Cast aluminum alloy and preparation method and application thereof

By adjusting the elemental composition and process processing of aluminum alloys, an optimized microstructure structure is formed, which solves the problem of insufficient performance of traditional aluminum alloys in harsh environments, and achieves the improvement of the high-temperature mechanical properties of aluminum alloys, which are suitable for high-performance engine components.

CN118932224APending Publication Date: 2024-11-12HEBEI GANGYAN DEKAI TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411148764.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional Al-Si aluminum alloys are difficult to meet the performance requirements in strict service environments, especially in engine components applications, which are difficult to take into account excellent casting performance, room temperature and high temperature mechanical properties.

Method used

By adjusting the elemental composition of aluminum alloy, the content of Mn, Gd, Nd and Ti is increased, and specific smelting and heat treatment processes are used to form an optimized microstructure structure, including primary α-Al dendrites, eutectic silicon phases, Al2Cu, Al3Ti and rare earth compounds are subjected to solid solution and aging to optimize the mechanical properties of aluminum alloys.

Benefits of technology

It significantly improves the heat resistance and mechanical properties of aluminum alloy, meets the strict room temperature and high temperature strength and plasticity requirements, and is suitable for the manufacture of high-performance engine parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932224A_ABST
    Figure CN118932224A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloys, in particular to a cast aluminum alloy and a preparation method and application thereof. The invention discloses a cast aluminum alloy which comprises the following elements in percentage by mass: 10%-12% of Si, 2.8%-3.2% of Cu, 1%-1.4% of Mg, 2.5%-3.2% of Ni, 0.65%-0.8% of Fe, 0.6%-1% of Mn, 0.2%-2% of Gd, 0.8%-1.2% of Nd, 1%-3% of Ti and the balance of Al and inevitable impurities. According to the cast aluminum alloy disclosed by the invention, the contents of Mn, Gd, Nd and Ti are increased to a certain extent by reasonably regulating and controlling the alloy elements, and the structure and the performance of the alloy are remarkably influenced by the synergistic effect of the elements and other elements, so that the heat resistance and the mechanical property of the cast aluminum alloy are remarkably improved under the condition that the good casting performance of the cast aluminum alloy is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aluminum alloys, and in particular to a casting aluminum alloy and a preparation method and application thereof. Background Art

[0002] At present, the widely used cast aluminum alloys are mostly Al-Si based binary alloys and ternary or multi-element Al-Si alloys containing a small amount of Mg, Cu, Ni, rare earth and other elements. The melt fluidity and mold filling properties of Al-Si alloys are better than other alloys, and there is almost no casting cracks. In addition, the thermal expansion coefficient is small and the wear resistance is good.

[0003] With the increasing demands for lightweight development, energy conservation and emission reduction, and strict emission standards, the requirements for engines are also getting higher and higher. Core components such as engines made of traditional Al-Si alloys are difficult to meet the performance requirements in harsh service environments.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] An object of the present invention is to provide a cast aluminum alloy having excellent casting properties and room temperature and high temperature mechanical properties.

[0006] Another object of the present invention is to provide a method for preparing a cast aluminum alloy.

[0007] Another object of the present invention is to provide application of the cast aluminum alloy in manufacturing engine parts.

[0008] In order to achieve the above-mentioned object of the present invention, the present invention provides a casting aluminum alloy on the one hand, comprising the following elements in mass percentage:

[0009] Si 10%~12%, Cu 2.8%~3.2%, Mg 1%~1.4%, Ni 2.5%~3.2%, Fe0.65%~0.8%, Mn 0.6%~1%, Gd 0.2%~2%, Nd 0.8%~1.2%, Ti 1%~3%, and the balance is Al and unavoidable impurities.

[0010] In a specific embodiment of the present invention, the sum of the mass percentages of Gd and Nd is 1.2% to 2.5%. Further, the mass percentage ratio of Gd to Nd is 0.5 to 1.

[0011] In a specific embodiment of the present invention, the ratio of the sum of the mass percentages of Gd and Nd to the sum of the mass percentages of Cu and Mg is (Gd+Nd) / (Cu+Mg)=0.35-0.45.

