Preparation method of ardealite aggregate, product of ardealite aggregate and application of ardealite aggregate in road water-stable layer
By preparing high-strength phosphogypsum aggregates, the high cost of phosphogypsum treatment and resource utilization problems are solved, the efficient utilization and environmental protection of phosphogypsum are achieved, the cost of road construction is reduced, and the cost of roads has significant economic and social value.
Patent Information
- Application Number
- CN202310576634.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-22
AI Technical Summary
The existing phosphogypsum treatment process is high and the amount of phosphogypsum is small, making it difficult to achieve resource utilization of phosphogypsum. In addition, a large amount of natural gravel is needed in road construction, which affects the ecological environment.
High-strength phosphogypsum aggregate is prepared using phosphogypsum, slag micro powder, cement and calcium oxide. By controlling the use of alkaline exciter components and cationic starch, high-strength phosphogypsum aggregate is successfully prepared to replace water stability The gravel in the layer reduces the cost of road construction and realizes the resource utilization of phosphogypsum.
It has achieved high strength and high amount of phosphogypsum aggregate, reduced the cost of phosphogypsum treatment, reduced the collection of natural gravel, protected the environment, met the requirements of sustainable development, and had broad market prospects and economic value.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of highway transportation, especially the field of highway construction materials, and specifically to a method for preparing phosphogypsum aggregate, its product and its application in road water-stabilizing layer. The present application uses phosphogypsum as the main raw material, successfully prepares high-strength phosphogypsum aggregate, and uses it in road water-stabilizing layer, which is conducive to reducing the accumulation of phosphogypsum and reducing the cost of road construction, and has significant economic and social value. Background Art
[0002] At present, my country's highway mileage is far ahead of other countries and ranks first in the world. According to the national highway network plan, in the next ten years, my country's highway construction (including highways) will still be an important part of my country's infrastructure construction. Road construction requires a large amount of crushed stone, and the current ways to obtain crushed stone are mainly mountain excavation and river collection. As a non-renewable resource, large-scale collection of natural crushed stone will inevitably have a certain impact on the ecological environment and is not in line with my country's sustainable development strategy. In order to meet the needs of highway construction and reduce damage to the environment, it is necessary to find new recycled aggregates to replace the crushed stone required for road engineering.
[0003] On the other hand, as an industrial by-product, phosphogypsum is currently mainly disposed of in open-air dumping due to its excessive production. This method not only requires a large amount of land, but also long-term dumping may pollute groundwater, soil and air, damage the ecological environment, and affect and hinder the sustainable development of the phosphorus chemical industry.
[0004] A lot of research has been conducted both at home and abroad to solve the problem of phosphogypsum treatment. At present, the existing phosphogypsum treatment process still has the following problems: (1) the cost of phosphogypsum harmless treatment process is high; (2) the amount of phosphogypsum in phosphogypsum products is small. How to reduce the cost of phosphogypsum treatment and develop phosphogypsum products with high added value and high phosphogypsum content is the key to solving the problem of phosphogypsum resource utilization.
[0005] Based on the characteristics of phosphogypsum, some studies have been conducted on its use in road construction. Studies from the University of Florida and the University of Miami in the United States have shown that the mixture made by adding a certain amount of clay sand to phosphogypsum is an excellent roadbed filler. Research from Southwest Jiaotong University has shown that the comprehensive performance of the roadbed made of phosphogypsum-modified soil filler has reached the indicators of a secondary highway, and has no obvious dynamic fatigue characteristics. Wuhan University of Technology has confirmed through experiments that the mechanical properties of phosphogypsum-modified fly ash materials are generally enhanced at all times. Experiments conducted by Southeast University have shown that a reasonable amount of phosphogypsum can replace part of the raw materials of the original fly ash crushed stone to a certain extent, and can effectively save highway construction costs while ensuring the road performance of the mixture.
