Electroslag remelting slag system as well as application and use method thereof

The new electroslag reslag system formed by using CaO instead of Al2O3 in the electroslag reslag system has solved the problem of large-head aluminum increase in smelting of high-titanium and low-aluminum alloys, reduced power consumption and smelting costs, and increased Surface quality and production efficiency of steel ingots.

CN118932185APending Publication Date: 2024-11-12AVIC SHANGDA METAL REGENERATION TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411164766.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing electroslag remelting slag system can easily lead to large-head aluminum increase in smelting in high-titanium and low-aluminum alloys, resulting in difficulty in quality control of steel ingots and waste production, and the cost of dealumination is high.

Method used

The electroslag remelting slag system formed by using CaO instead of Al2O3, including CaF2 63%~70%, CaO 12%~18%, MgO 10%~16%, TiO2 2%~6%, to reduce the conductivity of the slag system and melting point, improve fluidity, avoid the increase of Al elements, reduce power consumption and waste production.

Benefits of technology

It effectively solved the problem of excessive aluminum content at the bottom of high-titanium and low-aluminum alloy steel ingots, reduced power consumption and smelting costs, improved production efficiency and surface quality of steel ingots, and reduced waste production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932185A_ABST
    Figure CN118932185A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metal smelting, and particularly discloses an electroslag remelting slag system and application and a using method thereof. The electroslag remelting slag system comprises the following chemical components in percentage by mass: 63%-70% of CaF2, 12%-18% of CaO, 10%-16% of MgO and 3%-6% of TiO2. According to the method, Al2O3 in a traditional slag system is omitted, and the situation that Al2O3 is reduced into Al in the metal smelting process, and consequently aluminum in a steel ingot is increased is avoided; caO is adopted to replace Al2O3, so that the low conductivity of the slag system can be ensured, the power consumption is reduced, the production efficiency is improved, the melting point of the slag system is reduced, the melting point difference between the slag system and metal is increased, the viscosity of the slag system is reduced, and the slag system has good fluidity. By controlling the chemical components and content of an electroslag remelting slag system, metal can be fully melted in the metal smelting process, the slag system is prevented from being mixed with the metal, and the bottom forming problem of a remelting steel ingot is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal smelting, and in particular to an electroslag remelting slag system and an application and use method thereof. Background Art

[0002] R26 alloy is called Refractaloy26 alloy. It belongs to Ni-Cr-Co-Fe series high temperature resistant and corrosion resistant alloy. It contains high Ni, Co, Cr, Mo and other alloy elements. It has excellent relaxation resistance, stress resistance, creep resistance and mechanical properties. R26 alloy is mainly used for bolt materials of high pressure inner cylinder, medium pressure inner cylinder, high pressure side balance piston steam seal, high pressure stator ring and other parts of thermal power steam turbine. It has good plasticity at medium temperature and can be used under 540℃~570℃ steam conditions. It can meet the requirements of 300,000 kW~600,000 kW steam turbine fasteners.

[0003] R26 alloy is a typical high-titanium and low-aluminum alloy. This type of steel often increases aluminum in the large head and titanium in the small head during the electroslag remelting process. For high-titanium and low-aluminum alloys, there are two main electroslag remelting slag systems used at home and abroad: one is the traditional binary slag system, that is, CaF2 and Al2O3 with a mass ratio of 7:3, and the other is a quaternary slag system composed of CaF2, Al2O3, MgO and TiO2, with the mass percentages of the four being 75%~80%, 6%~10%, 6%~10% and 2%~5% respectively. However, since the existing electroslag remelting slag systems all contain a high Al2O3 content, it is very easy to cause a serious increase in aluminum in the large head (bottom) during the metal smelting process, and even exceed the standard requirements, resulting in the generation of more waste products, which brings great difficulties to the quality control of R26 alloy steel ingots. The traditional quality control method is to control the aluminum content as low as possible when smelting electrode rods. However, the cost of dealuminization in smelting electrode rod raw materials and subsequent smelting processes is huge. Therefore, there is an urgent need to study an electroslag remelting slag system for high-titanium, low-aluminum alloys to solve the serious problem of bulk aluminum addition, improve the comprehensive performance of high-titanium, low-aluminum alloys, reduce the generation of waste, and save production costs. Summary of the invention

[0004] In view of the above problems, the present invention provides an electroslag remelting slag system and its application and use method, which solves the problem of excessive aluminum content in the big head (bottom of the alloy steel ingot) of high-titanium and low-aluminum alloy steel ingot in the later stage of electroslag remelting.