[0012] In a specific embodiment of the present invention, the mass percentage ratio of Mn to Fe is 0.8 to 1.1.

[0013] In a specific embodiment of the present invention, the ratio of the sum of the mass percentages of Si and Cu to the mass percentage of Ti is (Si+Cu) / Ti=4.5-8.

[0014] Another aspect of the present invention provides a method for preparing any one of the above-mentioned cast aluminum alloys, comprising the following steps:

[0015] (a) Proportioning according to the stoichiometric ratio of cast aluminum alloy;

[0016] (b) melting the prepared raw materials to obtain aluminum alloy liquid;

[0017] (c) casting the aluminum alloy liquid to obtain a cast aluminum alloy casting.

[0018] In a specific embodiment of the present invention, the raw materials include industrial pure aluminum ingots, industrial pure magnesium ingots, Al-Si master alloys, Al-Cu master alloys, Al-Ni master alloys, Al-Fe master alloys, Al-Mn master alloys, Al-Gd master alloys, Al-Nd master alloys and Al-Ti master alloys.

[0019] In a specific embodiment of the present invention, the smelting includes: after melting the industrial pure aluminum ingot, adding the Al-Si master alloy at 760-780°C, after all are melted, adding Al-Cu master alloy, Al-Ni master alloy, Al-Fe master alloy, Al-Mn master alloy, Al-Gd master alloy, Al-Nd master alloy and part of Al-Ti master alloy at 780-800°C, after all are melted, adding industrial pure magnesium ingot at 740-750°C, after all are melted, refining at 700-740°C, after refining is completed, adding the remaining Al-Ti master alloy at 750-760°C, after all are melted, scooping and stirring to obtain alloy liquid.

[0020] In a specific embodiment of the present invention, the casting comprises: cooling the alloy liquid to 680-720° C. and pouring it into a mold.

[0021] In a specific embodiment of the present invention, in the smelting, the amount of the partial Al-Ti master alloy added before refining is 50% to 80% of the total amount of the Al-Ti master alloy.

[0022] In a specific embodiment of the present invention, the method further comprises: performing a solution treatment and an aging treatment on the cast aluminum alloy casting. Further, the solution treatment comprises: keeping the temperature at 510-530°C for 4-5 hours and then cooling with water; the aging treatment comprises: keeping the temperature at 170-180°C for 5-9 hours.

[0023] In a specific embodiment of the present invention, the cast microstructure of the casting includes primary α-Al dendrites, eutectic silicon phase, Al2Cu, Al3Ti, Q phase (ie Al5Cu2Mg8Si6) and rare earth compounds.

[0024] In a specific embodiment of the present invention, after the solution treatment and aging treatment, in the microstructure of the aluminum alloy casting, the average size of α-Al grains is ≤40 μm, and the average size of the eutectic silicon phase is ≤11.5 μm.

[0025] In a specific embodiment of the present invention, after the solution treatment and aging treatment, the performance of the aluminum alloy casting meets the following requirements: tensile strength ≥300MPa, yield strength ≥134MPa, and elongation ≥2% at room temperature; tensile strength ≥102MPa, yield strength ≥69MPa, and elongation ≥3.4% at 300°C.

[0026] Another aspect of the present invention provides use of any one of the above-mentioned cast aluminum alloys in manufacturing engine parts.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The cast aluminum alloy of the present invention increases the contents of Mn, Gd, Nd and Ti to a certain extent through reasonable regulation of alloying elements, which synergize with other elements to have a significant effect on the structure and properties of the alloy, so that the cast aluminum alloy significantly improves the heat resistance and mechanical properties while ensuring good casting performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 The as-cast metallographic structure of the cast aluminum alloy of Example 1 of the present invention;

[0031] Figure 2 This is the cast metallographic structure of the cast aluminum alloy of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0033] Al-Si alloys are important casting alloys and one of the most widely used materials in aluminum alloys. They are also important materials for the development of modern industry and play a pivotal role in strategic resources. Al-Si alloys have many excellent properties, such as casting performance, welding performance, thermal conductivity and electrical conductivity. However, with the increasing requirements for engine and other components, traditional Al-Si alloys are difficult to meet the new standards, resulting in great restrictions on the application of Al-Si alloys in new engine and other components.

