Method for recovering tungsten in tungsten-containing waste
By using manganese-containing compounds as additives in tungsten waste materials for calcination, the tungsten substance that is difficult to leaching is transformed into easy to leaching manganese tungstate, which solves the problems of low recovery rate and high cost in the prior art, and achieves high efficiency and low cost tungsten resource recycling.
Patent Information
- Application Number
- CN202411032853.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing tungsten-containing waste recycling methods have problems such as complex process flow, low recovery rate, high slag and high treatment cost, especially the high cost and environmental pollution of saltpeter smelting method and oxidative roasting soda leaching method, as well as the amount used when introducing additives High and low production efficiency problems.
The manganese-containing compounds are used as additives and tungsten waste materials to calcinate them, and the tungsten substances that are difficult to leach are easily leached manganese tungstenate, and leaching them during the alkali leaching process to reduce the tungsten content and additive usage of alkali leaching slag. Control the calcination temperature and time to improve recovery rate.
It realizes efficient recycling of tungsten at low additive dosage, improves recovery rate, reduces production costs, avoids equipment furnace stasis problems, simplifies process flow, and improves production efficiency.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling tungsten-containing waste, and in particular to a method for recycling tungsten in tungsten-containing waste. Background Art
[0002] At present, the main methods for recovering tungsten from tungsten-containing waste are saltpeter smelting method and oxidation roasting alkali leaching method, but both methods have certain problems:
[0003] (1) The saltpeter smelting method uses saltpeter as an oxidant to convert tungsten carbide in tungsten-containing waste into sodium tungstate at high temperature, while other impurity elements are oxidized into their metal oxides that are insoluble in water, thereby achieving the purpose of recovering tungsten. This method has a long industrial process, uses expensive raw and auxiliary materials, has high production costs, and the exhaust gas pollutes the environment. In addition, the recovery rate of the saltpeter smelting method is low.
[0004] (2) Oxidation roasting and alkali leaching is a method in which tungsten-containing waste is converted into tungsten oxide by oxidation roasting. During the alkali leaching process, the tungsten oxide reacts to form sodium tungstate and enters the solution, thereby achieving the purpose of recovering tungsten. During this method, the roasting equipment is severely blocked, the waste slag contains a high amount of tungsten, the recovery rate is low, and the cost of secondary slag treatment is high.
[0005] It can be seen that in the existing methods of leaching sodium tungstate from tungsten-containing waste, there are generally problems such as complex process flow, low recovery rate, high tungsten content in slag, and high processing cost.
[0006] In addition, the prior art also reports methods of introducing additive treatment, such as introducing magnesium-containing additives to improve the recovery rate of tungsten, but the amount of magnesium-containing additives used in this process is 1.1-4 times that of tungsten-containing waste. The high amount of magnesium-containing additives used leads to low production efficiency.
[0007] Therefore, there is an urgent need to develop a method for leaching sodium tungstate from tungsten-containing waste with a short process, high efficiency, cleanliness and low cost, so as to achieve the purpose of secondary efficient recovery and utilization of tungsten resources.
[0008] In view of this, the present invention is proposed. Summary of the invention
[0009] The object of the present invention is to provide a method for recovering tungsten from tungsten-containing waste, aiming to achieve efficient recovery of tungsten under the premise of low additive dosage and improve the recovery rate of tungsten.
[0010] The present invention is achieved in that:
[0011] In a first aspect, the present invention provides a method for recovering tungsten from tungsten-containing waste, comprising:
[0012] The tungsten-containing waste material is mixed with an additive to obtain a mixed material, the mixed material is calcined to obtain a calcined material, and the calcined material is mixed with a sodium hydroxide solution for reaction;
[0013] The additive is a manganese-containing compound, and the mass ratio of the manganese-containing compound to the tungsten-containing waste is 1: (10-100).
[0014] In an alternative embodiment, the manganese-containing compound is selected from at least one of manganese carbonate, manganese sulfate and manganese chloride.
[0015] In an optional embodiment, the mass ratio of the manganese-containing compound to the tungsten-containing waste is 1:(10-20).
[0016] In an optional embodiment, the mass fraction of tungsten in the tungsten-containing waste is 40%-98%;
[0017] Preferably, the tungsten-containing waste is powdered tungsten-containing waste with a particle size of 44 μm-149 μm.
