Table 10
[0082]
[0083] In the following examples and comparative examples, the phosphate modifier was purchased from PM2010SP of Guangzhou Jingde Chemical Materials Co., Ltd. MU-2305, MU-1204 and MU-2302 were purchased from Hemershi (Shenzhen) Materials Co., Ltd., and DM9605 and / or DM9603 were purchased from Chuangwo New Materials
[0084] Example 1
[0085] Table 11
[0086]
[0087]
[0088] After the PDLC composition in Table 11 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 24° C., and the curing light intensity was 5 mw / cm 2 , the curing time is 8min; the thickness of the PET conductive film is 188μm, the square resistance is 122.5Ω, the total light transmittance is 81.5%, and the haze is 0.52%. The UV-resistant PDLC is obtained, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0089] Example 2
[0090] Table 12
[0091]
[0092] After the PDLC composition in Table 12 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 26° C., and the curing light intensity was 3 mw / cm 2 , the curing time is 10min; the thickness of the PET conductive film is 188μm, the square resistance is 120Ω, the total light transmittance is 85%, and the haze is 0.50%. The UV-resistant PDLC is prepared, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0093] Example 3
[0094] Table 13
[0095]
[0096]
[0097] After the PDLC composition in Table 13 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 25° C., and the curing light intensity was 15 mw / cm 2, the curing time is 2min; the thickness of the PET conductive film is 188μm, the square resistance is 130Ω, the total light transmittance is 80%, and the haze is 1.0%. The UV-resistant PDLC is prepared, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0098] Example 4
[0099] Table 14
[0100]
[0101] After the PDLC composition in Table 14 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 24° C., and the curing light intensity was 5 mw / cm 2 , the curing time is 8min; the thickness of the PET conductive film is 188μm, the square resistance is 122.5Ω, the total light transmittance is 81.5%, and the haze is 0.52%. The UV-resistant PDLC is obtained, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0102] Example 5
[0103] Table 15
[0104]
[0105]
[0106] After the PDLC composition in Table 15 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 24° C., and the curing light intensity was 5 mw / cm 2 , the curing time is 8min; the thickness of the PET conductive film is 188μm, the square resistance is 122.5Ω, the total light transmittance is 81.5%, and the haze is 0.52%. The UV-resistant PDLC is obtained, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0107] Example 6
[0108] Table 16
[0109]
[0110] After the PDLC composition in Table 16 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 24° C., and the curing light intensity was 5 mw / cm 2 , the curing time is 8min; the thickness of the PET conductive film is 188μm, the square resistance is 122.5Ω, the total light transmittance is 81.5%, and the haze is 0.52%. The UV-resistant PDLC is obtained, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0111] Comparative Example 1
[0112] Table 17
[0113]
[0114] After the PDLC composition in Table 17 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 24° C., and the curing light intensity was 5 mw / cm 2 , the curing time is 8min; the thickness of the PET conductive film is 188μm, the square resistance is 122.5Ω, the total light transmittance is 81.5%, and the haze is 0.52%. The UV-resistant PDLC is obtained, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0115] Comparative Example 2
[0116] Table 18
[0117]
[0118] After the PDLC composition in Table 18 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 24° C., and the curing light intensity was 5 mw / cm 2 , the curing time is 8min; the thickness of the PET conductive film is 188μm, the square resistance is 122.5Ω, the total light transmittance is 81.5%, and the haze is 0.52%. The UV-resistant PDLC is obtained, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0119] Comparative Example 3
[0120] Table 19
[0121]
[0122] After the PDLC composition in Table 19 was fully stirred, a PDLC film was prepared, wherein the preparation method was: the PDLC composition was placed in two PET conductive films, rolled to form a sandwich structure, and then placed under ultraviolet light for photocuring, the curing temperature was 24° C., and the curing light intensity was 5 mw / cm 2 , the curing time is 8min; the thickness of the PET conductive film is 188μm, the square resistance is 122.5Ω, the total light transmittance is 81.5%, and the haze is 0.52%. The UV-resistant PDLC is obtained, and the PDLC haze is tested using a Japanese electrochromic haze meter NDH7000II.
[0123] The haze test results of the PDLC films of the above examples and comparative examples are shown in Table 20. The PDLC films prepared in Examples 1-6 and Comparative Examples 1-3 were placed under a metal halide lamp (intensity: 6 mW / cm 2 ) for 12 hours, and irradiated. The yellowing degree of the PDLC film (in foggy state) was tested using a CM-36dG colorimeter. The results are shown in Table 21.
[0124] Table 20 Fog haze of Example 1-Example 6, Comparative Example 1-Comparative Example 3
[0125]
[0126] Table 21 L*, a*, b* values of PDLC in fog state in Examples 1-6 and Comparative Examples 1-3
[0127]
[0128] Result analysis:
[0129] The haze values of Examples 1 to 6 in Table 20 are all greater than 97%, indicating that the addition of polybiphenyl monomers, ester-linked phenyl monomers, and ester-linked polyphenyl monomers in the liquid crystal composition can meet the requirement of high haze value in the foggy state of PDLC.
