Q690D high-strength steel and preparation method thereof
By using molybdenum oxide briquetting and alloying process in the production process of Q690D high-strength steel, the process parameters are controlled, the flaw detection problem is solved, the pass rate and performance of the steel plate is improved, the alloy cost is reduced, and high-quality steel plate production is achieved .
Patent Information
- Application Number
- CN202411127975.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Q690D high-strength steel often has defect detection in the production process, mainly due to abnormal non-metallic inclusions, resulting in inconsistent steel plate performance, affecting delivery and subsequent product quality.
Molybdenum oxide blocks are used instead of iron molybdenum. Through top-bottom reblowing converter smelting, LF refining, RH refining, continuous casting and rolling, chemical composition and process parameters are controlled, the number and size of inclusions are reduced, and the cleanliness of steel plates are improved. and tissue density, including alloying of molybdenum oxide blocks, silicon manganese, high-carbon ferromanganese, medium-carbon ferrochromium, ferroniobium ferromanganese, deoxygenation of aluminum-manganese, controlling the alkalinity of LF final slag and CaO/Al2O3 ratio, and carrying out the RH calcium treatment and rolling temperature control.
The flaw detection pass rate of Q690D high-strength steel has been significantly improved to more than 99.9%, reducing alloy cost, and improving the yield strength, tensile strength and impact work of the steel plate, reducing the total amount of inclusions and large-sized inclusions, and improving the product. quality.
Smart Images

Figure CN118932254A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and specifically relates to a Q690D high-strength steel and a preparation method thereof. Background Art
[0002] Q690D steel is a low-alloy high-strength steel with a yield strength of 690MPa. It is widely used in many fields such as marine engineering, oil and gas pipelines, construction, bridges, energy, and engineering machinery. It is generally required to be delivered in the state of flaw detection or flaw detection + heat treatment, but flaw detection failures often occur, affecting the delivery of steel plates and subsequent product orders. The most typical flaw detection failure is the abnormal non-metallic inclusions in the steel plate. The inclusions have different properties from the steel and behave inconsistently during the processing and stress process, which will cause stress concentration around the inclusions, easily generate microcracks, and cause flaw detection failures.
[0003] Chinese patent application CN117187695 A discloses a Q690D high-strength steel plate and its preparation method. The chemical composition of the Q690D high-strength steel plate includes, by weight percentage: C: 0.06-0.2%, Si: 0.1-0.6%, Mn: 0.8-2.0%, P≤0.03%, S≤0.02%, Nb: 0.01-0.05%, V: 0.08-0.12%, N: 0.01-0.02%, Ni: 0.2-0.3%, Cr: 0.3-0.5%, and the balance is iron and unavoidable impurities. The production process of the present invention is converter smelting, LF refining, continuous casting, heating, rolling, cooling, the steelmaking process does not undergo vacuum degassing and refining, the continuous casting billet is heated by hot charging, and no heat treatment is required after rolling, thereby reducing energy consumption and production costs. However, this patent application is aimed at the short-process and reduced-volume production of Q690D high-strength steel to reduce energy consumption, and it still has the problem of non-compliance with NDT. Summary of the invention
[0004] To solve the above problems, the present invention provides a Q690D high-strength steel and a preparation method thereof, which reduces the number and size of inclusions, improves product quality, and increases the steel plate flaw detection pass rate to more than 99.9%.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The invention provides a Q690D high-strength steel. The chemical composition of the Q690D high-strength steel comprises, by weight percentage, C: 0.14-0.2%, Si: 0.2-0.4%, Mn: 1.1-1.6%, P≤0.015%, S≤0.005%, Cr: 0.1-0.4%, Nb: 0.01-0.04%, Ti: 0.01-0.03%, Mo: 0.1-0.4%, Als: 0.01-0.045%, B: 0.001-0.003%, CEV≤0.62, and the balance is iron and unavoidable impurities.
[0007] The present invention further provides a method for preparing Q690D high-strength steel, comprising the following steps:
[0008] 1) Converter smelting:
[0009] The smelting process is carried out in a top and bottom combined blowing converter, the ladle is a red clean ladle with good bottom blowing, and the baking temperature is ≥800℃.