[0005] In order to solve the above technical problems, the technical solution provided by the present invention is: In a first aspect, the present invention provides an electroslag remelting slag system, comprising the following chemical components in percentage by mass: CaF2 63%~70%, CaO 12%~18%, MgO 10%~16% and TiO23%~6%.

[0006] The commonly used slag system for electroslag remelting is basically based on CaF2, with a certain amount of oxides such as A12O3, CaO, MgO or TiO2. Different components in the slag system have different functions. Among them, CaF2 can reduce the melting point, viscosity and surface tension of the slag system, but CaF2 has a high conductivity and large power consumption, and it is easy to cause environmental pollution and pose a threat to the health of workers; A12O3 can significantly reduce the conductivity of the slag system, reduce power consumption, and improve productivity, but A12O3 will increase the melting point and viscosity of the slag system, and will also reduce the desulfurization effect of the slag system; CaO can increase the basicity of the slag system, improve the desulfurization efficiency, and reduce the conductivity of the slag, but CaO has strong water absorption and is easy to bring hydrogen and oxygen impurities into the alloy.

[0007] Compared with the prior art, the electroslag remelting slag system provided by the present invention omits Al2O3 in the traditional slag system, avoiding the reduction of Al2O3 to Al during the metal smelting process, thereby causing an increase in the Al element in the steel ingot; in order to ensure a lower slag system conductivity, the present invention uses CaO instead of Al2O3 to ensure that the entire slag system has a lower conductivity, thereby reducing power consumption and improving production efficiency; using CaO instead of Al2O3 can also reduce the melting point of the slag system, increase the melting point difference between the slag system and the metal, and at the same time reduce the viscosity of the slag system, so that the slag system has good fluidity. The present invention controls the chemical composition and content of the electroslag remelting slag system, can fully melt the metal during the metal smelting process, avoid mixing of the slag system and the metal, and thus effectively improve the bottom forming problem of the remelted steel ingot.

[0008] Preferably, the electroslag remelting slag system is a quaternary slag system, consisting of the following chemical components in percentage by mass: CaF2 65%~70%, CaO 13%~16%, MgO 12%~15% and TiO23%~5%.

[0009] In a second aspect, the present invention provides an application of the above-mentioned electroslag remelting slag system in the electroslag remelting of high-titanium and low-aluminum alloys.

[0010] Preferably, the high-titanium and low-aluminum alloy is R26 alloy.

[0011] Since the existing electroslag remelting slag system will produce serious bottom aluminum increase phenomenon during the electroslag remelting process, the aluminum content of the consumable electrode rod must be strictly controlled, which puts higher requirements on the raw materials and smelting process of smelting. However, the electroslag remelting slag system provided by the present invention does not have aluminum increase phenomenon in the steel ingot during the electroslag remelting process, and the consumable electrode does not need to use low-aluminum raw materials during smelting. Instead, a large amount of low-cost returned steel can be selected as the raw material for electrode rod smelting, and there is no need to further remove the aluminum element during the smelting process, which greatly reduces the raw material cost and process cost of metal smelting and has a high market promotion value.

[0012] In a third aspect, the present invention provides a method for using the electroslag remelting slag system, comprising the following steps: The electrode rod is placed in the crystallizer, power is supplied to start the arc, the electroslag remelting slag system is added, and refining, steady-state remelting and ingot shrinkage feeding are carried out in sequence to obtain an alloy steel ingot.

[0013] Preferably, the electrode rod is an R26 alloy electrode rod.

[0014] In the present invention, the electrode rod can be produced by a vacuum reaction furnace, and the specific production process can be carried out by conventional methods.

[0015] For example, before adding the electroslag remelting slag system into the crystallizer, the electroslag remelting slag system needs to be baked to remove moisture in the electroslag remelting slag system; the baking temperature is ≥650° C. and the baking time is ≥6 hours.