[0034] Based on this, the present invention designs the element composition of Al-Si alloys and verifies through a large number of experiments, thereby obtaining a casting aluminum alloy that can significantly improve the heat resistance and mechanical properties while ensuring the casting performance.

[0035] In one aspect, the present invention provides a cast aluminum alloy, comprising the following elements in percentage by mass:

[0036] Si 10%~12%, Cu 2.8%~3.2%, Mg 1%~1.4%, Ni 2.5%~3.2%, Fe0.65%~0.8%, Mn 0.6%~1%, Gd 0.2%~2%, Nd 0.8%~1.2%, Ti 1%~3%, and the balance is Al and unavoidable impurities.

[0037] The cast aluminum alloy of the present invention increases the contents of Mn, Gd, Nd and Ti to a certain extent through reasonable regulation of alloying elements, which synergize with other elements to have a significant effect on the structure and properties of the alloy, so that the cast aluminum alloy significantly improves the heat resistance and mechanical properties while ensuring good casting performance.

[0038] The cast aluminum alloy of the present invention has a relatively high Mn content. A part of the Mn can eliminate the damage of Fe to the mechanical properties while ensuring a certain Fe content to prevent mold sticking; another part of the Mn can increase the number of nuclei, reduce the size of the eutectic, and improve the mechanical properties. Specifically, a part of the Mn can convert the aluminum-iron-silicon intermetallic compound into an aluminum-silicon-manganese-iron phase, eliminate the damage to the mechanical properties, and can produce solid solution strengthening on the alloy matrix while ensuring a certain Fe content to prevent mold sticking; another part of the Mn inhibits the large-sized lamellar binary β phase, promotes the formation of the α phase, weakens the harmful effects of the β phase, and the addition of Mn forms an α-Al 15 Mn3Si phase increases the number of nuclei, thereby reducing the size of the eutectic, which helps to improve the mechanical properties. When the amount of Mn added is too high, the number of aluminum-silicon-manganese-iron phases formed increases, and part of the Al / Si will be occupied by Cu, which reduces the Cu in the alloy matrix, thereby weakening the strengthening effect of Cu, resulting in poor performance; when the amount of Mn added is too low, it is impossible to fully eliminate the damage of Fe to the mechanical properties, and the reduction of the eutectic size is insufficient, and the mechanical properties cannot be effectively improved. For example, in the cast aluminum alloy of the present invention, the mass percentage of Mn can be 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1% or a range consisting of any two thereof; the mass percentage of Fe can be 0.65%, 0.7%, 0.75%, 0.8% or a range consisting of any two thereof.

[0039] In the cast aluminum alloy of the present invention, the addition of Gd and Nd refines the primary α phase, and the primary α-Al phase does not change significantly after heat treatment. In combination with the precipitation phase formed by Mg and Cu during the heat treatment process, the room temperature and high temperature strength of the alloy is greatly improved, and the alloy is guaranteed to have a certain plasticity. When the addition amount of Gd and / or Nd is too high, the alloy structure will become coarse, and the effect of refinement and performance improvement cannot be achieved, and the cost is high; when the addition amount of Gd and / or Nd is too low, the refinement effect is not obvious, and the improvement of the plastic part achieved cannot make up for the weakening of plasticity caused by the precipitation phase of Mg and Cu, and strength and plasticity cannot be taken into account. The present invention achieves the refinement effect by adding Gd and Nd, and the size will not change significantly during the heat treatment process. At this time, dislocations will not accumulate in the precipitation phase formed by Mg and Cu, and then will not cause excessive stress concentration, avoiding micro cracks and alloy fracture. For example, in the cast aluminum alloy of the present invention, the mass percentage of Gd can be 0.2%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.8%, 2% or a range consisting of any two of them; the mass percentage of Nd can be 0.8%, 0.9%, 1%, 1.1%, 1.2% or a range consisting of any two of them; the mass percentage of Mg can be 1%, 1.1%, 1.2%, 1.3%, 1.4% or a range consisting of any two of them; the mass percentage of Cu can be 2.8%, 2.9%, 3%, 3.1%, 3.2% or a range consisting of any two of them.