[0018] In an optional embodiment, preferably, the tungsten-containing waste material is derived from at least one of a cemented carbide production process, a tungsten carbide powder production process, and a tungsten powder production process;
[0019] Preferably, the tungsten-containing waste material is selected from at least one of floor material, dust collection material, grinding material and scrap material.
[0020] In an optional embodiment, during the calcination process, the calcination temperature is controlled to be 300° C.-1000° C., and the calcination time is 1 h-24 h;
[0021] Preferably, the calcination temperature is controlled to be 400° C.-600° C., and the calcination time is controlled to be 1 h-3 h.
[0022] In an optional embodiment, the calcination process is carried out in an oxygen-containing atmosphere, and the furnace is turned over during the calcination process, with the furnace being turned over every 20 minutes to 40 minutes.
[0023] In an optional embodiment, the calcined material and the sodium hydroxide solution are mixed and reacted for 60 minutes to 180 minutes to obtain a solid-liquid mixture, and the solid-liquid mixture is subjected to solid-liquid separation to obtain a sodium tungstate solution.
[0024] In an optional embodiment, the concentration of the sodium hydroxide solution is 50 g / L-300 g / L;
[0025] Preferably, the mass ratio of the sodium hydroxide content in the sodium hydroxide solution to the tungsten-containing waste is 1:(1-6).
[0026] In an optional embodiment, the method further comprises: obtaining a sodium tungstate product by evaporating and crystallizing the sodium tungstate solution;
[0027] And / or, extracting or ion exchanging the sodium tungstate solution to obtain an ammonium tungstate solution, and then evaporating and crystallizing the ammonium tungstate solution to obtain an ammonium paratungstate product;
[0028] And / or, the sodium tungstate solution is extracted or ion exchanged to obtain an ammonium tungstate solution, and then the ammonium tungstate solution is evaporated and crystallized to obtain an ammonium paratungstate product, and the ammonium paratungstate product is calcined to obtain a tungsten oxide product.
[0029] The present invention has the following beneficial effects: by using manganese-containing compounds as additives to calcine with tungsten-containing waste, the tungsten-containing substances (tungsten, tungsten carbide, etc.) that are difficult to leach in the tungsten-containing waste are selectively converted into manganese tungstate that is easy to leach, and the tungsten-containing substances are leached in the form of sodium tungstate in the subsequent alkali leaching process, which effectively reduces the tungsten content of the alkali-leached tungsten slag and the amount of additives used. At the same time, during the calcination process, the problem of equipment furnace blockage is avoided, the production efficiency is improved, and the production cost is reduced. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0031] The embodiment of the present invention provides a method for recovering tungsten from tungsten-containing waste, comprising the following steps:
[0032] S1, Mixed
[0033] The tungsten-containing waste is mixed with an additive to obtain a mixture, wherein the additive is a manganese-containing compound. The inventor creatively uses the manganese-containing compound as an additive, and can convert the tungsten-containing substances (tungsten, tungsten carbide, etc.) that are difficult to leach from the tungsten-containing waste into manganese tungstate during the calcination process under the condition of a lower additive dosage.
[0034] In some embodiments, the manganese-containing compound is selected from at least one of manganese carbonate, manganese sulfate and manganese chloride, and the manganese-containing compound can be any one or more of the above. The mass ratio of the manganese-containing compound to the tungsten-containing waste is 1: (10-100), preferably 1: (10-20), and the amount of the manganese-containing compound within the above range can convert the tungsten-containing substances (tungsten, tungsten carbide, etc.) that are difficult to leach from the tungsten-containing waste into manganese tungstate during the calcination process.
[0035] Specifically, the mass ratio of the manganese-containing compound to the tungsten-containing waste can be 1:10, 1:15, 1:20, 1:30, 1:50, 1:80, 1:100, etc.
[0036] In some embodiments, the mass fraction of tungsten in the tungsten-containing waste is 40%-98%, and the tungsten content within the above range is suitable for recovering tungsten from the tungsten-containing waste using the method provided in the embodiment of the present invention. The tungsten-containing waste can be powdered tungsten-containing waste with a particle size of 44μm-149μm.
