- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The high surface corrugation caused by surface defects and texture caused by solute atomic gas mass pinning and coarse grains during the production process of existing aluminum alloy sheets affects the quality of the spray paint.
By reasonably proportioning the aluminum alloy components Si, Fe, Cu, Mn, Mg, Cr, Zn and other elements, 6xxx series aluminum alloy sheets are prepared, and the crystals are controlled by hot rolling, cold rolling, solid solution heat treatment, pre-aging and other process steps. Particle refinement and surface treatment to reduce surface corrugation.
It significantly reduces the surface corrugation, meets the technical standards of automotive panels, improves the microstructure of the panels, inhibits PLC and orange peel defects, and improves mechanical properties and surface quality.
Smart Images

Figure CN118932226A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy plate production, and in particular relates to an aluminum alloy plate with low surface corrugation and a preparation method thereof. Background Art
[0002] With the improvement of environmental protection, energy consumption and cost standards, car companies have cancelled the intermediate coating process in the painting process, which reduces the thickness of the paint film on the surface. As a result, the undulating structure of the substrate surface morphology is more likely to appear on the painted surface. Therefore, the requirements for the surface waviness of the plate are further increased.
[0003] The production of plates requires processes such as rolling and stretching to produce plastic deformation, as well as heat treatment and surface treatment. These processes will affect the final surface waviness of the plate.
[0004] Generally, factors that affect the surface waviness of the plate include: PLC defects caused by the pinning effect of solute atom gas clusters, surface orange peel defects caused by coarse grains, and ribbed grain defects caused by the "strip" aggregation distribution of the texture. The combination of multiple factors leads to a high final surface waviness value of the plate, affecting the surface quality after painting.
[0005] In summary, the prior art obviously has inconveniences and defects in practical use, so it is necessary to improve it. Summary of the invention
[0006] In view of the above defects, the present invention mainly provides an aluminum alloy plate with low surface waviness to solve the technical problem of high surface waviness caused by various surface defect factors in the production process of the aluminum alloy plate.
[0007] In order to solve the above problems, the present invention provides an aluminum alloy plate with low surface waviness, comprising: the alloy composition of the aluminum alloy plate is:
[0008] Si: 0.85~1.20%, Fe: 0.10~0.20%, Cu: 0.06~0.16%, Mn: 0.10~0.16%, Mg: 0.35~0.40%, Cr≤0.10%, Zn≤0.10%, other impurity elements≤0.15%, and the rest is Al.
[0009] According to the low surface waviness aluminum alloy sheet material of the present invention, the aluminum alloy sheet material is a 6xxx series aluminum alloy.
[0010] According to the low surface waviness aluminum alloy sheet of the present invention, other impurity elements are composed of a plurality of elements, wherein the content of any one of the impurity elements does not exceed 0.05%.
[0011] According to the low surface waviness aluminum alloy sheet of the present invention, the alloy composition of the aluminum alloy sheet further includes Ti≤0.10%.
[0012] A method for preparing the aluminum alloy plate comprises the following steps:
[0013] S1, hot rolling, including rough rolling and finishing rolling; specific:
[0014] Rough rolling: rolling the aluminum alloy ingot for 17 to 25 times to obtain an intermediate plate with a thickness of 45 to 60 mm; the temperature range of the intermediate plate is controlled to be: 370 to 400°C;
[0015] Finish rolling: rolling the intermediate plate into a plate with a thickness of 4.0-6.0 mm, and then rolling it into a hot-rolled coil; the coiling temperature is controlled to be: 340-360°C;
[0016] S2, cold rolled;
[0017] The hot rolled coil is rolled into a plate with a thickness of 0.85 to 1.2 mm; the total cold rolling processing rate should be controlled at 75 to 80%;
[0018] S3, solution heat treatment;
[0019] The plate is kept at 545-565℃ for 10-40s, and then water-cooled; the cooling rate is: 35-50℃ / s;
[0020] S4, pre-aging;
[0021] The plate is heated to 60-100°C and then air-cooled to room temperature to obtain a finished product.
