Method for improving impact fatigue performance of martensitic stainless steel band
By treating martensitic stainless steel strips with lasers, cryogenics, and ultrasound, combined with carbon dioxide gas protection, the problem of insufficient impact fatigue performance of martensitic stainless steel strips has been solved, resulting in significant performance improvement and service life extension.
Patent Information
- Application Number
- CN202410989760.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Martensitic stainless steel strips are prone to impact fatigue failure during long-term service, and existing technologies are insufficient to effectively improve their impact fatigue performance.
By performing vertical double-sided laser shock treatment, cryogenic treatment, and ultrasonic shock treatment on martensitic stainless steel strips, combined with carbon dioxide gas protection, the microstructure is refined, residual compressive stress is formed, surface hardness is improved, residual austenite is eliminated, and fatigue crack formation is suppressed.
It significantly improves the impact fatigue performance of martensitic stainless steel strips, enhances surface hardness and compressive stress, and extends service life.
Smart Images

Figure BDA0004958533390000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal processing, and in particular to a method for improving the impact fatigue performance of a martensitic stainless steel strip. Background Art
[0002] High-performance steel strips used in refrigeration, printing, textile, cutting tools and other industries largely determine the performance and service life of related equipment and parts. They are key basic materials with large quantities and wide applications in the national economy and are recognized as high value-added products in the steel industry. With the continuous expansion of application occasions, the application environment of steel strip products has become more complex and harsh, often requiring them to have good mechanical properties such as high hardness, wear resistance, fatigue resistance, and certain corrosion resistance. Traditional steel strip materials are mainly carbon steel and austenitic stainless steel represented by 301 stainless steel. Although carbon steel has good mechanical properties, its corrosion resistance is difficult to meet higher requirements. The performance characteristics of austenitic stainless steel are just the opposite, and austenitic stainless steel processed by cold deformation inevitably has performance anisotropy. Martensitic stainless steel strips have both excellent mechanical properties and certain corrosion resistance. They can also eliminate anisotropy through heat treatment. They are ideal steel grades for use as high-performance steel strips and have been widely used in high-end products abroad.
[0003] Valve plates made of martensitic stainless steel strips are important parts in air compressors. During the service process, valve plates are subjected to the impact of high-pressure gas for a long time, and impact fatigue is the main form of failure of martensitic stainless steel strip valve plates. Therefore, how to improve the impact fatigue performance of martensitic stainless steel strips is the key to improving the service performance of martensitic stainless steel strip valve plates. Summary of the invention
[0004] In order to improve the impact fatigue performance of a martensitic stainless steel strip, the present application provides a method for improving the impact fatigue performance of a martensitic stainless steel strip.
[0005] The present application provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, comprising the following steps: Step S1: firstly covering the upper surface and the lower surface of the martensitic stainless steel strip with energy absorption layers respectively, and then simultaneously performing vertical laser shock treatment on the upper surface and the lower surface of the martensitic stainless steel strip; Step S2: after the laser shock treatment is completed, the martensitic stainless steel strip is transferred to a cryogenic environment for cryogenic treatment; Step S3: after the cryogenic treatment is completed, the martensitic stainless steel strip is transferred to a room temperature environment and warmed to room temperature, and ultrasonic impact treatment in a vertical direction is simultaneously performed on the upper and lower surfaces of the martensitic stainless steel strip; Step S4: After the ultrasonic impact treatment is completed, the energy absorbing layer is removed and the martensitic stainless steel strip is covered with a protective layer.
[0006] The present application sequentially performs laser shock treatment, cryogenic treatment and ultrasonic shock treatment on the martensitic stainless steel strip, thereby being able to substantially eliminate the residual austenite inside the martensitic stainless steel strip, and forming residual compressive stress on the surface of the steel strip and improving the surface hardness, thereby inhibiting the generation of fatigue cracks inside and on the surface of the steel strip under the action of impact loads, and significantly improving the impact fatigue performance of the martensitic stainless steel strip.