[0040] The cast aluminum alloy of the present invention, in combination with a certain amount of Ti, can refine the matrix of the alloy and improve the mechanical properties; at the same time, by adjusting Si and Cu, after heat treatment, Ti is promoted to form a dispersed Al3Ti phase and an intermetallic compound phase with Al, Si, Cu, etc., which plays a role in dispersion strengthening of the matrix. When the addition amount of Ti is too high, segregation is easily caused during the smelting and pouring process, affecting the grain refinement effect; when the addition amount of Ti is too low, sufficient dispersion strengthening cannot be achieved. For example, in the cast aluminum alloy of the present invention, the mass percentage of Ti can be 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3% or a range consisting of any two of them.

[0041] The present invention adopts a certain feeding time and method for the Al-Ti master alloy during the smelting process to ensure the uniformity of Ti distribution and significantly reduce segregation.

[0042] In a specific embodiment of the present invention, the sum of the mass percentages of Gd and Nd is 1.2% to 2.5%. Further, the ratio of the sum of the mass percentages of Gd and Nd to the sum of the mass percentages of Cu and Mg is (Gd+Nd) / (Cu+Mg)=0.35 to 0.45.

[0043] For example, in different embodiments, the sum of the mass percentages of Gd and Nd can be 1.2%, 1.4%, 1.5%, 1.8%, 2%, 2.2%, 2.5% or any two thereof. The total amount of Gd and Nd is further adjusted within the above range to give full play to the refinement effect of Gd and Nd and the improvement effect on plasticity.

[0044] For example, in different embodiments, the ratio of the sum of the mass percentages of Gd and Nd to the sum of the mass percentages of Cu and Mg (Gd+Nd) / (Cu+Mg) can be 0.35, 0.36, 0.38, 0.4, 0.42, 0.44, 0.45, or a range consisting of any two of them. Studies have found that when the amounts of Gd, Nd, Cu and Mg meet the above conditions, it is more helpful to improve the room temperature and high temperature strength and plasticity of the cast aluminum alloy.

[0045] In a specific embodiment of the present invention, the mass percentage ratio of Gd to Nd is 0.5-1.

[0046] For example, in different embodiments, the mass percentage ratio of Gd to Nd can be 0.5, 0.6, 0.7, 0.8, 0.9, 1, or any two thereof. By adjusting the usage ratio of Gd to Nd within the above range, it is more helpful to improve the structure of the cast aluminum alloy and improve the plasticity.

[0047] In a specific embodiment of the present invention, the mass percentage ratio of Mn to Fe is 0.8 to 1.1.

[0048] For example, in different embodiments, the ratio of the mass percentage of Mn to Fe can be 0.8, 0.85, 0.9, 0.95, 1, 1.05, 1.1, or any two thereof. Regulating the mass percentage of Mn to Fe within the above range is more conducive to eliminating the damage of Fe to the mechanical properties, while increasing the number of nuclei, reducing the eutectic size, and thus significantly improving the mechanical properties.

[0049] In a specific embodiment of the present invention, the ratio of the sum of the mass percentages of Si and Cu to the mass percentage of Ti is (Si+Cu) / Ti=4.5-8.

[0050] For example, in different embodiments, the ratio of the sum of the mass percentages of Si and Cu to the mass percentage of Ti (Si+Cu) / Ti can be 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, or a range consisting of any two of them. When the amounts of Si, Cu, and Ti further meet the above conditions, it is more helpful to exert the refinement effect of Ti, form an appropriate amount of intermetallic compound phase, and improve multiple properties of the alloy.

[0051] Another aspect of the present invention provides a method for preparing any one of the above-mentioned cast aluminum alloys, comprising the following steps:

[0052] (a) Proportioning according to the stoichiometric ratio of cast aluminum alloy;

[0053] (b) melting the prepared raw materials to obtain aluminum alloy liquid;

[0054] (c) Casting the aluminum alloy liquid to obtain a cast aluminum alloy casting.