[0130] Table 21 shows the L*, a*, and b* values of the PDLC in the foggy state tested by the colorimeter. The b* value in the L*, a*, and b* values tested by the colorimeter can reflect the yellow-blue color change of the film, with a positive value indicating yellow and a negative value indicating blue. The b* values of the PDLC in the foggy state in Examples 1-6 and Comparative Examples were tested, and it was found that the b* values were all between 7.5 and 7.9 before the irradiation of the metal halide lamp, with no significant difference; after irradiation with the metal halide lamp for 12 hours, the b* values of the PDLC in the foggy state were tested again, and it was found that the b* values of Examples 1-6 had no significant change, and the b* values of Comparative Examples 1, 2, and 3 increased significantly. It was observed with the naked eye that the color of the PDLC film in Examples 1-6 did not turn yellow significantly, and the PDLC film in Comparative Examples 1, 2, and 3 turned yellow, indicating that the use of polyphenyl monomers, ester-linked phenyl monomers, and ester-linked polyphenyl monomers can synergistically enhance the anti-aging effect of PDLC.
[0131] In summary, the use of polyphenyl monomers, ester-linked phenyl monomers, and ester-linked polyphenyl monomers in the liquid crystal composition of the present invention can maintain the high haze requirement of PDLC; at the same time, it is resistant to UV radiation to avoid yellowing of its color; and can be widely used in the fields of building glass curtain walls, automobile sunroofs, automobile side windows, etc.
[0132] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0133] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
Claims
1. A UV-resistant PDLC composition, characterized in that: The PDLC composition is composed of 35 to 60 parts of photocurable glue, 40 to 65 parts of nematic liquid crystals and 0.1 to 3 parts of spacers by weight, wherein the photocurable glue and the nematic liquid crystals total 100 parts; The nematic liquid crystal comprises, by mass percentage, 40-60% of component I, 5-20% of component II, 0.5-20% of component III, and 5-20% of component IV; The structures of components Ⅰ to Ⅳ are as follows: Wherein, R1 to R5 are independently alkyl-C n H 2n+1 or alkoxy-OC n H 2n+1 , wherein n is any integer between 1 and 9; Z1, Z2, and Z3 independently represent a single bond or a -COO-ester bond; A1 to A3 independently represent 1,4-phenylene or 1,4-cyclohexyl; L1 represents -F or alkyl-C n H 2n+1 Or -H, wherein n is any integer between 1 and 9; m represents any integer between 0 and 2.
2. The UV-resistant PDLC composition according to claim 1, characterized in that: The component I is selected from one or more of the following compounds:
3. The UV-resistant PDLC composition according to claim 1, characterized in that: The component II is selected from one or more of the following compounds:
4. The UV-resistant PDLC composition according to claim 1, characterized in that: The component III is selected from one or more of the following compounds:
5. The UV-resistant PDLC composition according to claim 1, characterized in that: The component IV is selected from one or more of the following compounds:
6. The UV-resistant PDLC composition according to claim 1, characterized in that: The light-curing glue comprises 15-30% of acrylate oligomer, 65-80% of acrylate diluent, 0.5-5% of phosphate modifier and 0.5-3% of photoinitiator in terms of mass percentage.
7. The UV-resistant PDLC composition according to claim 1, characterized in that: The particle size of the spacer is 3-20 μm, and the material is polystyrene or silicon dioxide.
8. The UV-resistant PDLC composition according to claim 6, characterized in that: The acrylate oligomer is selected from one or more of aliphatic urethane acrylate, alicyclic urethane acrylate, aromatic urethane acrylate, polyester acrylate, polyether-modified acrylate and epoxy acrylate; The acrylate diluent is selected from one or more of monofunctional acrylate, monofunctional methacrylate, difunctional acrylate, difunctional methacrylate, multifunctional acrylate and multifunctional methacrylate; The photoinitiator is selected from one or more of photoinitiator TPO, photoinitiator 1173, photoinitiator 651, photoinitiator 907, photoinitiator ITX, photoinitiator MBF, photoinitiator 369, photoinitiator 819, photoinitiator 184, photoinitiator TPO-L, photoinitiator OXE-02, photoinitiator OXE-04 and photoinitiator 2959.
9. A PDLC film prepared based on a UV-resistant PDLC composition according to any one of claims 1 to 8, characterized in that: The preparation method of the PDLC film comprises: placing the PDLC composition in two PET conductive films, rolling them to form a sandwich structure, and then placing them under ultraviolet light for photocuring, wherein the curing temperature is 24-26° C. and the curing light intensity is 3-15 mw / cm 2 , the curing time is 2-10min; the thickness of the PET conductive film is 188μm, the square resistance is 120-130Ω, the total light transmittance is 80-85%, and the haze is 0.5-1%.
10. Use of the PDLC film as claimed in claim 9 in outdoor building curtain walls, automobile skylights or automobile side windows.