[0022] According to the preparation method of the present invention, the aluminum alloy ingot is subjected to sawing and milling treatment before hot rolling; then the ingot is subjected to homogenization treatment: at 535-555° C., and kept warm for 8-12 hours.
[0023] According to the preparation method of the present invention, before the pre-aging step, the plate is subjected to surface treatment; specifically:
[0024] The plate is immersed in the tank for acid and alkali washing and passivation surface treatment; the etching amount is not less than 0.5g / m 2 ; Erode the raised parts of the plate to reduce the value of surface waviness.
[0025] According to the preparation method of the present invention, the free fluorine concentration in the bath solution is 300-800 ppm.
[0026] According to the preparation method of the present invention, the peak density (Rpc) of the cold rolling roller used in the cold rolling step is ≥90cm -1 , surface roughness Ra≤0.25μm.
[0027] According to the preparation method of the present invention, the aluminum alloy plate obtained by the preparation method is pre-stretched with a deformation amount of 5%; the test results are as follows:
[0028] Tensile strength: 190-310MPa, yield strength: 90-135MPa, elongation ≥24%, yield strength after baking: ≥200MPa. Surface waviness ≤0.35μm, surface flatness grade 1 or 2.
[0029] In summary, the low surface waviness aluminum alloy sheet of the present invention improves the microstructure of the sheet by rationally proportioning the components of each element, suppresses the surface PLC defect and the surface orange peel defect, and significantly reduces the value of the surface waviness, so that it can meet the requirements of the technical standards of automobile sheets. The present invention also provides a method for preparing an aluminum alloy sheet, which controls the temperature of the intermediate plate after rough rolling, reduces the temperature during the rough rolling process, suppresses the growth of grains, and further reduces the aggregation of grain clusters with similar orientations after rolling, and finally reduces or avoids the formation of ribbed grain defects on the surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a schematic diagram of the metallographic structure of an embodiment of the present invention;
[0031] Figure 2 Schematic diagram of the metallographic structure of the comparative example of the present invention
[0032] Figure 3 is a surface ribbed grain physiognomy diagram of an embodiment of the present invention;
[0033] Figure 4 is a surface ribbed grain morphology diagram of a comparative example of the present invention;
[0034] In the attached figure:
[0035] Figure 1 This is a typical picture selected after metallographic observation and picture collection of the samples of all embodiments, and the grain size in the picture is 32μm;
[0036] Figure 2 This is a typical picture selected after metallographic observation and picture collection of all comparative samples. The grain size in the picture is 41μm;
[0037] Figure 3 This is a typical picture selected after testing and rating the surface grooving appearance of the samples of all embodiments, and the surface grooving grade in the picture is level 2;
[0038] Figure 4 This is a typical picture selected after testing and rating the surface grooving appearance of all the samples in the comparative examples. The surface grooving grade in the picture is 4; DETAILED DESCRIPTION
[0039] See also Figure 1 The present invention provides an aluminum alloy plate with low surface waviness, comprising: the alloy composition of the aluminum alloy plate is:
[0040] Si: 0.85~1.20%, Fe: 0.10~0.20%, Cu: 0.06~0.16%, Mn: 0.10~0.16%, Mg: 0.35~0.40%, Cr≤0.10%, Zn≤0.10%, other impurity elements≤0.15%, and the rest is Al.
[0041] Preferably, the composition of the aluminum alloy sheet of the present invention is 6xxx series aluminum alloy.
[0042] Optionally, the other impurity elements of the present invention are composed of multiple elements, wherein the content of any one of the impurity elements does not exceed 0.05%.
[0043] Compared with the composition of existing aluminum alloys, the Si content of the present invention is increased, and the Mg content is correspondingly reduced; as the two elements play a strengthening role, the composition ratio of the present invention can meet the strength requirements of the aluminum alloy, while reducing the Mg element can weaken the pinning effect of the solute atomic gas group, thereby inhibiting the occurrence of PLC defects on the surface of the plate.