[0006] One type of road base uses a cement-stabilized graded gravel base, referred to as a water-stable layer. It uses graded gravel as aggregate, uses a certain amount of gel material and a sufficient volume of mortar to fill the gaps in the aggregate, and is spread and compacted according to the principle of interlocking. The inventor found that the amount of graded gravel required for the water-stable layer is extremely large. If products prepared from phosphogypsum can be used to replace the gravel in the existing water-stable layer, it can not only solve the problem that road construction requires a large amount of gravel and affects the ecological environment, but also realize the resource utilization of phosphogypsum, which is of great significance and value. To this end, the inventor conducted in-depth research and finally obtained the technical solution of this application. Summary of the invention
[0007] The purpose of the invention is to provide a method for preparing phosphogypsum aggregate, its product and its application in the road water-stabilizing layer in view of the above-mentioned problems. This application uses phosphogypsum as the main raw material, blast furnace slag powder and cement as composite gel materials, and alkaline activator mainly composed of calcium oxide. By controlling the alkaline activator components, high-strength phosphogypsum aggregate is successfully prepared. This application does not require sintering to prepare aggregates, which can effectively simplify the aggregate preparation process. On the basis of the prepared phosphogypsum aggregate, the inventor uses it in road construction, which can be used to replace the crushed stone of the water-stabilizing layer, and can also be used as a roadbed filler and a modified fly ash stabilized road base material. This application uses phosphogypsum aggregate as a highway base material, which has a wide source of raw materials, a huge demand for road construction, and has broad application prospects. The use of this application can effectively reduce the cost of road construction and realize the resource utilization of phosphogypsum, which is of great significance for protecting the environment, reducing environmental pollution, and achieving sustainable development.
[0008] In order to achieve the above object, the present invention adopts the following technical solution: A method for preparing phosphogypsum aggregate comprises the following steps: (1) drying the phosphogypsum to obtain dried phosphogypsum; (2) Weighing the powders of each component according to the ratio, mixing and stirring the weighed powders of each component to form a first intermediate; (3) placing the prepared first intermediate into a mold of a pressure gauge for pressing, and compacting the mixture into a block, which is recorded as the second intermediate; (4) Mechanically crushing the second intermediate obtained in step 3 to form a coarse aggregate, which is recorded as a third intermediate; (5) Screening the third intermediate to obtain aggregate blanks with different particle sizes; (6) curing the aggregate blank obtained in step 5 at room temperature and a humidity of ≥70%; after the curing is completed, phosphogypsum aggregate is obtained; In step 2, the mass percentage of each component is as follows: 55-65wt% phosphogypsum, 20-30wt% slag powder, 8-10wt% formed cement, 0.5-1.5wt% calcium oxide, 1.5-2.5wt% ammonium sulfate, 1.5-2.5wt% sodium silicate, and 1-3wt% cationic starch.
[0009] In the step 1, the water content of the dried phosphogypsum is ≤5wt%.
[0010] The mass ratio of ammonium sulfate to sodium silicate is 1:0.9-1.2.
[0011] The molding cement is PO42.5.
[0012] In step 6, the room temperature is 5-40° C., and the curing time is 1 d to 10 d.
[0013] The product prepared by the above-mentioned method for preparing phosphogypsum aggregate.
[0014] The application of the aforementioned phosphogypsum aggregate in road water-stabilizing layer.
[0015] It includes phosphogypsum aggregate with a particle size of 9.5 to 19 mm and phosphogypsum aggregate with a particle size of 4.75 to 9.5 mm.
[0016] The phosphogypsum aggregate with a particle size of 9.5 to 19 mm was recorded as coarse aggregate, and the phosphogypsum aggregate with a particle size of 4.75 to 9.5 mm was recorded as fine aggregate; In the warm water layer of the road, the mass ratio of fine aggregate to coarse aggregate is 1:2~5.
[0017] In response to the above-mentioned problems, the present application provides a preparation method, product and application of phosphogypsum-based concrete solid bricks. In the present application, phosphogypsum aggregate is prepared using raw materials including the following components: phosphogypsum, slag powder, formed cement, calcium oxide, ammonium sulfate, sodium silicate, and cationic starch. Among them, phosphogypsum is used as the main raw material, blast furnace slag powder and cement are used as composite gel materials (blast furnace slag powder is based on steel slag and is a secondary recycled product of waste), supplemented by an alkaline activator mainly composed of calcium oxide. By controlling the components of the alkaline activator, high-strength phosphogypsum aggregate is successfully prepared.
[0018] Under normal conditions, slag powder contains a large amount of glass. After contact with water, the weakest Ca-O bond in the glass breaks, and the alkaline activator increases the pH value of the solution, accelerating the dissociation of Si-O and Al-O structures in the glass, generating silicate ions and aluminate ions, which react with the Ca2+ ions released by the slag hydrolysis. 2+Reaction to generate hydrated calcium silicate and tricalcium aluminate; tricalcium aluminate reacts with gypsum to generate hydraulic ettringite; in addition, slag hydration produces hydrated calcium silicate gel (CSH gel). A small amount of hydraulic ettringite can fill the pores to reduce the shrinkage of the system and has almost no effect on the strength, but too much alkali activator will generate more hydraulic ettringite, causing the system to expand and generate greater internal stress, and then the strength will decrease with the increase of alkali activator. The structure of hydraulic ettringite will be destroyed under the evaporation of water over a long period of time, thereby reducing the strength.