[0055] In a specific embodiment of the present invention, the raw materials include industrial pure aluminum ingots, industrial pure magnesium ingots, Al-Si master alloys, Al-Cu master alloys, Al-Ni master alloys, Al-Fe master alloys, Al-Mn master alloys, Al-Gd master alloys, Al-Nd master alloys and Al-Ti master alloys.

[0056] Among them, the Al-Si master alloy can be an Al-35Si master alloy, the Al-Cu master alloy can be an Al-50Cu master alloy, the Al-Ni master alloy can be an Al-10Ni master alloy, the Al-Fe master alloy can be an Al-20Fe master alloy, the Al-Mn master alloy can be an Al-10Mn master alloy, the Al-Gd master alloy can be an Al-20Gd master alloy, the Al-Nd master alloy can be an Al-10Nd master alloy, and the Al-Ti master alloy can be an Al-10Ti master alloy, but is not limited to this.

[0057] In a specific embodiment of the present invention, smelting includes: after melting an industrial pure aluminum ingot, adding an Al-Si master alloy at 760-780°C, after all are melted, adding an Al-Cu master alloy, an Al-Ni master alloy, an Al-Fe master alloy, an Al-Mn master alloy, an Al-Gd master alloy, an Al-Nd master alloy and part of an Al-Ti master alloy at 780-800°C, after all are melted, adding an industrial pure magnesium ingot at 740-750°C, after all are melted, refining at 780-800°C, after refining is completed, adding the remaining Al-Ti master alloy at 750-760°C, and after all are melted, scooping the bottom and stirring to obtain an alloy liquid.

[0058] In a specific embodiment of the present invention, during smelting, the amount of the partial Al-Ti master alloy added before refining is 50% to 80% of the total amount of the Al-Ti master alloy.

[0059] For example, in different embodiments, during smelting, the amount of the Al-Ti master alloy added before refining can be 50%, 55%, 60%, 65%, 70%, 75%, 80% of the total amount of the Al-Ti master alloy. By adjusting the timing of adding the Al-Ti master alloy and the amount of addition at different stages, the aggregation and deposition problems during smelting and casting are significantly reduced, the degree of segregation is reduced, and the refinement effect of Ti is fully guaranteed.

[0060] In a specific embodiment of the present invention, the casting comprises: cooling the alloy liquid to 680-720° C. and pouring it into a mold.

[0061] In a specific embodiment of the present invention, it also includes: performing a solution treatment and an aging treatment on the cast aluminum alloy casting. Further, the solution treatment includes: keeping the temperature at 510-530°C for 4-5 hours and then cooling with water; the aging treatment includes: keeping the temperature at 170-180°C for 5-9 hours.

[0062] In a specific embodiment of the present invention, the microstructure of the cast aluminum alloy in the cast state includes primary α-Al dendrites, eutectic silicon phase, Al2Cu, Al3Ti, Q phase (ie Al5Cu2Mg8Si6) and rare earth compounds.

[0063] In a specific embodiment of the present invention, in the cast microstructure, the volume fractions of primary α-Al dendrites, eutectic silicon phase and Al3Ti are 73% to 86%, 7.5% to 11% and 3.5% to 7.5%, respectively, and the average sizes of primary α-Al dendrites, eutectic silicon phase and Al3Ti are 21 to 62 μm, 7 to 12.5 μm and 1 to 2.2 μm, respectively. Further, in the cast microstructure, the volume fractions of primary α-Al dendrites, eutectic silicon phase and Al3Ti are 75.2% to 78.5%, 7.8% to 10.5% and 4.1% to 7.1%, respectively, and the average sizes of primary α-Al dendrites, eutectic silicon phase and Al3Ti are 21.0 to 22.7 μm, 7 to 11.5 μm and 1 to 1.7 μm, respectively.