[0010] The molybdenum oxide briquette is placed in the front of the scrap steel bucket and added together with the scrap steel. The amount of molybdenum oxide briquette added is 4.38-8.77kg / t steel.
[0011] The molybdenum oxide briquette is made by mixing molybdenum oxide powder with 10% reduction promoter, 7% volatility suppressing binder and 3% water. The reduction promoter and volatility suppressing binder used in the present invention are common raw materials in the field and can be purchased.
[0012] Molybdenum oxide briquette: Mo: 48%-55%, Si≤0.1%, P≤0.05%.
[0013] The C content at the end point of smelting is controlled at 0.05-0.09%, the tapping temperature is controlled at 1630-1650°C, and the final slag basicity is controlled within the range of 3.0-4.0.
[0014] Silicon manganese, high carbon ferromanganese, medium carbon ferrochrome and ferroniobium are used for alloying. The added amounts are 14.15-16.18kg / t steel of silicon manganese, 2.65-4.65kg / t steel of high carbon ferromanganese, 2.6-3.5kg / t steel of medium carbon ferrochrome and 0.23-0.31kg / t steel of ferroniobium. The addition is completed when one-fifth to three-quarters of the steel is released, and the alloy is added to the impact zone of the steel flow.
[0015] Silicon manganese: Mn: 60%-70%, Si: 16.5%-20%, C≤1.8%, P≤0.25%, S≤0.04%;
[0016] High carbon ferromanganese: Mn: 65%-72%, Si≤2.5%, C≤7%, P≤0.25%, S≤0.03%;
[0017] Medium carbon ferrochrome: Cr ≥ 52%, C ≤ 2.0%, Si ≤ 3.0%, P ≤ 0.06%, S ≤ 0.05%;
[0018] Ferroniobium: Nb: 50%-60%, Si≤2.5%, Al≤2.0%, C≤0.05%, P≤0.05%, S≤0.03%;
[0019] Aluminum-manganese-iron is used for deoxidation, and the amount of aluminum-manganese-iron added is 2.0-2.5kg / t steel. Additional aluminum-manganese-iron is added depending on the overoxidation of the molten steel.
[0020] When placing steel, slide plates are used to block slag, and top lime is added along with the steel flow.
[0021] The use of molybdenum oxide to provide molybdenum element to steel is to use a reducing agent to react chemically with molybdenum oxide during the steelmaking process to achieve molybdenum alloying. In the early and middle stages of converter blowing, the molten pool temperature is low, the volatility of molybdenum oxide is low, and the molten pool contains relatively high levels of [C], [Si], [Mn] and other elements, which can undergo reduction reactions with molybdenum oxide. Therefore, the molybdenum oxide briquette is placed in the front of the scrap steel hopper and added together with the scrap steel, and the molybdenum recovery rate can reach 96.7-97%.
[0022] 2) LF refining:
[0023] The LF inlet temperature is 1540-1560℃.
[0024] LF refining adopts bottom blowing argon stirring throughout the whole process. The argon flow rate in the early strong stirring and shell breaking stage is 500-750L / min, and the argon blowing stirring time is 2-3min; the argon flow rate in the power-on slag adding and white slag making stage is 100-200L / min; the argon flow rate in the white slag refining and fine-tuning composition stage is 100-180L / min; low-pressure soft blowing is adopted before leaving the station, the argon flow rate is 50-70L / min, and the soft blowing time is 5-7min.
[0025] According to the viscosity, color and foaming degree of the slag, lime and calcium carbide are added in batches to adjust the slag. The added amounts are 200-500kg / furnace of lime and 40-60kg / furnace of calcium carbide respectively. The top slag should reach yellow-white slag before leaving the station, the final slag basicity is controlled at 5-6, the refined slag CaO / Al2O3 is controlled at 1.8-2.0, and the slag thickness is 110-120mm to improve the adsorption capacity of the refined slag for inclusions in the steel.