[0044] At the same time, the invention increases the content of Mn element and the number of dispersed phase particles containing Mn element in the alloy, thereby inhibiting the growth of grains and weakening or eliminating the surface orange peel defect caused by coarse grains.
[0045] As an embodiment, the alloy composition of the aluminum alloy plate of the present invention also includes Ti≤0.10%, which plays a role in refining the grains, further suppressing the orange peel defects on the surface, and optimizing the mechanical properties of the aluminum alloy plate.
[0046] The Cu content of the invention is 0.06-0.16%, which can improve the room temperature and baking hardening strength of the aluminum alloy plate; at the same time, the Cu content is limited to no more than 0.16% to avoid reducing the corrosion resistance of the aluminum alloy plate.
[0047] The aluminum alloy plate of the present invention improves the microstructure of the plate by reasonably matching the components of various elements, suppresses surface PLC defects and surface orange peel defects, and significantly reduces the value of surface waviness, so that it can meet the requirements of technical standards for automobile plates.
[0048] The present invention also provides a method for preparing the aluminum alloy sheet, comprising the following steps:
[0049] S1, hot rolling, including rough rolling and finishing rolling; specific:
[0050] Rough rolling: rolling the aluminum alloy ingot for 17 to 25 times to obtain an intermediate plate with a thickness of 45 to 60 mm; the temperature range of the intermediate plate is controlled to be: 370 to 400°C;
[0051] Finish rolling: rolling the intermediate plate into a plate with a thickness of 4.0-6.0 mm, and then rolling it into a hot-rolled coil; the coiling temperature is controlled to be: 340-360°C;
[0052] As an embodiment, the aluminum alloy ingot of the present invention is subjected to sawing and milling treatment before hot rolling; thereafter, the ingot is subjected to homogenization treatment: at 535-555° C., and kept warm for 8-12 hours.
[0053] S2, cold rolled;
[0054] The hot rolled coil is rolled into a plate with a thickness of 0.85 to 1.2 mm; the total cold rolling processing rate should be controlled at 75 to 80%;
[0055] Furthermore, in order to ensure the surface quality of the plate, the peak density (Rpc) of the cold rolling roller used in the cold rolling step of the present invention is ≥90cm -1 , surface roughness Ra≤0.25μm;
[0056] Generally, during rough rolling, the grains of aluminum alloy grow due to heat; during rolling, the coarse grains are elongated along the rolling direction. After the grains recrystallize, clusters of grains with similar orientations are formed. After the sheet is deformed by stamping, ribbed grain defects are easily formed on the surface.
[0057] The present invention controls the temperature of the intermediate plate after rough rolling to reduce the temperature during rough rolling, inhibit the growth of crystal grains, and further reduce the aggregation of crystal grain clusters with similar orientations after rolling, ultimately reducing or avoiding the formation of rib defects on the surface.
[0058] The present invention also controls the total processing rate of cold rolling to be not less than 75%, which is beneficial to the refinement of recrystallized grains and reduces the aforementioned grain clustering effect, thereby controlling the appearance of rib patterns.
[0059] S3, solution heat treatment;
[0060] The plate is kept at 545-565℃ for 10-40s, and then water-cooled; the cooling rate is: 35-50℃ / s;
[0061] S4, pre-aging;
[0062] The plate is heated to 60-100°C and then air-cooled to room temperature to obtain a finished product.