[0007] Through vertical double-sided laser shock treatment, the microstructure of the upper and lower surfaces is refined at the same time, forming a work hardening effect on the upper and lower surfaces of the steel strip, improving the surface hardness, and forming compressive stress on the upper and lower surfaces, which can inhibit the generation of fatigue cracks on the surface of the steel strip during long-term service and impact loads; in addition, simultaneous laser shock treatment on the upper and lower surfaces can offset the forces, avoid macroscopic deformation of the steel strip, and ensure the smooth progress of subsequent processing; through laser shock treatment and utilizing the hardness difference between martensite and residual austenite in the martensitic stainless steel strip, a large number of dislocations can be formed in the residual austenite, which can prevent the martensitic stainless steel strip from deforming; Then, deep cryogenic treatment is carried out to induce a large number of nuclei of martensite at the dislocations of the retained austenite, so that the retained austenite forms fine martensite grains, eliminates the weak positions in the martensitic stainless steel strip, and avoids the generation of fatigue cracks inside the steel strip during long-term service under impact loads; Finally, ultrasonic impact treatment can further improve the surface hardness and compressive stress of the steel strip, and inhibit the generation of fatigue cracks on the surface of the steel strip during long-term service under impact loads; in addition, since the surface roughness of the steel strip increases due to the transformation of residual austenite after laser impact, ultrasonic impact treatment can reduce the surface roughness of the steel strip and ensure the surface quality of the steel strip; in addition, after ultrasonic impact, the energy absorption layer that absorbs laser energy can be quickly separated from the surface of the steel strip, which is convenient for post-processing.
[0008] Furthermore, when performing laser shock processing, it is also possible to consider using carbon dioxide gas as an auxiliary gas to act on the surface of the workpiece together with the laser beam to generate shock waves, thereby improving the mechanical properties and surface quality of the workpiece. Specifically, carbon dioxide gas can be used to protect the laser beam and the surface of the steel strip during laser shock processing to prevent impurities in the air from adversely affecting the processing process. As an inert gas, carbon dioxide has stable chemical properties and will not react chemically with the laser beam or the target surface. It can not only effectively prevent oxidation reactions during the processing process and maintain the purity of the material, but also help remove residues and oxides generated during the processing process to keep the processing area clean.
[0009] Although carbon dioxide itself does not directly increase the hardness and strength of stainless steel, it can effectively prevent the oxidation of stainless steel during laser processing and maintain the purity of the material, which is beneficial to the improvement of hardness and strength in subsequent processing.
[0010] During the laser shock treatment process, the flow rate of carbon dioxide is 5-20 L / min, preferably 10 L / min. The flow rate within this range can provide sufficient protection effect and avoid affecting the focus of the laser beam, thereby ensuring the stability and efficiency of the treatment process.
[0011] Optionally, both the laser shock treatment and the ultrasonic shock treatment adopt a fixed shock source, and the martensitic stainless steel strip is configured to move at a uniform speed along the length direction of the martensitic stainless steel strip.
[0012] By adopting the above technical solution, under the condition of consistent movement speed, it can be ensured that all martensitic stainless steel strips can be subjected to uniform laser shock and ultrasonic shock during the movement process, thereby ensuring the uniformity of the product.
[0013] Optionally, the laser shock spot of the laser shock treatment is a square spot, and the side length of the square spot is the same as the width of the martensitic stainless steel strip.
[0014] By adopting the above technical solution, it can be ensured that the laser impact range completely covers the surface of the martensitic stainless steel strip, ensuring that the laser impact received at each location is consistent, without duplication or omission.
[0015] Optionally, the impact head used in the ultrasonic impact treatment is a square impact head, and the side length of the impact head is the same as the width of the martensitic stainless steel strip.
[0016] By adopting the above technical solution, it can be ensured that the ultrasonic impact range completely covers the surface of the martensitic stainless steel strip, ensuring that the ultrasonic impact received at each location is consistent without duplication or omission.
[0017] Optionally, the martensitic stainless steel strip has a width of 10 to 20 mm and a thickness of 0.4 to 1.2 mm.
[0018] Optionally, the energy of the laser shock treatment is 5-10J, and the frequency of the laser is 30Hz.
[0019] By adjusting the laser parameters, it can be ensured that martensitic stainless steel strips of different thicknesses can be fully impacted by the laser from the surface to the core, ensuring that sufficient dislocations are formed in the residual austenite, laying the foundation for the refinement of martensite grains in subsequent deep cryogenic treatment.
[0020] Optionally, the cryogenic treatment temperature is -150°C to -50°C, and the cryogenic treatment time is 10 min to 20 min.