[0016] Preferably, the voltage of the power transmission arc starting is 56V~68V, and the current of the power transmission arc starting is 4500A~6500A.

[0017] Preferably, the amount of the electroslag remelting slag system added is 33kg~38kg.

[0018] The present invention limits the amount of the electroslag remelting slag system added to ensure that its height in the crystallizer is 200 mm to 250 mm.

[0019] Preferably, the electroslag remelting slag system is added for 10 min to 15 min.

[0020] Preferably, the refining voltage is 56V~68V, the refining current is 4500A~6500A, and the refining time is 10min~15min.

[0021] Preferably, the voltage of the steady-state remelting is 55V~65V, the current of the steady-state remelting is 5000A~6500A, and the time of the steady-state remelting is 200min~250min.

[0022] Preferably, the voltage of the steel ingot shrinkage feeding is 30V~38V, the current of the steel ingot shrinkage feeding is 3000A~3800A, and the time of the steel ingot shrinkage feeding is ≥40min (more preferably 40min~60min).

[0023] Preferably, after the shrinkage compensation of the steel ingot is completed, furnace cooling is performed; and the time of the furnace cooling is ≥50 min.

[0024] The present invention can better control the conductivity and melting point of the slag system by controlling the addition amount of the electroslag remelting slag system and the smelting conditions, increase the melting point difference between the slag system and the metal, reduce the viscosity of the slag system, melt the metal more fully, avoid mixing of the slag system and the metal, effectively improve the bottom forming problem of the remelted steel ingot, and at the same time reduce power consumption and improve production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a diagram showing the molding effect of the bottom of the alloy steel ingot in Application Example 1 of the present invention; Figure 2 This is a diagram showing the forming effect of the bottom of the alloy steel ingot in comparative application example 1 of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] Example 1 This embodiment provides an electroslag remelting slag system, which consists of the following chemical components in percentage by mass: CaF2 65%, CaO 15%, MgO 15% and TiO 25%.

[0028] Example 2 This embodiment provides an electroslag remelting slag system, which consists of the following chemical components in percentage by mass: CaF2 68%, CaO 15%, MgO 12% and TiO 25%.

[0029] Example 3 This embodiment provides an electroslag remelting slag system, which consists of the following chemical components in percentage by mass: CaF2 67%, CaO 13%, MgO 15% and TiO 25%.

[0030] Example 4 This embodiment provides an electroslag remelting slag system, which consists of the following chemical components in percentage by mass: CaF2 70%, CaO 17%, MgO 10% and TiO 23%.

[0031] Example 5 This embodiment provides an electroslag remelting slag system, which consists of the following chemical components in percentage by mass: CaF2 63%, CaO 18%, MgO 13% and TiO 26%.

[0032] Comparative Example 1 This comparative example provides an electroslag remelting slag system, which consists of the following chemical components in percentage by mass: CaF2 75%, A12O3 10%, MgO 10% and TiO 25%.

[0033] Comparative Example 2 This comparative example provides an electroslag remelting slag system, which consists of the following chemical components in percentage by mass: CaF2 77%, CaO 8%, MgO 12% and TiO 23%.

[0034] Comparative Example 3 This comparative example provides an electroslag remelting slag system, which is composed of the following chemical components in percentage by mass: CaF2 70%, A12O3 30%.

[0035] Application Example 1 This application embodiment provides a method for using the electroslag remelting slag system provided in Embodiment 1, comprising the following steps: Put 1t of φ250mm R26 alloy electrode rod into the crystallizer, power on to start the arc (voltage is 60V, current is 5200A), add 35kg of baked electroslag remelting slag system, add for 12 minutes, then refine at 62V, 5200A for 13 minutes, remelt at 60V, 5800A for 230 minutes, feed the steel ingot at 34V, 3400A for 50 minutes, cool with the furnace for 60 minutes, demould, and get a φ360mm alloy steel ingot. The forming effect of the bottom of the alloy steel ingot is shown in the figure below. Figure 1 shown.

[0036] The chemical composition and mass percentage of the R26 alloy electrode rod are shown in Table 1.