[0019] In the present application, a method of controlling the amount of calcium oxide added and doping part of the cationic starch is adopted. When preparing the phosphogypsum aggregate, the components are evenly mixed together, and the cationic starch is evenly coated on the phosphogypsum. When the aggregate blank is prepared and cured in a high humidity environment, the phosphogypsum dissolves sulfate anions in water, which will adsorb with the cationic starch of the coating layer, thereby preventing the sulfate ions from hydrating with cement to form calcium sulfate. It should be noted that the present application does not use an external heat source to gelatinize the cationic starch, but gelatinizes the cationic starch based on the heat generated by the pyrolysis of calcium oxide in a high humidity environment. In this way, not only can the heat consumption required for heating and gelatinization be reduced, but also after gelatinization, mixing will cause the uniformity of the material to deteriorate, making the overall strength of the prepared phosphogypsum aggregate unstable. Based on the improved method, the problem of uneven mixing of phosphogypsum aggregate raw materials is solved, the energy consumption is reduced, and it is gelatinized after obtaining the aggregate blank, and the prepared phosphogypsum aggregate has higher strength and more stability. At the same time, the present application is doped with part of ammonium sulfate and sodium silicate; on the one hand, ammonium sulfate, sodium silicate and calcium oxide jointly act as stimulators; on the other hand, the test results show that there is an obvious synergistic effect between ammonium sulfate, sodium silicate, calcium oxide and components such as phosphogypsum and slag powder, which can effectively solidify calcium ions, inhibit the further dissolution of phosphogypsum in water, and improve the strength of phosphogypsum aggregate.
[0020] Based on the improved scheme, the phosphogypsum content in the phosphogypsum aggregate of the present application is greater than 40%, and the compressive strength of the phosphogypsum aggregate is greater than the strength of the diagenetic rock (not less than 30MPa). Furthermore, the present application successfully avoids the purification process of phosphogypsum, avoids the pollution of the environment by harmful components in phosphogypsum, and has a high utilization rate of phosphogypsum, which opens up a new way for phosphogypsum emission enterprises to comprehensively utilize phosphogypsum.
[0021] For the prepared phosphogypsum aggregate, the particle size distribution of the aggregate gradation is calculated by the "n" method in the maximum density theory method according to the dense gradation particle group recommended in the "Highway Engineering Aggregate Test Code" (JTG E42-2005), and the aggregate gradation with different proportions is designed by controlling the proportion of coarse particles. The test results show that the phosphogypsum aggregate prepared by this application meets the strength requirements of the water-stabilized layer of highways at or below the second level in the "Highway Asphalt Pavement Design Code" (JTG D50-2017).
[0022] Due to the adoption of the above technical solution, the beneficial effects of the present invention are: (1) In the present application, the raw materials used for the preparation of phosphogypsum aggregate are cheap and sintering is not required, so the manufacturing cost of phosphogypsum aggregate is low; at the same time, the large-scale application of phosphogypsum (phosphogypsum dosage>40%) can not only reduce the waste disposal cost of the phosphorus chemical industry, but also increase the added value generated by the phosphorus chemical industry, and has broad market prospects; (2) The adoption of this application can effectively solve the problem of resource utilization of phosphogypsum, open up a new way for resource utilization of phosphogypsum, and meet the requirements of circular economy and resource conservation and comprehensive utilization; (3) The phosphogypsum aggregate of the present application can be used not only for the preparation of concrete solid bricks, but also for the preparation of the water-stabilizing layer of the highway in the present application, thereby reducing the mining and use of natural gravel, effectively reducing the damage to the environment caused by gravel mining, and meeting the strength requirements of the water-stabilizing layer of secondary and lower highways, which is beneficial to reducing the cost of highway construction, increasing the added value of phosphorus chemical enterprises, improving the corresponding economic benefits, and promoting the healthy development of the phosphorus chemical industry. DETAILED DESCRIPTION
[0023] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0024] Any feature disclosed in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0025] In the examples of this application, phosphogypsum (PG) was purchased from a place in Sichuan and is in the form of gray powder, with CaSO4•2H2O as its main component. 42.5 Ordinary Portland cement was purchased from a place in Sichuan; sodium silicate pentahydrate (AR), ammonium sulfate (AR), and quicklime (AR) were purchased from a company in Tianjin. Blast furnace slag powder is a commercially available product, and its activity index detection method complies with the national standard GB / T18046-2008. The product characteristics are: specific surface area 480-580m 2 / kg, physical appearance is spherical; activity index 3d ≥ 90%, 7d ≥ 100%, 28d ≥ 110%; fluidity ratio ≥ 100%, water content (mass fraction) ≤ 1.0%, sulfur trioxide (mass fraction) ≤ 4.0%, chloride ion (mass fraction) ≤ 0.06%, loss on ignition (mass fraction) ≤ 3.0%.