[0037] The source of tungsten-containing waste is not limited, and can be derived from at least one of the cemented carbide production process, the tungsten carbide powder production process, and the tungsten powder production process. In other words, the tungsten-containing waste can be derived from any one of the above processes, or a mixture of wastes obtained from the above processes.
[0038] Furthermore, the tungsten-containing waste is selected from at least one of floor materials, dust collection materials, grinding materials and waste materials, and the tungsten-containing waste can be any one or a mixture of several of the above waste forms.
[0039] S2. Calcination
[0040] The mixed material is calcined to obtain a calcined material for later use. During the calcination process, the tungsten-containing substances (tungsten, tungsten carbide, etc.) that are difficult to leach from the tungsten-containing waste are selectively converted into manganese tungstate that is easy to leach, and the conversion rate is very high, which can significantly improve the recovery rate of tungsten.
[0041] In some embodiments, during the calcination process, the calcination temperature is controlled to be 300°C-1000°C, and the calcination time is 1h-24h; preferably, the calcination temperature is controlled to be 400°C-600°C, and the calcination time is 1h-3h. By optimizing the calcination temperature and time, the tungsten-containing substances (tungsten, tungsten carbide, etc.) that are difficult to leach in the tungsten-containing waste are transformed into manganese tungstate that is easy to leach, thereby further improving the recovery rate of tungsten.
[0042] Specifically, the calcination temperature can be 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, etc.; the calcination time can be 1h, 2h, 3h, 5h, 10h, 15h, 20h, 24h, etc.
[0043] In some embodiments, the calcination process is carried out in an oxygen-containing atmosphere, such as an air-rich atmosphere. During the calcination process, the material can be fully contacted with the air by means of turning over or the like. In actual operation, the material can be turned over once every 20-40 minutes (such as 20 minutes, 30 minutes, 40 minutes, etc.) to ensure an air-rich atmosphere during the calcination process.
[0044] S3, alkali leaching
[0045] The calcined material is mixed with sodium hydroxide solution for reaction. During the alkaline leaching process, tungsten-containing substances such as manganese tungstate are leached out in the form of sodium tungstate, which effectively reduces the tungsten content of the alkaline leached tungsten slag and improves the recovery rate of tungsten.
[0046] In some embodiments, the calcined material is mixed with the sodium hydroxide solution for 60-180 minutes to obtain a solid-liquid mixture, and the solid-liquid mixture is subjected to solid-liquid separation to obtain a sodium tungstate solution, thereby achieving efficient recovery of tungsten. The solid-liquid separation method is not limited, and common filtering means can be used.
[0047] In some embodiments, the concentration of the sodium hydroxide solution is 50 g / L-300 g / L, such as 50 g / L, 100 g / L, 150 g / L, 200 g / L, 250 g / L, 300 g / L, etc. The mass ratio of the sodium hydroxide content in the sodium hydroxide solution to the tungsten-containing waste is 1:(1-6), such as 1:6, 1:3, 1:2, 1:1.5, 1:1.2, 1:1, etc. By further adjusting the concentration and dosage of the sodium hydroxide solution, tungsten can be leached more fully.
[0048] In some embodiments, the method for recovering tungsten further includes: obtaining a sodium tungstate product by evaporating and crystallizing the sodium tungstate solution. The sodium tungstate product can be obtained by evaporating and crystallizing the sodium tungstate solution, thereby increasing the added value of the product. It should be noted that the temperature and other conditions of the evaporation and crystallization are conventional operations in the art, and those skilled in the art can select them according to actual needs, which will not be repeated here.
[0049] In another embodiment, sodium tungstate solution is extracted or ion exchanged to obtain ammonium tungstate solution, and then the ammonium tungstate solution is evaporated and crystallized to obtain ammonium paratungstate product. Sodium tungstate solution is extracted or ion exchanged to obtain ammonium tungstate solution, and then the ammonium tungstate solution is evaporated and crystallized to obtain ammonium paratungstate product, thereby increasing the added value of the product. Among them, the extractant used for extraction can be selected from at least one of N235, TOA, Alamine-336, quaternary ammonium salts, etc., and the ion exchange resin used for ion exchange can be D201×7, Amberlite IRA-400, AB-17Π, Amberlite IRA-4200 and other strong basic anion exchange resins or AH-80Π and other weak basic anion exchange resins. It should be noted that the specific operation process of extracting sodium tungstate solution or ion exchange to obtain ammonium tungstate solution is conventional in the art under evaporation and crystallization conditions, which will not be repeated here.