[0037] Table 1 Chemical composition of R26 alloy electrode rod (%)

[0038] Application Example 2 This application embodiment provides a method for using the electroslag remelting slag system provided in Embodiment 2, comprising the following steps: 1 ton of φ250 mm R26 alloy electrode rod (chemical composition as shown in Table 1) was placed in the crystallizer, and the arc was started (voltage was 56 V, current was 4500 A). 33 kg of baked electroslag remelting slag system was added. After 10 minutes of addition, it was refined at 56 V and 4500 A for 15 minutes, remelted at 55 V and 5000 A for 250 minutes, and fed at 30 V and 3000 A for 60 minutes. The ingot was cooled with the furnace for 52 minutes and demolded to obtain a φ360 mm alloy steel ingot. The forming effect of the bottom of the alloy steel ingot is similar to that of the Figure 1 similar.

[0039] Application Example 3 This application embodiment provides a method for using the electroslag remelting slag system provided in Embodiment 3, comprising the following steps: 1 ton of φ250 mm R26 alloy electrode rod (chemical composition as shown in Table 1) was placed in the crystallizer, and the arc was started (voltage was 68 V, current was 6500 A), and 38 kg of baked electroslag remelting slag system was added. After 15 minutes of addition, it was refined at 68 V and 6500 A for 10 minutes, and then remelted at 65 V and 6500 A for 200 minutes. The steel ingot was fed at 38 V and 3800 A for 43 minutes, and then cooled with the furnace for 55 minutes. After demolding, a φ360 mm alloy steel ingot was obtained. The forming effect of the bottom of the alloy steel ingot is similar to that of the Figure 1 similar.

[0040] Application Example 4 This application example provides a method for using the electroslag remelting slag system provided in Example 4. The specific steps are similar to those in Application Example 1, except that the electroslag remelting slag system provided in Example 1 is replaced by the electroslag remelting slag system provided in Example 4. The remaining operations are the same as those in Application Example 1 and will not be described in detail. Figure 1 similar.

[0041] Application Example 5 This application example provides a method for using the electroslag remelting slag system provided in Example 5. The specific steps are similar to those in Application Example 1, except that the electroslag remelting slag system provided in Example 1 is replaced by the electroslag remelting slag system provided in Example 5. The remaining operations are the same as those in Application Example 1 and will not be described in detail. Figure 1 similar.

[0042] Comparative application example 1 This comparative application example provides a method for using an electroslag remelting slag system. The specific steps are similar to those of application example 1, except that the electroslag remelting slag system provided in example 1 is replaced with the electroslag remelting slag system provided in comparative example 1. The remaining operations are the same as those of application example 1 and will not be described in detail. Figure 2 shown.

[0043] Comparative Application Example 2 This comparative application example provides a method for using an electroslag remelting slag system. The specific steps are similar to those of application example 1, except that the electroslag remelting slag system provided in example 2 is replaced by the electroslag remelting slag system provided in comparative example 2. The remaining operations are the same as those in application example 2 and will not be described in detail. Figure 1 similar.

[0044] Comparative Application Example 3 This comparative application example provides a method for using an electroslag remelting slag system. The specific steps are similar to those of application example 3, except that the electroslag remelting slag system provided in example 3 is replaced by the electroslag remelting slag system provided in comparative example 3. The remaining operations are the same as those of application example 3 and will not be described in detail. Figure 2 similar.

[0045] Performance Testing The large head (bottom) and small head (upper part) of the alloy steel ingots provided in Application Examples 1 to 5 of the present invention and Comparative Application Examples 1 to 3 were sampled and analyzed to obtain the mass percentage of aluminum element. The test results are shown in Table 2.

[0046] The alloy steel ingots provided in Application Examples 1 to 5 of the present invention and Comparative Application Examples 1 to 3 were forged into alloy rods with a diameter of φ130 mm, respectively. The mechanical properties of the alloy rods were tested in accordance with standard Q / ZHSD-012-2024. The test results are shown in Table 2.