[0026] PG and PO42.5 cements were tested respectively, and their chemical compositions are shown in Table 1 below.
[0027] Table 1 Chemical composition raw materials CaO / % <![CDATA[SO3 / %]]> SrO / % <![CDATA[SiO2 / %]]> <![CDATA[Al2O3 / %]]> <![CDATA[Fe2O3 / %]]> <![CDATA[P2O5 / %]]> <![CDATA[R2O / %]]> PG 30.85 31.85 - 4.65 4.2 - 3.22 0.32 PO 42.5 cement 65.34 4.63 - 19.43 4.88 1.2 0.04 0.27 raw materials <![CDATA[TiO2 / %]]> MgO / % BaO / % MnO / % ZnO / % <![CDATA[Zr2O / %]]> Cl / % PG 0.2 0.24 - - - - - PO 42.5 cement 0.06 0.61 0.43 - 0.02 0.02 0.04
[0028] Note: In Table 1, R2O represents an alkali metal oxide.
[0029] In this embodiment, since the phosphogypsum sample used is in the form of gray powder and has been dried, the corresponding drying step is omitted. In this embodiment, the curing temperature is 20-25°C; for ease of comparison, the curing time of all embodiments is 2 days, and the humidity of the curing box is 80-90%. After the curing of the phosphogypsum aggregate to be prepared is completed, the compressive strength at 3 days, 7 days, and 28 days is tested respectively.
[0030] The process of preparing phosphogypsum aggregate in the embodiment of the present application is as follows (wherein the mass percentage of each component in the phosphogypsum aggregate is shown in Table 2 below).
[0031] (1) Weigh the raw materials Weigh each component according to the ratio, mix and stir the weighed components to obtain a first intermediate.
[0032] (2) Pressing The prepared first intermediate is placed in a mold of a pressure gauge for pressing, and the mixture is compacted into a block, which is recorded as the second intermediate.
[0033] (3) Crushing The obtained second intermediate is mechanically crushed to form a coarse aggregate, which is recorded as the third intermediate.
[0034] (4) Screening The obtained third intermediate is sieved to obtain aggregate blanks with different particle sizes.
[0035] (5) Maintenance The obtained aggregate blank is cured in a curing box at room temperature and 80-90% humidity. After the curing is completed, phosphogypsum aggregate is obtained.
[0036] Table 2 Group distribution ratio in each embodiment Phosphogypsum (wt%) Slag differential (wt%) Cement (wt%) Calcium oxide (wt%) Ammonium sulfate (wt%) Sodium silicate (wt%) Cationic starch (wt%) Example 1 62 25 10 1 0 0 2 Example 2 61 25 10 2 0 0 2 Example 3 62 25 10 0 1 0 2 Example 4 60 25 10 0 3 0 2 Example 5 62 25 10 0 0 1 2 Example 6 60 25 10 0 0 3 2 Example 7 61 25 10 1 1 0 2 Example 8 60 25 8 1 2 2 2 Example 9 61 25 8 1 1.5 1.5 2 Example 10 55 28.5 9 1 2 2 2.5
[0037] The properties of the phosphogypsum aggregates prepared in Examples 1 to 10 above were tested, and the results are shown in Table 3.
[0037] Table 3 Compressive strength test results of phosphogypsum aggregate
[0038] Embodiment 11 The phosphogypsum aggregate prepared in Example 10 is taken as raw material, the phosphogypsum aggregate with a particle size of 0.475 to 9.5 mm is used as fine aggregate, and the phosphogypsum aggregate with a particle size of 9.5 to 19 mm is used as coarse aggregate.