[0026] Aluminum wire is used to increase aluminum, titanium wire is used to increase titanium, and ferroboron is used to increase boron. The added amounts are 0.76-2.3m / t steel for aluminum wire, 0.53-0.84m / t steel for titanium wire, and 0.08-0.12kg / t steel for ferroboron.
[0027] The TS content in the steel is 75-80ppm when LF leaves the station.
[0028] 3)RH refining:
[0029] RH adopts this treatment operation mode. During treatment, the immersion tube is inserted to a depth of 400 mm, the vacuum degree is 120-133 Pa and maintained for 15-20 min, the pure degassing time is 10-15 min, and fine-tuning is performed according to the target composition.
[0030] After the RH treatment, feed nano high calcium wire 70-80m / furnace, soft blowing time is 10-12min, slag thickness is 100-120mm, and T.Ca content in steel is controlled at 8-10ppm.
[0031] 4) Continuous casting
[0032] During the continuous casting process, full-process protective pouring is adopted, the argon sealing flow rate of the large ladle is 90-100L / min, and the liquid surface of the tundish is covered with carbonized rice husks, and the added amount is 1-1.5kg / t steel.
[0033] The crystallizer adopts non-sinusoidal vibration, the liquidus temperature is 1510-1520℃, the superheat of the tundish is controlled at 20-30℃, and the pulling speed is 1.1-1.4m / min.
[0034] The continuous casting billet is slowly cooled down after leaving the production line and pile cooled to below 400℃.
[0035] The slab thickness is 200-250mm, and the TO content in the continuous casting slab is 6-7ppm.
[0036] 5) Rolling
[0037] Continuous casting billet heating: the tapping temperature is 1180-1210℃, the heating rate is 8-10min / cm, and the time in the furnace is 210-230min.
[0038] The total number of rolling passes is 12-16, the total number of rough rolling passes is 5-7, the total number of finishing rolling passes is 7-9, and the rolling thickness is 24.7-25.05mm.
[0039] Rough rolling: The starting temperature of rough rolling is 1140-1170℃, and the final rolling temperature of rough rolling is 1050-1120℃.
[0040] Finishing rolling: The starting rolling temperature of finishing rolling is 890-950℃, and the final rolling temperature of finishing rolling is 810-860℃.
[0041] Cooling: Cooling inlet temperature 770-820℃, cooling outlet temperature 670-700℃, cooling rate controlled at 5-10℃ / s.
[0042] 6) Heat treatment
[0043] The quenching heating temperature is 900-920℃, the holding time is 7-13min, the tempering heating temperature is 510-530℃, and the holding time is 15-25min.
[0044] The steel plate obtained by the invention has a yield strength of 720-790 MPa, a tensile strength of 770-940 MPa, an elongation after fracture of 14.5-19.5%, an impact energy of 114-252 J at -20°C, and both D and Ds inclusions in the rolled material are less than 1.0 grade.
[0045] Compared with the prior art, the advantages of the present invention are:
[0046] 1. The present invention adopts molybdenum oxide briquettes instead of ferromolybdenum, 0.01% Mo can save 1-1.5 yuan, the molybdenum content of Q690D high-strength steel is 0.2-0.4%, and the alloy cost can be reduced by 20-60 yuan / ton of steel; it is calculated that the most economical and applicable manganese alloy type of Q690D is silicon manganese + high carbon ferromanganese, the cost of high carbon ferromanganese per 0.01% Mn in the manganese alloy is 0.99 yuan, the cost of medium carbon ferromanganese per 0.01% Mn is 1.13 yuan, and the cost of metallic manganese per 0.01% Mn is 1.25 yuan. The use of high carbon ferromanganese can save 0.14-0.26 yuan, the manganese content of Q690D high-strength steel is 1.1-1.6%, and the alloy cost can be reduced by 15-30 yuan / ton of steel. In summary, the alloy cost can be significantly reduced.