[0021] By providing a suitable low temperature environment, a large number of martensite nucleations can be induced at the dislocations of retained austenite, which can promote the formation of fine-grained martensite grains in the retained austenite.
[0022] Optionally, the amplitude of the ultrasonic impact treatment is 10-20 μm.
[0023] By adjusting the ultrasonic parameters, it can be ensured that martensitic stainless steel strips of different thicknesses can be fully subjected to ultrasonic impact from the surface to the core, thereby improving the surface hardness and compressive stress of the steel strips and inhibiting the generation of fatigue cracks on the surface of the steel strips during long-term service under impact loads.
[0024] Optionally, the energy absorbing layer is a black tape, and the thickness of the energy absorbing layer is 100-120 μm.
[0025] The present application provides an energy absorption layer on the surface of the martensitic stainless steel strip, so that it can ensure high energy absorption efficiency during the laser shock process.
[0026] Optionally, the step S1 further includes the step of providing a constraining layer outside the energy absorbing layer.
[0027] The constrained layer has a synergistic effect on the laser shock, so that the laser shock generates a sufficiently large shock pressure. Flowing water can be used as the constrained layer for laser shock, and the surface tension of water can be used to constrain the direction of the force of the laser-induced plasma shock wave, thereby increasing the amplitude and time of the force, thereby improving the effect of laser shock strengthening.
[0028] In summary, this application has the following beneficial effects: Through vertical double-sided laser shock treatment, the microstructure of the upper and lower surfaces is refined at the same time, forming a work hardening effect on the upper and lower surfaces of the steel strip, improving the surface hardness, and forming compressive stress on the upper and lower surfaces, which can inhibit the generation of fatigue cracks on the surface of the steel strip during long-term service and impact loads; in addition, simultaneous laser shock treatment on the upper and lower surfaces can offset the forces, avoid macroscopic deformation of the steel strip, and ensure the smooth progress of subsequent processing; through laser shock treatment and utilizing the hardness difference between martensite and residual austenite in the martensitic stainless steel strip, a large number of dislocations can be formed in the residual austenite, which can prevent the martensitic stainless steel strip from deforming; Then, deep cryogenic treatment is carried out to induce a large number of nuclei of martensite at the dislocations of the retained austenite, so that the retained austenite forms fine martensite grains, eliminates the weak positions in the martensitic stainless steel strip, and avoids the generation of fatigue cracks inside the steel strip during long-term service under impact loads; Finally, ultrasonic impact treatment can further improve the surface hardness and compressive stress of the steel strip, and inhibit the generation of fatigue cracks on the surface of the steel strip during long-term service under impact loads; in addition, since the surface roughness of the steel strip increases due to the transformation of residual austenite after laser impact, ultrasonic impact treatment can reduce the surface roughness of the steel strip and ensure the surface quality of the steel strip; in addition, after ultrasonic impact, the energy absorption layer that absorbs laser energy can be quickly separated from the surface of the steel strip, which is convenient for post-processing. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its application or use. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0030] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the application. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0031] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards; if there is no corresponding national standard, it is carried out according to the general international standards or the standard requirements proposed by relevant enterprises. Unless otherwise specified, all parts are by weight and all percentages are by weight.
[0032] Based on the technical issues raised in the background technology section, the applicant has found through analysis that the impact fatigue of martensitic stainless steel strips mainly comes from two aspects. First, there is residual austenite inside the material. During long-term service, the residual austenite becomes a weak position in the deformation process due to insufficient strength and hardness, resulting in fatigue cracks. Second, fatigue cracks are formed on the surface of the steel strip under the action of tensile stress. Therefore, in order to improve the impact fatigue life of martensitic stainless steel strips, it is necessary to reduce or eliminate the residual austenite in the martensitic stainless steel strips, and at the same time reduce or eliminate the tensile stress on the surface of the steel strips, or increase the compressive stress on the surface of the steel strips.
[0033] By sequentially subjecting the martensitic stainless steel strip to laser shock treatment, cryogenic treatment and ultrasonic shock treatment, the applicant can not only substantially eliminate the residual austenite in the martensitic stainless steel strip, but also further improve the surface hardness and compressive stress of the steel strip, thereby fundamentally suppressing the generation of fatigue cracks on the surface of the steel strip during long-term service under impact loads.