[0063] As an embodiment, before the pre-aging step of the present invention, the plate is subjected to surface treatment; specifically:
[0064] The plate is immersed in the tank for acid and alkali washing and passivation surface treatment; the etching amount is not less than 0.5g / m 2 ; Erosion of the raised parts of the plate to reduce the value of surface waviness;
[0065] Further, in the bath: the free fluorine concentration is 300 to 800 ppm;
[0066] The inventor used the preparation method of the present invention to prepare aluminum alloy plates, and collected multiple samples for pre-stretching with a deformation of 5% to simulate stamping deformation. After that, multiple tests were performed on the pre-stretched samples, and the test results are as follows:
[0067] Tensile strength: 190-310MPa, yield strength: 90-135MPa, elongation A≥24%, yield strength after baking: BHYS≥200MPa. Surface waviness (Wsa) ≤0.35μm, surface flatness level is 1 or 2. The test results meet the requirements of mechanical properties of aluminum alloy automobile outer panels.
[0068] In order to further illustrate the technical effect of the present invention, the inventor selected six aluminum alloy ingots with different compositions, and prepared aluminum alloy plates using the above-mentioned preparation method, and then pre-stretched the plates with a deformation amount of 5% to obtain several examples and comparative samples. Finally, the tensile strength, yield strength, elongation, yield strength after baking, surface waviness (Wsa), surface level and grain size of each sample were tested and recorded.
[0069] For each aluminum alloy ingot of each composition, one embodiment sample and one comparative example sample were prepared. The difference between the embodiment and the comparative example is that the process parameters of the embodiment are within the range defined by the aforementioned preparation method; and one process parameter of the comparative example exceeds the range defined by the aforementioned preparation method.
[0070] In addition, the inventors also selected an aluminum alloy ingot with a seventh component and made two comparative samples. By changing the surface treatment parameters, the inventors verified the effect of the surface treatment process on the final surface quality of the plate.
[0071] The composition of the aluminum alloy of each embodiment and comparative example is shown in Table 1. The process parameters and test results of each embodiment and comparative example are shown in Table 2. The test standards are:
[0072] Tensile strength: 190-310MPa, yield strength: 90-135MPa, elongation A≥24%, yield strength after baking: BHYS≥200MPa. Surface waviness (Wsa) ≤0.35μm, surface flatness level not exceeding level 2.
[0073] Note: In Table 2, the process parameters that are out of range and the test results that are out of standard used in the comparative examples are underlined for easy identification.
[0074] Table 1 Composition of aluminum alloy used in each embodiment and comparative example
[0075] Sample No. Si Fe Cu Mn Mg Cr Zn Ti Al Example 1, Comparative Example 1 0.86 0.15 0.08 0.12 0.38 0.03 0.01 0.02 margin Example 2, Comparative Example 2 1.19 0.18 0.12 0.13 0.37 0.04 0.01 0.02 margin Example 3, Comparative Example 3 0.98 0.16 0.09 0.13 0.40 0.02 0.01 0.02 margin Example 4, Comparative Example 4 0.96 0.15 0.10 0.15 0.35 0.02 0.01 0.02 margin Example 5, Comparative Example 5 1.03 0.15 0.13 0.10 0.39 0.03 0.01 0.02 margin Example 6, Comparative Example 6 1.01 0.17 0.08 0.16 0.38 0.03 0.01 0.02 margin Comparative Examples 7 and 8 1.05 0.18 0.09 0.14 0.37 0.02 0.01 0.02 margin
[0076] Table 2 Process parameters and test results of each embodiment and comparative example
[0077]
[0078]
[0079] See also Figure 3 From the test results, it can be seen that the mechanical properties, surface waviness and surface quality of the plate prepared by the preparation method of the present invention all meet the requirements. Figure 1 In terms of microstructure, the grains are refined and evenly distributed, with good strength and plasticity.
[0080] Combination Figure 2 and Figure 4 Although the process steps of each comparative example are the same as those of the embodiment, some process parameters exceed the limits, so one or more test results are unqualified. In addition, the grains of some comparative samples are coarse and obvious ribbed defects appear on the surface.