[0064] In a specific embodiment of the present invention, in the cast microstructure, the volume fractions of primary α-Al dendrites, eutectic silicon phase and Al3Ti are 75.2% to 76.8%, 8.6% to 10.5% and 5.3% to 7.1%, respectively, and the average sizes of primary α-Al dendrites, eutectic silicon phase and Al3Ti are 21.0 to 22.7 μm, 7 to 10.3 μm and 1 to 1.4 μm, respectively.

[0065] In a specific embodiment of the present invention, after solution treatment and aging treatment, in the microstructure of the aluminum alloy casting, the average size of α-Al grains is ≤40 μm, and the average size of eutectic silicon phase is ≤11.5 μm.

[0066] In a specific embodiment of the present invention, after solution treatment and aging treatment, the performance of the aluminum alloy casting meets the following requirements: tensile strength ≥300MPa, yield strength ≥134MPa, and elongation ≥2% at room temperature (20°C); tensile strength ≥102MPa, yield strength ≥69MPa, and elongation ≥3.4% at 300°C.

[0067] Among them, after solution treatment and aging treatment, the room temperature tensile strength of the aluminum alloy casting can be 300MPa, 302MPa, 305MPa, 308MPa, 310MPa, 312MPa, 315MPa or a range consisting of any two thereof; the room temperature yield strength can be 134MPa, 140MPa, 145MPa, 150MPa, 155MPa, 160MPa, 165MPa, 170MPa, 175MPa, 180MPa, 187MPa or a range consisting of any two thereof; the room temperature elongation can be 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 4.9% or a range consisting of any two thereof; the aluminum alloy The 300°C tensile strength of the casting can be 102MPa, 108MPa, 110MPa, 115MPa, 120MPa, 130MPa, 135MPa, 140MPa, 145MPa, 148MPa or a range consisting of any two of them; the 300°C yield strength can be 69MPa, 75MPa, 80MPa, 85MPa, 90MPa, 95MPa, 100MPa, 101MPa or a range consisting of any two of them; the 300°C elongation can be 3.4%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 8.7% or a range consisting of any two of them.

[0068] Another aspect of the present invention provides use of any one of the above-mentioned cast aluminum alloys in manufacturing engine parts.

[0069] Examples 1 to 14

[0070] Examples 1 to 14 provide cast aluminum alloys and preparation methods, respectively. The measured composition of each cast aluminum alloy is shown in Table 1. The preparation method of each cast aluminum alloy comprises the following steps:

[0071] (1) According to the element ratio principle of cast aluminum alloy, a certain amount of smelting raw materials that can obtain Si, Cu, Mg, Ni, Fe, Mn, Gd, Nd, Ti and Al elements are weighed, such as industrial pure aluminum ingots, industrial pure magnesium ingots, Al-Si master alloys, Al-Cu master alloys, Al-Ni master alloys, Al-Fe master alloys, Al-Mn master alloys, Al-Gd master alloys, Al-Nd master alloys and Al-Ti master alloys.

[0072] (2) Melting industrial pure aluminum ingots to obtain pure aluminum liquid. When the temperature of the pure aluminum liquid reaches 770°C, adding Al-Si master alloy, after all are melted, heating to 790°C, adding Al-Cu master alloy, Al-Ni master alloy, Al-Fe master alloy, Al-Mn master alloy, Al-Gd master alloy, Al-Nd master alloy and 7 / 10 amount of Al-Ti master alloy, after all are melted, standing for 20 minutes, then cooling to 745°C, adding industrial pure magnesium ingots, after all are melted, heating to 790°C for refining (high-purity argon gas is passed to the surface of the alloy liquid for refining during the refining process), then cooling to 755°C, adding the remaining amount of Al-Ti master alloy, after all are melted, scooping the bottom and stirring to obtain alloy liquid.

[0073] (3) After the alloy liquid is cooled to a pouring temperature of 700±10°C, pouring is performed to obtain a cast aluminum alloy.

[0074] (4) subjecting the cast aluminum alloy obtained in step (3) to solution treatment and aging treatment; wherein the solution treatment comprises: keeping at 520° C. for 5 h and then water cooling; and the aging treatment comprises: keeping at 175° C. for 8 h.