[0050] In another embodiment, the sodium tungstate solution is extracted or ion exchanged to obtain an ammonium tungstate solution, and then the ammonium tungstate solution is evaporated and crystallized to obtain an ammonium paratungstate product, and the ammonium paratungstate product is calcined to obtain a tungsten oxide product. The specific instructions for obtaining the ammonium paratungstate product can refer to the above content and will not be repeated here. The ammonium paratungstate product can be further calcined to obtain a tungsten oxide product, thereby increasing the added value of the product.
[0051] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0052] It should be noted that in the following embodiments and comparative examples, the tungsten-containing waste is conventional commercially available tungsten-containing waste, and its composition includes: a tungsten mass content of 40% to 98%, and also contains other elements M, wherein M is selected from one or more of Fe, Cu, Ca, Zn, Ni, Mg, C, Ta, Co, Ti, Nb, Mn, Sn, Cr, V, K, Na, Zr, Pb, Mo, P, S, Al, and Si.
[0053] Example 1
[0054] This embodiment provides a method for recovering tungsten from tungsten-containing waste, comprising the following steps:
[0055] (1) Mixing: Take 300g of tungsten-containing waste, add manganese carbonate and mix evenly to obtain a mixture. The mass ratio of manganese carbonate to tungsten-containing waste is 1:10. The composition of the tungsten-containing waste is 81wt% tungsten, and the remainder is M. The particle size of the tungsten-containing waste is 44μm-149μm.
[0056] (2) Calcination: The mixed material prepared in step (1) is calcined at 500° C. in an air atmosphere for 2 h, and is continuously stirred during the calcination process at a frequency of 30 min / time to obtain a calcined material.
[0057] (3) Alkali leaching: the calcined material obtained in step (2) is added to 1 L of sodium hydroxide solution with a concentration of 200 g / L, and mixed and reacted for 120 min under stirring conditions to obtain a solid-liquid mixture. After solid-liquid separation, a sodium tungstate solution is obtained. The residue is dried, weighed, and the residual tungsten content is analyzed.
[0058] According to the test, the residual slag obtained in this embodiment contains 3.23% tungsten, and the recovery rate of tungsten is calculated to be 98.81%.
[0059] Example 2
[0060] This embodiment provides a method for recovering tungsten from tungsten-containing waste, which is different from Embodiment 1 only in that manganese carbonate is replaced with manganese sulfate of equal mass, and the rest is the same as Embodiment 1.
[0061] According to the test, the residual slag obtained in this embodiment contains 4.40% tungsten, and the recovery rate of tungsten is calculated to be 98.31%.
[0062] Example 3
[0063] This embodiment provides a method for recovering tungsten from tungsten-containing waste, which is different from Embodiment 1 only in that manganese carbonate is replaced with manganese chloride of equal mass, and the rest is the same as Embodiment 1.
[0064] According to the test, the residual slag obtained in this embodiment contains 5.49% tungsten, and the recovery rate of tungsten is calculated to be 97.83%.
[0065] Example 4
[0066] This embodiment provides a method for recovering tungsten from tungsten-containing waste. The only difference from Embodiment 1 is that the mass ratio of manganese carbonate to tungsten-containing waste is replaced from 1:10 to 1:20, and the rest is the same as Embodiment 1.
[0067] According to the test, the residual slag obtained in this embodiment contains 3.94% tungsten, and the recovery rate of tungsten is calculated to be 98.52%.
[0068] Example 5
[0069] This embodiment provides a method for recovering tungsten from tungsten-containing waste. The only difference from Embodiment 1 is that the mass ratio of manganese carbonate to tungsten-containing waste is replaced from 1:10 to 1:50, and the rest is the same as Embodiment 1.
[0070] According to the test, the residual slag obtained in this embodiment contains 5.48% tungsten, and the recovery rate of tungsten is calculated to be 97.81%.
[0071] Example 6
[0072] This embodiment provides a method for recovering tungsten from tungsten-containing waste. The only difference from Embodiment 1 is that the mass ratio of manganese carbonate to tungsten-containing waste is replaced from 1:10 to 1:100, and the rest is the same as Embodiment 1.