[0034] The scheme of the present application will be described below with reference to specific embodiments and comparative examples.
[0035] Example 1 Example 1 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 0.4 mm.
[0036] The processing process includes the following steps: S1. The upper and lower surfaces of the above-mentioned 95Cr18 high-carbon martensitic stainless steel strip are covered with a black tape with a thickness of 100 μm as an energy absorption layer for laser shock. The upper and lower surfaces of the martensitic stainless steel strip are simultaneously subjected to laser shock treatment perpendicular to the upper and lower surfaces. During the shock process, the position of the laser light source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 5 J and the laser shock frequency is 30 Hz. S2, the martensitic stainless steel strip after laser shock treatment is immediately transferred to a -50°C environment for deep cryogenic treatment for 10 minutes; S3. After the cryogenic treatment, the martensitic stainless steel strip is transferred to a room temperature environment. When the temperature returns to room temperature, ultrasonic impact treatment is performed simultaneously on the upper and lower surfaces perpendicular to the martensitic stainless steel strip. During the ultrasonic impact process, the position of the ultrasonic source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. The ultrasonic impact head is square with a side length of 20 mm and an ultrasonic amplitude of 10 μm. After the ultrasonic impact, rinse the entire surface of the martensitic stainless steel strip with water to remove the remaining black tape, and then apply oil for protection after drying.
[0037] Example 2 Example 2 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 1.2 mm.
[0038] The processing process includes the following steps: S1. The upper and lower surfaces of the above-mentioned 95Cr18 high-carbon martensitic stainless steel strip are covered with a black tape with a thickness of 120 μm as an energy absorption layer for laser shock. The upper and lower surfaces of the martensitic stainless steel strip are simultaneously subjected to laser shock treatment perpendicular to the upper and lower surfaces. During the shock process, the position of the laser light source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 10 J and the laser shock frequency is 30 Hz. S2, the martensitic stainless steel strip after laser shock treatment is immediately transferred to a -150°C environment for deep cryogenic treatment for 20 minutes; S3. After the cryogenic treatment, the martensitic stainless steel strip is transferred to a room temperature environment. When the temperature returns to room temperature, ultrasonic impact treatment is performed simultaneously on the upper and lower surfaces perpendicular to the martensitic stainless steel strip. During the ultrasonic impact process, the position of the ultrasonic source remains unchanged, and the martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. The ultrasonic impact head is square with a side length of 20 mm and an ultrasonic amplitude of 20 μm. After the ultrasonic impact, rinse the entire surface of the martensitic stainless steel strip with water to remove the remaining black tape, and then apply oil for protection after drying.
[0039] Example 3 Example 3 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 0.8 mm.
[0040] The processing process includes the following steps: S1. The upper and lower surfaces of the above-mentioned 95Cr18 high-carbon martensitic stainless steel strip are covered with a black tape with a thickness of 110 μm as an energy absorption layer for laser shock. The upper and lower surfaces of the martensitic stainless steel strip are simultaneously subjected to laser shock treatment perpendicular to the upper and lower surfaces. During the shock process, the position of the laser light source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 8 J and the laser shock frequency is 30 Hz. S2, the martensitic stainless steel strip after laser shock treatment is immediately transferred to a -100°C environment for deep cryogenic treatment for 15 minutes; S3. After the cryogenic treatment, the martensitic stainless steel strip is transferred to a room temperature environment. When the temperature returns to room temperature, ultrasonic impact treatment is performed simultaneously on the upper and lower surfaces perpendicular to the martensitic stainless steel strip. During the ultrasonic impact process, the position of the ultrasonic source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. The ultrasonic impact head is square with a side length of 20 mm and an ultrasonic amplitude of 15 μm. After the ultrasonic impact, rinse the entire surface of the martensitic stainless steel strip with water to remove the remaining black tape, and then apply oil for protection after drying.
[0041] Example 4 Example 4 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 0.8 mm.
[0042] The processing process is basically the same as that of Example 3, except that, when laser shock treatment is performed in step S1, carbon dioxide gas will be used as an auxiliary gas to act on the workpiece surface together with the laser beam, and the flow rate of carbon dioxide is 10L / min.