[0075] Table 1 Measured composition (wt%) of cast aluminum alloys of different embodiments

[0076]

[0077] Embodiment 15

[0078] Example 15 provides a cast aluminum alloy and a preparation method, with reference to Example 1, except that in the preparation method, the amounts of the Al-Ti intermediate alloy added twice in step (2) are different.

[0079] In this embodiment, the Al-Ti master alloy added for the first time accounts for 1 / 2 of the total amount.

[0080] Example 16

[0081] Example 16 provides a cast aluminum alloy and a preparation method, with reference to Example 1, except that in the preparation method, the amounts of the Al-Ti intermediate alloy added twice in step (2) are different.

[0082] In this embodiment, the Al-Ti master alloy added for the first time accounts for 9 / 10 of the total amount.

[0083] Embodiment 17

[0084] Example 17 provides a cast aluminum alloy and a preparation method, with reference to Example 1, the only difference being that, in the preparation method, step (2) is different.

[0085] In this embodiment, the Al-Ti master alloy is not added in steps, but is added all together with the other master alloys, and the other operations are the same.

[0086] Comparative Examples 1 to 6

[0087] The preparation methods of the cast aluminum alloys of Comparative Examples 1 to 6 refer to Examples 1 to 14, except that the components of the cast aluminum alloys are different. The measured components of the cast aluminum alloys of Comparative Examples 1 to 6 are shown in Table 2.

[0088] Table 2 Measured composition of cast aluminum alloys of different comparative examples (wt%)

[0089] serial number Si Cu Mg Ni Fe Mn G Nd Ti Al Comparative Example 1 11.2 3.02 1.23 3.00 0.73 0.46 0.72 1.00 2.17 margin Comparative Example 2 11.0 3.02 1.22 3.01 0.73 1.09 0.74 1.01 2.18 margin Comparative Example 3 11.0 3.04 1.19 3.02 0.72 0.71 0.74 1.01 — margin Comparative Example 4 11.1 3.03 1.19 3.01 0.72 0.70 0.73 1.01 0.25 margin Comparative Example 5 11.0 3.01 1.20 2.99 0.72 0.72 0.51 0.73 2.16 margin Comparative Example 6 11.1 3.02 1.20 3.00 0.74 0.71 2.12 1.32 2.15 margin

[0090] Experimental Example 1

[0091] In order to compare and illustrate the differences in the structures of the cast aluminum alloys of different embodiments and comparative examples, a high-resolution transmission electron microscope was used to observe the microstructures of the cast aluminum alloys and characterize the typical structures. The results are shown in Table 3. Figure 1 is the as-cast metallographic structure of the cast aluminum alloy of Example 1 of the present invention, Figure 2 The as-cast metallographic structure of the cast aluminum alloy of comparative example 1 of the present invention. After solution and aging treatment, the grain size of the cast aluminum alloy of the embodiment of the present invention does not change significantly, the average size of the α-Al grains can be ≤40μm, and the average size of the eutectic silicon phase can be ≤11.5μm. However, after solution and aging treatment, the grain size of the cast aluminum alloy of the comparative example becomes larger.

[0092] Table 3 As-cast microstructures of different embodiments and comparative examples

[0093]

[0094]

[0095] Experimental Example 2

[0096] The properties of the cast aluminum alloys of different embodiments and comparative examples were tested using "HB 5143" and "GB / T 228.2". The test results are shown in Table 4.

[0097] Table 4 Performance test results of casting alloys of different embodiments and comparative examples

[0098]

[0099]

[0100] It can be seen from the above test results that the cast aluminum alloy of the present invention has excellent room temperature and high temperature mechanical properties, and can meet the performance requirements under existing harsh service environments.

[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A cast aluminum alloy, characterized in that: Includes the following elements in mass percentage: Si 10%~12%, Cu 2.8%~3.2%, Mg 1%~1.4%, Ni 2.5%~3.2%, Fe0.65%~0.8%, Mn 0.6%~1%, Gd 0.2%~2%, Nd 0.8%~1.2%, Ti 1%~3%, and the balance is Al and unavoidable impurities.