[0073] According to the test, the residual slag obtained in this embodiment contains 7.78% tungsten, and the recovery rate of tungsten is calculated to be 97.15%.
[0074] Example 7
[0075] This embodiment provides a method for recovering tungsten from tungsten-containing waste. The only difference from Embodiment 1 is that the composition of the tungsten-containing waste is 40wt% tungsten, and the remainder is M. The rest is the same as Embodiment 1.
[0076] According to the test, the residual slag obtained in this embodiment contains 3.87% tungsten, and the recovery rate of tungsten is calculated to be 98.39%.
[0077] Example 8
[0078] This embodiment provides a method for recovering tungsten from tungsten-containing waste. The only difference from Embodiment 1 is that the composition of the tungsten-containing waste is 98wt% tungsten, and the remainder is M. The rest is the same as Embodiment 1.
[0079] According to the test, the residual slag obtained in this embodiment contains 3.83% tungsten, and the recovery rate of tungsten is calculated to be 98.63%.
[0080] Comparative Example 1
[0081] This comparative example provides a method for recovering tungsten from tungsten-containing waste, which differs from Example 1 only in that step (1) is not performed, i.e., no additive is added. The specific steps are as follows:
[0082] (1) Calcination: 300 g of tungsten-containing waste was calcined at 500° C. in an air atmosphere for 2 h, and the waste was continuously turned over during the calcination process at a frequency of 30 min / time to obtain a calcined material.
[0083] (2) Alkali leaching: the calcined material obtained in step (1) is added to 1 L of a sodium hydroxide solution having a concentration of 200 g / L, and mixed and reacted for 120 min under stirring conditions to obtain a solid-liquid mixture. After solid-liquid separation, a sodium tungstate solution is obtained. The residue is dried, weighed, and the residual tungsten content is analyzed.
[0084] According to the test, the residual slag obtained in this embodiment contains 31.17% tungsten, and the recovery rate of tungsten is calculated to be 80.41%.
[0085] Comparative Example 2
[0086] This comparative example provides a method for recovering tungsten from tungsten-containing waste, which is different from Example 1 only in that manganese carbonate is replaced with an equal mass of manganese dioxide, and the rest is the same as Example 1.
[0087] The test showed that the residual slag obtained in this comparative example contained 26.76% tungsten, and the recovery rate of tungsten was calculated to be 86.47%.
[0088] Comparative Example 3
[0089] This comparative example provides a method for recovering tungsten from tungsten-containing waste, which is different from Example 1 only in that manganese carbonate is replaced with potassium permanganate of equal mass, and the rest is the same as Example 1.
[0090] The test showed that the residual slag obtained in this comparative example contained 23.14% tungsten, and the recovery rate of tungsten was calculated to be 87.65%.
[0091] Comparative Example 4
[0092] This comparative example provides a method for recovering tungsten from tungsten-containing waste. The only difference from Example 1 is that the mass ratio of manganese carbonate to tungsten-containing waste is replaced from 1:10 to 1:200, and the rest is the same as Example 1.
[0093] According to the test, the residual slag obtained in this embodiment contains 19.12% tungsten, and the recovery rate of tungsten is calculated to be 91.44%.
[0094] Comparative Example 5
[0095] This comparative example provides a method for recovering tungsten from tungsten-containing waste, which is different from Example 1 only in that the mass ratio of manganese carbonate to tungsten-containing waste is replaced from 1:10 to 1:5, and the rest is the same as Example 1.
[0096] The test showed that the residual slag obtained in this comparative example contained 26.38% tungsten, and the recovery rate of tungsten was calculated to be 86.27%.
[0097] The results are analyzed as follows:
[0098] From the comparison results of the recovery rates of tungsten in Comparative Example 1 and Examples 1, 2 and 3, it can be seen that when calcined without adding additives, the recovery rate of tungsten is only 80.41%. When manganese carbonate, manganese sulfate and manganese chloride in manganese-containing compounds are used as additives for calcination, the tungsten-containing substances (tungsten, tungsten carbide, etc.) that are difficult to leach in the tungsten-containing waste can be selectively converted into manganese tungstate that is easy to leach. In the subsequent alkali leaching process, the tungsten-containing substances are leached in the form of sodium tungstate, which can increase the recovery rate of tungsten to more than 95%.