[0047] 2. The present invention controls the LF final slag basicity and the CaO / Al2O3 ratio and formulates a reasonable argon blowing system to improve the adsorption efficiency of LF for inclusions, and at the same time controls the RH calcium treatment timing and the amount of calcium wire added, taking into account both castability and inclusion removal efficiency, so that the TS content in the steel is controlled at 75-80ppm, the T.Ca content is controlled at 8-10ppm, and the TO content is controlled at 6-7ppm, thereby improving the cleanliness of the molten steel, reducing the central element segregation of the ingot, reducing the total amount of inclusions and large-sized inclusions, and the D and Ds inclusions in the rolled product are both less than grade 1.0.
[0048] 3. The present invention reduces internal segregation of the ingot by controlling the heating temperature and rolling method of the continuous casting ingot, fully breaks up the grains in the core of the ingot, loosens the welding center, refines the grains inside the steel plate, improves the density of the internal structure, and increases the qualified rate of steel plate flaw detection to more than 99.9%. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is an OTS inclusion analysis diagram of the steel plate produced in Example 1.
[0050] Figure 2 This is the OTS inclusion analysis diagram of the steel plate produced in Example 2.
[0051] Figure 3This is the OTS inclusion analysis diagram of the steel plate produced in Example 1. DETAILED DESCRIPTION
[0052] The technical solution of the present invention is described in detail below with reference to the accompanying drawings and embodiments.
[0053] Example 1
[0054] The chemical composition weight percentage is:
[0055] Brand C Si Mn P S Cr Nb Ti Mo Als B CEV Q690D 0.154 0.25 1.25 0.014 0.004 0.18 0.017 0.018 0.107 0.043 0.0014 0.42
[0056] Main process measures of preparation method:
[0057] 1) Converter smelting:
[0058] The smelting process is carried out in a top and bottom combined blowing converter, the ladle is a red clean ladle with good bottom blowing, and the baking temperature is ≥800℃.
[0059] Molybdenum oxide briquettes are placed in the front of the scrap steel bucket and added together with the scrap steel. The amount of molybdenum oxide briquettes added is 5.0 kg / t steel.
[0060] The C content at the end of smelting is controlled at 0.06%, the tapping temperature is controlled at 1634°C, and the final slag basicity is controlled within the range of 3.2.
[0061] Silicon manganese, high carbon ferromanganese, medium carbon ferrochrome and ferroniobium are used for alloying. The added amounts are 14.3kg / t steel, 2.95kg / t steel, 3.0kg / t steel and 0.25kg / t steel respectively. The addition is completed when one-fifth to three-quarters of the steel is released. The alloy is added to the impact zone of the steel flow.
[0062] Aluminum-manganese-iron is used for deoxidation, and the amount of aluminum-manganese-iron added is 2.3kg / t steel.
[0063] When placing steel, slide plates are used to block slag, and top lime is added along with the steel flow.
[0064] 2) LF refining:
[0065] The LF station entry temperature is 1545℃.
[0066] LF refining adopts bottom blowing argon stirring throughout the whole process. The argon flow rate in the early strong stirring and shell breaking stage is 550L / min, and the argon blowing stirring time is 3min; the argon flow rate in the power-on slag adding and white slag making stage is 150L / min; the argon flow rate in the white slag refining and fine-tuning composition stage is 150L / min; before leaving the station, low-pressure soft blowing is adopted, the argon flow rate is 60L / min, and the soft blowing time is 6min.
[0067] According to the viscosity, color and foaming degree of the slag, lime and calcium carbide are added in batches to adjust the slag. The added amounts are 300kg / furnace and 45kg / furnace respectively. The top slag should reach yellow-white slag before leaving the station, the final slag basicity is controlled at 5.5, the refined slag CaO / Al2O3 is controlled at 1.9, and the slag thickness is 110mm to improve the adsorption capacity of the refined slag for inclusions in the steel.
[0068] Aluminum wire is used to increase aluminum, titanium wire is used to increase titanium, and ferroboron is used to increase boron. The added amounts are 1.5m / t steel, 0.6m / t steel, and 0.1kg / t steel respectively.
[0069] 3)RH refining:
[0070] RH adopts this treatment operation mode. During treatment, the immersion tube is inserted to a depth of 400 mm, the vacuum degree is 130 Pa and maintained for 15 minutes, and the pure degassing time is 12 minutes.