[0043] Comparative Example 1 Comparative Example 1 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip, and the width of the steel strip is 20 mm and the thickness is 0.8 mm.
[0044] The processing process includes the following steps: The upper surface of the 95Cr18 high-carbon martensitic stainless steel strip is covered with a black tape with a thickness of 110 μm as an energy absorption layer for laser shock, and the upper surface of the martensitic stainless steel strip is subjected to vertical laser shock treatment. During the shock process, the position of the laser light source remains unchanged, and the martensitic stainless steel strip moves uniformly along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 8 J, and the laser shock frequency is 30 Hz. The above laser shock treatment operation was repeated 3 times. After the laser shock treatment was completed, the upper surface of the martensitic stainless steel strip was washed with water to remove the residual black tape, and then oil was applied for protection after drying.
[0045] Comparative Example 2 Comparative Example 2 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 0.8 mm.
[0046] The processing process includes the following steps: The upper and lower surfaces of the 95Cr18 high-carbon martensitic stainless steel strip are covered with a black tape with a thickness of 110 μm as an energy absorption layer for laser shock. The upper and lower surfaces of the martensitic stainless steel strip are simultaneously subjected to laser shock treatment perpendicular to the upper and lower surfaces. During the shock process, the position of the laser light source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 8 J and the laser shock frequency is 30 Hz. The above laser shock treatment operation was repeated 3 times. After the laser shock treatment was completed, the entire surface of the martensitic stainless steel strip was washed with water to remove the residual black tape, and then the strip was dried and oiled for protection.
[0047] Comparative Example 3 Comparative Example 3 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 0.8 mm.
[0048] The processing process includes the following steps: S1. The upper and lower surfaces of the above-mentioned 95Cr18 high-carbon martensitic stainless steel strip are covered with a black tape with a thickness of 110 μm as an energy absorption layer for laser shock. The upper and lower surfaces of the martensitic stainless steel strip are simultaneously subjected to laser shock treatment perpendicular to the upper and lower surfaces. During the shock process, the position of the laser light source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 8 J and the laser shock frequency is 30 Hz. S2, the martensitic stainless steel strip after laser shock treatment is immediately transferred to a -100°C environment for deep cryogenic treatment for 15 minutes; S3. After the cryogenic treatment, transfer the martensitic stainless steel strip to room temperature. When the temperature returns to room temperature, rinse the entire surface of the martensitic stainless steel strip with water to remove the remaining black tape. After drying, apply oil for protection.
[0049] Comparative Example 4 Comparative Example 4 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 0.8 mm.
[0050] The processing process includes the following steps: S1. Performing ultrasonic impact treatment in a vertical direction on the upper and lower surfaces of the above-mentioned 95Cr18 high-carbon martensitic stainless steel strip simultaneously. During the ultrasonic impact process, the position of the ultrasonic source remains unchanged, and the martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. The ultrasonic impact head is square with a side length of 20 mm and an ultrasonic amplitude of 15 μm. S2, immediately transferring the martensitic stainless steel strip after ultrasonic impact treatment to a -100°C environment for deep cryogenic treatment for 15 minutes; S3. After the cryogenic treatment, transfer the martensitic stainless steel strip to room temperature. When the temperature returns to room temperature, rinse the entire surface of the martensitic stainless steel strip with water, and then apply oil for protection after drying.
[0051] Comparative Example 5 Comparative Example 5 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 0.8 mm.
[0052] The processing process includes the following steps: S1. The upper and lower surfaces of the above-mentioned 95Cr18 high-carbon martensitic stainless steel strip are covered with a black tape with a thickness of 110 μm as an energy absorption layer for laser shock. The upper and lower surfaces of the martensitic stainless steel strip are simultaneously subjected to laser shock treatment perpendicular to the upper and lower surfaces. During the shock process, the position of the laser light source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 8 J and the laser shock frequency is 30 Hz. S2. Then, ultrasonic impact treatment is simultaneously performed on the upper and lower surfaces perpendicular to the martensitic stainless steel strip. During the ultrasonic impact process, the position of the ultrasonic source remains unchanged, and the martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. The ultrasonic impact head is square with a side length of 20 mm and an ultrasonic amplitude of 15 μm. After the ultrasonic impact, rinse the entire surface of the martensitic stainless steel strip with water to remove the remaining black tape, and then apply oil for protection after drying.