[0099] During the reaction, the generated gas stirs the material, which is beneficial to the reaction. From the comparison of the recovery rates of tungsten in Comparative Examples 2 and 3 with those in Example 1, it can be seen that when manganese carbonate is used as an additive for calcination, more carbon dioxide gas is generated during the reaction to stir the material, thereby promoting the full progress of the reaction, and ultimately making the recovery rate of tungsten better than that of manganese dioxide and potassium permanganate as additives.
[0100] From the comparison of the recovery rates of tungsten in Comparative Examples 4 and 5 with Example 1, it can be seen that when the mass ratio of the added additive to the tungsten-containing waste is too low or too high, the recovery rate of tungsten decreases. Therefore, it is appropriate to control the mass ratio of the additive to the tungsten-containing waste to be 1:100-1:10.
[0101] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for recovering tungsten from tungsten-containing waste, It is characterized in that include: The tungsten-containing waste material is mixed with an additive to obtain a mixed material, the mixed material is calcined to obtain a calcined material, and the calcined material is mixed with a sodium hydroxide solution for reaction; Wherein, the additive is a manganese-containing compound, and the mass ratio of the manganese-containing compound to the tungsten-containing waste is 1:(10-100).
2. The method according to claim 1, It is characterized in that The manganese-containing compound is selected from at least one of manganese carbonate, manganese sulfate and manganese chloride.
3. The method according to claim 1 or 2, It is characterized in that The mass ratio of the manganese-containing compound to the tungsten-containing waste is 1:(10-20).
4. The method according to claim 1, It is characterized in that The mass fraction of tungsten in the tungsten-containing waste is 40%-98%; Preferably, the tungsten-containing waste is powdered tungsten-containing waste with a particle size of 44 μm-149 μm.
5. The method according to claim 4, It is characterized in that The tungsten-containing waste material is derived from at least one of a cemented carbide production process, a tungsten carbide powder production process, and a tungsten powder production process; Preferably, the tungsten-containing waste is selected from at least one of floor materials, dust collection materials, grinding materials and waste materials.
6. The method according to claim 1, It is characterized in that During the calcination process, the calcination temperature is controlled to be 300°C-1000°C, and the calcination time is 1h-24h; Preferably, the calcination temperature is controlled to be 400° C.-600° C., and the calcination time is controlled to be 1 h-3 h.
7. The method according to claim 6, It is characterized in that The calcination process is carried out in an oxygen-containing atmosphere, and the pellets are turned over during the calcination process, with each turn being performed every 20 minutes to 40 minutes.
8. The method according to claim 1, It is characterized in that The calcined material and the sodium hydroxide solution are mixed and reacted for 60 minutes to 180 minutes to obtain a solid-liquid mixture, and the solid-liquid mixture is subjected to solid-liquid separation to obtain a sodium tungstate solution.
9. The method according to claim 8, It is characterized in that The concentration of the sodium hydroxide solution is 50g / L-300g / L; Preferably, the mass ratio of the sodium hydroxide content in the sodium hydroxide solution to the tungsten-containing waste is 1:(1-6).
10. The method according to claim 8, It is characterized in that Also includes: The sodium tungstate solution is evaporated and crystallized to obtain a sodium tungstate product; And / or, extracting or ion exchanging the sodium tungstate solution to obtain an ammonium tungstate solution, and then evaporating and crystallizing the ammonium tungstate solution to obtain an ammonium paratungstate product; And / or, the sodium tungstate solution is extracted or ion exchanged to obtain an ammonium tungstate solution, and then the ammonium tungstate solution is evaporated and crystallized to obtain an ammonium paratungstate product, and the ammonium paratungstate product is calcined to obtain a tungsten oxide product.
Citation Information
Patent Citations
Method for recovering valuable metal from electrode waste
CN113957247A
Method for leaching tungsten and molybdenum and application
CN113981207A
Comprehensive utilization and treatment method for wolframite resources
CN114477288A
Method for recovering tungsten or cobalt from cemented carbide powder
JP2013204068A
Method for recovery of tungsten from manganese-tungstate concentrate
RU2024638C1