[0081] In summary, the present invention provides a low surface waviness aluminum alloy sheet, which improves the microstructure of the sheet by rationally proportioning the components of each element, suppresses surface PLC defects and surface orange peel defects, and significantly reduces the value of surface waviness, so that it can meet the requirements of the technical standards of automobile sheets. The present invention also provides a method for preparing an aluminum alloy sheet, which controls the temperature of the intermediate plate after rough rolling, reduces the temperature during the rough rolling process, suppresses the growth of grains, and further reduces the aggregation of grain clusters with similar orientations after rolling, and finally reduces or avoids the formation of ribbed grain defects on the surface.
[0082] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art may make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A low surface corrugation aluminum alloy sheet, characterized in that: include: The alloy composition of the aluminum alloy sheet is: Si: 0.85~1.20%, Fe: 0.10~0.20%, Cu: 0.06~0.16%, Mn: 0.10~0.16%, Mg: 0.35~0.40%, Cr≤0.10%, Zn≤0.10%, other impurity elements≤0.15%, and the rest is Al.
2. The low surface corrugation aluminum alloy sheet material according to claim 1, characterized in that: The aluminum alloy plate is a 6xxx series aluminum alloy.
3. The low surface corrugation aluminum alloy sheet material according to claim 1, characterized in that: Other impurity elements are composed of a plurality of elements, wherein the content of any one of the impurity elements does not exceed 0.05%.
4. The low surface corrugation aluminum alloy sheet material according to claim 1, characterized in that: The alloy composition of the aluminum alloy plate also includes Ti≤0.10%.
5. A method for preparing an aluminum alloy sheet according to any one of claims 1 to 4, characterized in that: The steps include: S1, hot rolling, including rough rolling and finishing rolling; specific: Rough rolling: rolling the aluminum alloy ingot for 17 to 25 times to obtain an intermediate plate with a thickness of 45 to 60 mm; the temperature range of the intermediate plate is controlled to be: 370 to 400°C; Finish rolling: rolling the intermediate plate into a plate with a thickness of 4.0-6.0 mm, and then rolling it into a hot-rolled coil; the coiling temperature is controlled to be: 340-360°C; S2, cold rolled; The hot rolled coil is rolled into a plate with a thickness of 0.85 to 1.2 mm; the total cold rolling processing rate should be controlled at 75 to 80%; S3, solution heat treatment; The plate is kept at 545-565℃ for 10-40s, and then water-cooled; the cooling rate is: 35-50℃ / s; S4, pre-aging; The plate is heated to 60-100°C and then air-cooled to room temperature to obtain a finished product.
6. The preparation method according to claim 5, characterized in that: The aluminum alloy ingot is subjected to sawing and milling treatment before hot rolling; then the ingot is subjected to homogenization treatment: the temperature is 535-555° C. and the temperature is kept for 8-12 hours.
7. The preparation method according to claim 5, characterized in that: Before the pre-aging step, the plate is subjected to surface treatment; specifically: The plate is immersed in the tank for acid and alkali washing and passivation surface treatment; the etching amount is not less than 0.5g / m 2 .
8. The preparation method according to claim 7, characterized in that: In the bath solution, the free fluorine concentration is 300-800 ppm.
9. The preparation method according to claim 5, characterized in that: The peak density (Rpc) of the cold rolling roller used in the cold rolling step is ≥90cm -1 , surface roughness Ra≤0.25μm.
10. The preparation method according to any one of claims 6 to 9, characterized in that: The aluminum alloy sheet obtained by the preparation method was pre-stretched with a deformation amount of 5%; the test results are as follows: Tensile strength: 190-310MPa, yield strength: 90-135MPa, elongation ≥24%, yield strength after baking: ≥200MPa. Surface waviness ≤0.35μm, surface flatness grade 1 or 2.
Citation Information
Patent Citations
Aluminum alloy sheet for press forming, process for manufacturing same, and press-formed product thereof
CN105102645A
Aluminum alloy sheet and production method thereof
CN105925858A
High-strength aluminum plate for truck fuel tank and production method therefor
CN113862498A
Preparation method of 6xxx series aluminum alloy plate strip with high surface quality
CN115305329A
6xxx aluminum alloy plate as well as preparation method and application thereof
CN115354179A