2. The cast aluminum alloy according to claim 1, characterized in that The sum of the mass percentages of Gd and Nd is 1.2% to 2.5%; Preferably, the mass percentage ratio of Gd to Nd is 0.5-1.

3. The cast aluminum alloy according to claim 1, characterized in that: The ratio of the sum of the mass percentages of Gd and Nd to the sum of the mass percentages of Cu and Mg is (Gd+Nd) / (Cu+Mg)=0.35-0.

45.

4. The cast aluminum alloy according to claim 1, characterized in that: The mass percentage ratio of Mn to Fe is 0.8 to 1.

1.

5. The cast aluminum alloy according to claim 1, characterized in that: The ratio of the sum of the mass percentages of Si and Cu to the mass percentage of Ti is (Si+Cu) / Ti=4.5-8.

6. The method for preparing a cast aluminum alloy according to any one of claims 1 to 5, characterized in that: The steps include: (a) Proportioning according to the stoichiometric ratio of cast aluminum alloy; (b) melting the prepared raw materials to obtain aluminum alloy liquid; (c) casting the aluminum alloy liquid to obtain a cast aluminum alloy casting.

7. The method for preparing a cast aluminum alloy according to claim 6, characterized in that: The raw materials include industrial pure aluminum ingots, industrial pure magnesium ingots, Al-Si master alloys, Al-Cu master alloys, Al-Ni master alloys, Al-Fe master alloys, Al-Mn master alloys, Al-Gd master alloys, Al-Nd master alloys and Al-Ti master alloys; Preferably, the smelting comprises: after melting the industrial pure aluminum ingot, adding the Al-Si master alloy at 760-780° C., after all are melted, adding Al-Cu master alloy, Al-Ni master alloy, Al-Fe master alloy, Al-Mn master alloy, Al-Gd master alloy, Al-Nd master alloy and part of Al-Ti master alloy at 780-800° C., after all are melted, adding industrial pure magnesium ingot at 740-750° C., after all are melted, refining at 700-740° C., after refining, adding the remaining Al-Ti master alloy at 750-760° C., after all are melted, scooping and stirring to obtain alloy liquid; Preferably, in the smelting, the amount of the partial Al-Ti master alloy added before refining is 50% to 80% of the total amount of the Al-Ti master alloy; Preferably, the casting comprises: cooling the alloy liquid to 680-720° C. and pouring it into a mold.

8. The method for preparing a cast aluminum alloy according to claim 6, characterized in that: Also includes: performing a solution treatment and an aging treatment on the cast aluminum alloy casting; The solution treatment comprises: keeping the temperature at 510-530° C. for 4-5 hours and then cooling with water; the aging treatment comprises: keeping the temperature at 170-180° C. for 5-9 hours.

9. The method for preparing a cast aluminum alloy according to claim 6, characterized in that: In the as-cast microstructure of the casting, there are primary α-Al dendrites, eutectic silicon phase and Al3Ti phase; After the solution treatment and aging treatment, in the microstructure of the aluminum alloy casting, the average size of α-Al grains is ≤40 μm, and the average size of eutectic silicon phase is ≤11.5 μm; After the solution treatment and aging treatment, the properties of the aluminum alloy casting meet the following requirements: tensile strength ≥300MPa, yield strength ≥134MPa, and elongation ≥2% at room temperature; tensile strength ≥102MPa, yield strength ≥69MPa, and elongation ≥3.4% at 300°C.

10. Use of the cast aluminum alloy according to any one of claims 1 to 5 or the cast aluminum alloy prepared by the preparation method according to any one of claims 6 to 9 in manufacturing engine parts.

Citation Information

Cited By

  • High-toughness aluminum alloy as well as preparation method and application thereof

    CN121204477A

  • High-strength and high-toughness aluminum alloys, their preparation methods and applications

    CN121204477B

  • A high-strength multi-cavity thin-walled 6-series aluminum alloy profile for automotive chassis structural beams, its preparation method and application

    CN123063659A