[0053] Comparative Example 6 Comparative Example 6 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip with a width of 20 mm and a thickness of 0.8 mm.
[0054] The processing process includes the following steps: S1. Ultrasonic impact treatment is simultaneously performed on the upper and lower surfaces perpendicular to the above-mentioned 95Cr18 high-carbon martensitic stainless steel strip. During the ultrasonic impact process, the position of the ultrasonic source remains unchanged, and the martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. The ultrasonic impact head is square with a side length of 20 mm and an ultrasonic amplitude of 15 μm. S2. The upper and lower surfaces of the martensitic stainless steel strip are covered with a black tape with a thickness of 110 μm as an energy absorption layer for laser shock. The upper and lower surfaces of the martensitic stainless steel strip are simultaneously subjected to laser shock treatment perpendicular to the upper and lower surfaces. During the shock process, the position of the laser light source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 8 J and the laser shock frequency is 30 Hz. After the laser shock is completed, the entire surface of the martensitic stainless steel strip is rinsed with water to remove the residual black tape, and then oil is applied for protection after drying.
[0055] Comparative Example 7 Comparative Example 7 provides a method for improving the impact fatigue performance of a martensitic stainless steel strip, wherein the martensitic stainless steel strip is a 95Cr18 high-carbon martensitic stainless steel strip, and the width of the steel strip is 20 mm and the thickness is 0.8 mm.
[0056] The processing process includes the following steps: S1. Ultrasonic impact treatment is simultaneously performed on the upper and lower surfaces perpendicular to the above-mentioned 95Cr18 high-carbon martensitic stainless steel strip. During the ultrasonic impact process, the position of the ultrasonic source remains unchanged, and the martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. The ultrasonic impact head is square with a side length of 20 mm and an ultrasonic amplitude of 15 μm. S2, immediately transferring the martensitic stainless steel strip after ultrasonic impact treatment to a -100°C environment for deep cryogenic treatment for 15 minutes; S1. After the cryogenic treatment, the martensitic stainless steel strip is transferred to a room temperature environment. When the temperature returns to room temperature, the upper and lower surfaces of the martensitic stainless steel strip are covered with a black tape with a thickness of 110 μm as an energy absorption layer for laser shock. The upper and lower surfaces perpendicular to the martensitic stainless steel strip are simultaneously subjected to laser shock treatment. During the shock process, the position of the laser light source remains unchanged. The martensitic stainless steel strip moves at a uniform speed along the length direction at a speed of 1 mm / s. Flowing water is used as a constraint layer for laser shock. The laser shock spot is a square spot with a side length of 20 mm. The single-pulse laser energy is 8 J and the laser shock frequency is 30 Hz. After the ultrasonic impact, rinse the entire surface of the martensitic stainless steel strip with water to remove the remaining black tape, and then apply oil for protection after drying.
[0057] Comparative Example 8 Comparative Example 8 is substantially the same as Example 3, except that the cryogenic treatment temperature is -100°C and the cryogenic treatment time is 8 minutes.
[0058] Comparative Example 9 Comparative Example 9 is substantially the same as Example 3, except that the cryogenic treatment temperature is -40°C and the cryogenic treatment time is 15 min.
[0059] A 95Cr18 high carbon martensitic stainless steel strip without any treatment was selected as a blank test group. The martensitic stainless steel strips obtained in the above Examples 1-4 and Comparative Examples 1-9 and the blank test group were tested for surface hardness, surface roughness and impact fatigue tests, and the test results are shown in Table 1.
[0060] (1) Surface hardness: measured with a Rockwell hardness tester; (2) Surface roughness Ra: obtained by roughness meter test; (3) Impact fatigue life: A non-contact high-pressure gas impact fatigue test was conducted, using a pulsed airflow impact method to simulate the normal opening and closing of the strip during use. By controlling the switching frequency of the high-speed solenoid valve and the air pressure of the air source, the strip was stimulated with different frequencies and pressure differences. The strip length was 50 mm, the amplitude was ±30°, and the frequency was 50 Hz. If the strip broke, it was judged as an impact fatigue failure, and the life was calculated by the number of cycles.