[0071] After the RH treatment, 70m / furnace of nano high calcium wire was fed, the soft blowing time was 11min, the slag thickness was 110mm, and the T.Ca content in the steel was controlled at 8-10ppm.
[0072] 4) Continuous casting
[0073] During the continuous casting process, full-process protective pouring is adopted, the argon sealing flow rate of the large ladle is 90L / min, and the liquid surface of the tundish is covered with carbonized rice husks, and the added amount is 1.2kg / t steel.
[0074] The crystallizer adopts non-sinusoidal vibration, the liquidus temperature is 1510℃, the superheat of the tundish is controlled at 20℃, and the pulling speed is 1.2m / min.
[0075] The slab thickness is 200mm. The continuous casting slab is slowly cooled down and pile cooled to below 400℃.
[0076] 5) Rolling
[0077] Heating of continuous casting billet: tapping temperature is 1202℃, heating rate is 9min / cm, and time in the furnace is 230min.
[0078] The total number of rolling passes is 12, the total number of rough rolling passes is 5, the total number of finishing rolling passes is 7, and the rolling thickness is 24.7mm.
[0079] Rough rolling: The starting temperature of rough rolling is 1163℃, and the final rolling temperature of rough rolling is 1115℃.
[0080] Finishing rolling: The starting rolling temperature of finishing rolling is 899℃, and the final rolling temperature of finishing rolling is 856℃.
[0081] Cooling: cooling inlet temperature 808°C, cooling outlet temperature 700°C, cooling rate controlled at 7°C / s.
[0082] 6) Heat treatment
[0083] The quenching heating temperature is 900℃, the holding time is 10min, the tempering heating temperature is 520℃, and the holding time is 20min.
[0084] When the LF of the present invention leaves the station, the TS content in the steel is 75ppm, the T.Ca content in the steel is controlled at 8ppm, the TO content in the continuous casting billet is 7ppm, the maximum size of the casting billet inclusions is 15μm, and the D and Ds inclusions in the rolled product are both less than grade 1.0.
[0085] The steel plate obtained by the invention has a yield strength of 726-790MPa, a tensile strength of 770-940MPa, an elongation after fracture of 14.5-19.5%, an impact energy of 114-252J at -20°C, and a steel plate flaw detection qualified rate of 100%.
[0086] Example 2
[0087] The chemical composition weight percentage is:
[0088] Brand C Si Mn P S Cr Nb Ti Mo Als B CEV Q690D 0.161 0.25 1.24 0.012 0.003 0.18 0.017 0.017 0.135 0.035 0.0017 0.43
[0089] 1) Converter smelting:
[0090] The smelting process is carried out in a top and bottom combined blowing converter, the ladle is a red clean ladle with good bottom blowing, and the baking temperature is ≥800℃.
[0091] The molybdenum oxide briquettes are placed in the front of the scrap steel bucket and added together with the scrap steel. The amount of molybdenum oxide briquettes added is 7.5kg / t steel.
[0092] The C content at the end of smelting is controlled at 0.06%, the tapping temperature is controlled at 1630°C, and the final slag basicity is controlled within the range of 3.0.
[0093] Silicon manganese, high carbon ferromanganese, medium carbon ferrochrome and ferroniobium are used for alloying. The added amounts are 14.5kg / t steel, 4.0kg / t steel, 3.2kg / t steel and 0.25kg / t steel respectively. The addition is completed when one-fifth to three-quarters of the steel is released. The alloy is added to the impact zone of the steel flow.
[0094] Aluminum-manganese-iron is used for deoxidation, and the amount of aluminum-manganese-iron added is 2.5kg / t steel.
[0095] When placing steel, slide plates are used to block slag, and top lime is added along with the steel flow.
[0096] 2) LF refining:
[0097] The LF inlet temperature is 1550℃.