[0047] Table 2 Test results of alloy steel ingots and alloy rods provided by application examples and comparative application examples

[0048] From Table 1~2 and Figure 1~2It can be seen that the alloy steel ingots smelted by the traditional electroslag remelting slag system of R26 alloy (Comparative Example 1 and Comparative Example 3) have serious aluminum increase in the big head; and the remelting slag system for R26 alloy electroslag production provided by the present invention can solve the problem of serious aluminum increase in the big head of the alloy steel ingot, and the difference in Al element content between the big and small heads is less than 0.04%. In addition, the use of CaO instead of Al2O3 in the slag lowers the melting point of the slag system and reduces the viscosity. The slag melts more fully and has better fluidity in the early stage of smelting. Therefore, under the same process parameters, the electroslag remelting slag system provided by the present invention can effectively improve the surface quality of the bottom of the steel ingot, with less grinding, which effectively ensures the smooth progress of subsequent hot processing. Comparative Example 2 Compared with the chemical composition of the electroslag remelting slag system provided by the present invention, the CaF2 content is increased and the CaO content is reduced, and the surface quality of the steel ingot smelted is qualified. This is because the increase in the CaF2 ratio further reduces the melting point of the slag system, and at the same time, the viscosity of the slag system is reduced and the fluidity is enhanced. Because the slag system does not contain Al2O3, the large head of the steel ingot does not increase aluminum; but because the viscosity of the slag system is too low and the fluidity is too good, the surface of the liquid slag cannot form a semi-solidified film, which makes it easy to absorb oxygen in the slag system. As a result, at the end of the steel ingot smelting, the slag pool in the crystallizer is closer to the atmosphere, causing serious burning of small head aluminum, and then leading to uneven composition and performance of the large and small heads of the steel ingot. The difference in Al element content of the large and small heads is 0.07%. In addition, a high proportion of CaF2 will cause the conductivity of the slag system to be too high, thereby reducing the smelting efficiency and increasing the smelting cost.

[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An electroslag remelting slag system, characterized in that: It includes the following chemical components in mass percentage: CaF2 63%~70%, CaO 12%~18%, MgO 10%~16% and TiO2 3%~6%.

2. The electroslag remelting slag system according to claim 1, characterized in that: The electroslag remelting slag system is a quaternary slag system, which is composed of the following chemical components in percentage by mass: CaF2 65%-70%, CaO 13%-16%, MgO 12%-15% and TiO2 3%-5%.

3. Use of the electroslag remelting slag system according to claim 1 or 2 in electroslag remelting of high-titanium and low-aluminum alloys.

4. The use of the electroslag remelting slag system according to claim 3 in electroslag remelting of high-titanium and low-aluminum alloys, characterized in that: The high titanium and low aluminum alloy is R26 alloy.

5. The method for using the electroslag remelting slag system according to claim 1 or 2, characterized in that: The following steps are involved: The electrode rod is placed in the crystallizer, power is supplied to start the arc, the electroslag remelting slag system is added, and refining, steady-state remelting and ingot shrinkage feeding are carried out in sequence to obtain an alloy steel ingot.

6. The method for using the electroslag remelting slag system according to claim 5, characterized in that: The electrode rod is an R26 alloy electrode rod.

7. The method for using the electroslag remelting slag system according to claim 5, characterized in that: The amount of the electroslag heavy melting slag system added is 33kg~38kg; The adding time of the electroslag remelting slag system is 10min~15min.

8. The method for using the electroslag remelting slag system according to claim 5, characterized in that: The voltage of the power transmission arc starting is 56V~68V, and the current of the power transmission arc starting is 4500A~6500A; The refining voltage is 56V~68V, the refining current is 4500A~6500A, and the refining time is 10min~15min.

9. The method for using the electroslag remelting slag system according to claim 5, characterized in that: The voltage of the steady-state remelting is 55V~65V, the current of the steady-state remelting is 5000A~6500A, and the time of the steady-state remelting is 200min~250min; The voltage of the steel ingot shrinkage compensation is 30V~38V, the current of the steel ingot shrinkage compensation is 3000A~3800A, and the time of the steel ingot shrinkage compensation is ≥40min.

10. The method for using the electroslag remelting slag system according to claim 5, characterized in that: After the shrinkage compensation of the steel ingot is completed, the ingot is cooled in the furnace; the time of the cooling in the furnace is ≥50min.