[0061] Table 1 Martensitic stainless steel strip properties of the embodiments and comparative examples It can be seen from the data in Table 1 that, compared with the blank test group, Examples 1-4 adopt a process sequence of double-sided laser, deep cooling, and double-sided ultrasound as well as appropriate process parameters, and the austenite residual rate of the treated martensitic stainless steel strip is greatly reduced, the surface hardness of the steel strip is also improved, the surface roughness of the steel strip is greatly reduced, and the impact fatigue life is increased by at least 120%.
[0062] It can be seen from the data of Example 3 and Comparative Examples 1 and 2 that when laser shock treatment is used alone, whether it is single-sided shock or double-sided simultaneous shock, even if the laser shock is repeated 3 times, the surface hardness and impact fatigue life of the obtained martensitic stainless steel strip are slightly increased, but the austenite retention rate is not reduced, but increased, and the surface roughness is also increased by nearly 1 times due to multiple shocks.
[0063] It can be seen from the data of Example 3 and Comparative Examples 3-6 that Comparative Examples 3-6 use a combination of any two processes of double-sided laser, deep cooling, and double-sided ultrasound to treat the martensitic stainless steel strip, and the various properties of the obtained martensitic stainless steel strip are not as good as those of Example 3.
[0064] It can be seen from the data of Example 3 and Comparative Example 7 that although Comparative Example 7 also adopts the three processes of double-sided laser, deep cooling and double-sided ultrasound, since Comparative Example 7 adjusts the order of these three processes, the various properties of the obtained martensitic stainless steel strip are not as excellent as those of Example 3.
[0065] It can be seen from Example 3 and Comparative Examples 8-9 that the cryogenic treatment time of Comparative Example 8 is shorter than that of Example 3, resulting in a slightly worse impact fatigue life of the martensitic stainless steel strip obtained therefrom. The cryogenic treatment temperature of Comparative Example 9 is higher than that of Example 3, resulting in the surface hardness and impact fatigue life of the martensitic stainless steel strip obtained therefrom not being as good as those of Example 3.
[0066] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for improving the impact fatigue performance of a martensitic stainless steel strip, characterized in that: The steps include: Step S1: firstly covering the upper surface and the lower surface of the martensitic stainless steel strip with energy absorption layers respectively, and then simultaneously performing vertical laser shock treatment on the upper surface and the lower surface of the martensitic stainless steel strip; Step S2: after the laser shock treatment is completed, the martensitic stainless steel strip is transferred to a cryogenic environment for cryogenic treatment; Step S3: after the cryogenic treatment is completed, the martensitic stainless steel strip is transferred to a room temperature environment and warmed to room temperature, and ultrasonic impact treatment in a vertical direction is simultaneously performed on the upper and lower surfaces of the martensitic stainless steel strip; Step S4: After the ultrasonic impact treatment is completed, the energy absorbing layer is removed and the martensitic stainless steel strip is covered with a protective layer.
2. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to claim 1, characterized in that: The laser shock treatment and the ultrasonic shock treatment both adopt a fixed shock source, and the martensitic stainless steel strip is configured to move at a uniform speed along the length direction of the martensitic stainless steel strip.
3. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to claim 2, characterized in that: The laser shock spot of the laser shock treatment is a square spot, and the side length of the square spot is the same as the width of the martensitic stainless steel strip.
4. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to claim 2, characterized in that: The impact head used in the ultrasonic impact treatment is a square impact head, and the side length of the impact head is the same as the width of the martensitic stainless steel strip.
5. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to claim 1, characterized in that: The width of the martensitic stainless steel strip is 10-20 mm, and the thickness is 0.4-1.2 mm.
6. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to claim 1, characterized in that: The energy of the laser shock treatment is 5-10J, and the laser frequency is 30Hz.
7. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to claim 1, characterized in that: The cryogenic treatment temperature is -150°C to -50°C, and the cryogenic treatment time is 10min to 20min.
8. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to claim 1, characterized in that: The amplitude of the ultrasonic impact treatment is 10-20 μm.
9. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to claim 1, characterized in that: The energy absorbing layer is a black tape, and the thickness of the energy absorbing layer is 100-120 μm.
10. The method for improving the impact fatigue performance of a martensitic stainless steel strip according to any one of claims 1 to 9, characterized in that: The step S1 also includes the step of providing a constraining layer outside the energy absorbing layer.