[0098] LF refining adopts bottom blowing argon stirring throughout the whole process. The argon flow rate in the early strong stirring and shell breaking stage is 600L / min, and the argon blowing stirring time is 3min; the argon flow rate in the power-on slag adding and white slag making stage is 160L / min; the argon flow rate in the white slag refining and fine-tuning composition stage is 150L / min; low-pressure soft blowing is adopted before leaving the station, with an argon flow rate of 70L / min and a soft blowing time of 7min.
[0099] According to the viscosity, color and foaming degree of the slag, lime and calcium carbide are added in batches to adjust the slag. The added amounts are 400kg / furnace and 60kg / furnace respectively. The top slag should reach yellow-white slag before leaving the station, the final slag basicity is controlled at 6, the refined slag CaO / Al2O3 is controlled at 2.0, and the slag thickness is 110mm to improve the adsorption capacity of the refined slag for inclusions in the steel.
[0100] Aluminum wire is used to increase aluminum, titanium wire is used to increase titanium, and ferroboron is used to increase boron. The added amounts are 1.5m / t steel, 0.8m / t steel, and 0.11kg / t steel respectively.
[0101] 3)RH refining:
[0102] RH adopts this treatment operation mode. During treatment, the immersion tube is inserted to a depth of 400 mm, the vacuum degree is 130 Pa and maintained for 18 minutes, and the pure degassing time is 13 minutes.
[0103] After RH treatment, feed nano high calcium wire 80m / furnace, soft blowing time is 10min, slag thickness is 100mm,
[0104] 4) Continuous casting
[0105] During the continuous casting process, full-process protective pouring is adopted, the argon sealing flow rate of the large ladle is 100L / min, and the liquid surface of the tundish is covered with carbonized rice husks, and the added amount is 1.2kg / t steel.
[0106] The crystallizer adopts non-sinusoidal vibration, the liquidus temperature is 1520℃, the superheat of the tundish is controlled at 25℃, and the pulling speed is 1.15m / min.
[0107] The slab thickness is 250mm, and the continuous casting slab is slowly cooled down and pile cooled to below 400℃.
[0108] 5) Rolling
[0109] Continuous casting billet heating: the tapping temperature is 1193°C, the heating rate is 9 min / cm, and the time in the furnace is 210 min.
[0110] The total number of rolling passes is 14, the total number of rough rolling passes is 7, the total number of finishing rolling passes is 7, and the rolling thickness is 25.05mm.
[0111] Rough rolling: The starting temperature of rough rolling is 1147℃, and the final rolling temperature of rough rolling is 1098℃.
[0112] Finishing rolling: The starting rolling temperature of finishing rolling is 943℃, and the final rolling temperature of finishing rolling is 824℃.
[0113] Cooling: cooling inlet temperature 793°C, cooling outlet temperature 672°C, cooling rate controlled at 8°C / s.
[0114] 6) Heat treatment
[0115] The quenching heating temperature is 910℃, the holding time is 10min, the tempering heating temperature is 530℃, and the holding time is 20min.
[0116] When the LF of the present invention leaves the station, the TS content in the steel is 80ppm, the T.Ca content in the steel is controlled at 9ppm, the TO content in the continuous casting billet is 6ppm, the maximum size of the casting billet inclusions is 18μm, and the D and Ds inclusions in the rolled product are both less than grade 1.0.
[0117] The steel plate obtained by the invention has a yield strength of 720-785MPa, a tensile strength of 760-920MPa, an elongation after fracture of 15-17.5%, an impact energy of 125-243J at -20°C, and a steel plate flaw detection qualified rate of 99.9%.
[0118] Comparative Example 1
[0119] The chemical composition weight percentage is:
[0120] Brand C Si Mn P S Cr Nb Ti Mo Als B CEV Q690D 0.154 0.28 1.22 0.013 0.002 0.2 0.018 0.018 0.16 0.036 0.0016 0.43
[0121] 1) Converter smelting:
[0122] The smelting process is carried out in a top and bottom combined blowing converter, the ladle is a red clean ladle with good bottom blowing, and the baking temperature is ≥800℃.
[0123] Silicon manganese, low carbon ferromanganese, medium carbon ferrochrome, ferroniobium and ferromolybdenum are used for alloying.