[0039] Fine aggregate and coarse aggregate are graded in a ratio of 1:4, added into a mixer, and mixed thoroughly to form graded crushed stone.
[0040] Weigh the components according to the following weight ratio: 4 parts of PO325 cement, 10 parts of fly ash, and 86 parts of graded crushed stone; make the weighed components into a highway water-stabilizing layer and carry out maintenance. After the maintenance is completed, it is ready.
[0041] The highway water-stabilizing layer prepared in this embodiment was measured, and its 7d unconfined compressive strength was 4.7MPa, and its 28d unconfined compressive strength was 16.9MPa.
[0042] The above test results show that this application successfully prepared the corresponding highway water-stabilizing layer by grading phosphogypsum aggregates of different particle sizes, which can meet the strength requirements of the water-stabilizing layer of secondary and lower highways. At the same time, this application uses phosphogypsum as the main raw material, which accounts for a high proportion of the aggregate in the water-stabilizing layer, realizes the resource utilization of phosphogypsum, is conducive to reducing the cost of road construction, and has high economic value, social value, and broad application prospects.
[0043] The above description is only a specific embodiment of the present application, which is only used to illustrate the technical solution of the present invention, but not to limit it. The present invention extends to any new features or any new combination disclosed in this specification, as well as any new method or process steps or any new combination disclosed.
Claims
1. A method for preparing phosphogypsum aggregate, characterized in that: The steps include: (1) drying the phosphogypsum to obtain dried phosphogypsum; (2) Weighing the powders of each component according to the ratio, mixing and stirring the weighed powders of each component to form a first intermediate; (3) placing the prepared first intermediate into a mold of a pressure gauge for pressing, and compacting the mixture into a block, which is recorded as the second intermediate; (4) Mechanically crushing the second intermediate obtained in step 3 to form a coarse aggregate, which is recorded as a third intermediate; (5) Screening the third intermediate to obtain aggregate blanks with different particle sizes; (6) curing the aggregate blank obtained in step 5 at room temperature and a humidity of ≥70%; after the curing is completed, phosphogypsum aggregate is obtained; In step 2, the mass percentage of each component is as follows: 55-65wt% phosphogypsum, 20-30wt% slag powder, 8-10wt% formed cement, 0.5-1.5wt% calcium oxide, 1.5-2.5wt% ammonium sulfate, 1.5-2.5wt% sodium silicate, and 1-3wt% cationic starch.
2. The method for preparing phosphogypsum aggregate according to claim 1, characterized in that: In the step 1, the water content of the dried phosphogypsum is ≤5wt%.
3. The method for preparing phosphogypsum aggregate according to claim 1, characterized in that: The mass ratio of ammonium sulfate to sodium silicate is 1:0.9-1.
2.
4. The method for preparing phosphogypsum aggregate according to any one of claims 1 to 3, characterized in that: The molding cement is PO42.
5.
5. The method for preparing phosphogypsum aggregate according to any one of claims 1 to 4, characterized in that: In step 6, the room temperature is 5-40° C., and the curing time is 1 d to 10 d.
6. A product prepared by the method for preparing phosphogypsum aggregate according to any one of claims 1 to 5.
7. Use of the phosphogypsum aggregate according to claim 6 in a road water-stabilizing layer.
8. The use according to claim 7, characterized in that: It includes phosphogypsum aggregate with a particle size of 9.5 to 19 mm and phosphogypsum aggregate with a particle size of 4.75 to 9.5 mm.
9. The use according to claim 7 or 8, characterized in that: The phosphogypsum aggregate with a particle size of 9.5 to 19 mm was recorded as coarse aggregate, and the phosphogypsum aggregate with a particle size of 4.75 to 9.5 mm was recorded as fine aggregate; In the warm water layer of the road, the mass ratio of fine aggregate to coarse aggregate is 1:2~5.
Citation Information
Patent Citations
Solid waste-based unfired high-strength ceramsite and preparation method thereof
CN113200731A
Phosphogypsum-based aggregate and preparation method thereof
CN113354376A
Method for preparing cement-based wet-mixed mortar aggregate through phosphogypsum modification and mortar
CN113429145A
Preparation method of phosphogypsum high-strength aggregate
CN114907037A
Unfired artificial ardealite-based lightweight aggregate and preparation method thereof
CN115321865A
Cited By
Acid-excited RAP cold-recycled base material and preparation method thereof
CN121063895A
Phosphogypsum road water stable layer material and preparation method
CN122789683A