[0124] Aluminum-manganese-iron is used for deoxidation, and the amount of aluminum-manganese-iron added is 2.5kg / t steel.
[0125] When placing steel, slide plates are used to block slag, and top lime is added along with the steel flow.
[0126] 2) LF refining:
[0127] According to the viscosity, color and foaming degree of the slag, lime and calcium carbide are added in batches to adjust the slag. The top slag should reach yellow-white slag before leaving the station, the final slag basicity is controlled at 4.91, the refined slag CaO / Al2O3 is controlled at 3.5, and the slag thickness is 110mm.
[0128] Aluminum wire is used to increase aluminum, titanium wire is used to increase titanium, and boron iron is used to increase boron.
[0129] 3)RH refining:
[0130] RH adopts this treatment operation mode. After the RH treatment, 100m of nano high calcium wire is fed / furnace, the soft blowing time is 10min, and the slag thickness is 100mm.
[0131] 4) Continuous casting
[0132] During the continuous casting process, full-process protective pouring is adopted, the argon sealing flow rate of the large ladle is 100L / min, and the liquid surface of the tundish is covered with carbonized rice husks, and the added amount is 1.5kg / t steel.
[0133] The crystallizer adopts non-sinusoidal vibration, the liquidus temperature is 1520℃, the superheat of the tundish is controlled at 25℃, and the pulling speed is 1.15m / min.
[0134] The continuous casting billet is slowly cooled down after leaving the production line and pile cooled to below 400℃.
[0135] 5) Rolling
[0136] Continuous casting billet heating: the tapping temperature is 1195°C, the heating rate is 9 min / cm, and the time in the furnace is 214 min.
[0137] Rough rolling: The starting rolling temperature of rough rolling is 1160℃, and the final rolling temperature of rough rolling is 1111℃.
[0138] Finishing rolling: The starting temperature of finishing rolling is 896℃, and the final rolling temperature of finishing rolling is 832℃.
[0139] Cooling: cooling inlet temperature 802°C, cooling outlet temperature 695°C, cooling rate controlled at 8°C / s.
[0140] 6) Heat treatment
[0141] The quenching heating temperature is 910℃, the holding time is 10min, the tempering heating temperature is 530℃, and the holding time is 20min.
[0142] When the comparative example LF leaves the station, the TS content in the steel is 115ppm, the T.Ca content in the steel is controlled at 12ppm, the TO content in the continuous casting billet is 12ppm, the maximum size of the casting billet inclusions is 35μm, the D-type inclusions in the rolled product are level 1.0, and the Ds-type inclusions are level 2.5.
[0143] The yield strength of the steel plate obtained in the comparative example is 710-780MPa, the tensile strength is 750-930MPa, the elongation after fracture is 14-17.5%, the impact energy at -20°C is 90-185J, and the qualified rate of steel plate flaw detection is 96%.
[0144] In Examples 1 and 2, molybdenum oxide briquettes are used instead of ferromolybdenum for alloying. The price of ferromolybdenum is 216,372 yuan / ton, and the price of molybdenum oxide briquettes is 164,035 yuan / ton. Every 0.01% Mo can save 1-1.5 yuan, and the alloy cost is reduced by 20-60 yuan / ton of steel compared with the comparative example of ferromolybdenum alloying. In Examples 1 and 2, silicon manganese + high carbon ferromanganese is used, and the alloy cost is reduced by 15-30 yuan / ton of steel compared with the comparative example of silicon manganese + low carbon ferromanganese.
[0145] Example 1 OTS inclusion analysis diagram of steel plate produced as shown in Figure 1 As shown; Example 2 OTS inclusion analysis diagram of the steel plate produced Figure 2 As shown; OTS inclusion analysis diagram of steel plate produced in Comparative Example 1 is as follows Figure 3 As shown. Figure 1-3 It can be seen that when the LF of Examples 1 and 2 leaves the station, the TS content in the steel is 75-80ppm, the T.Ca content in the steel is controlled at 8-9ppm, the TO content in the continuous casting billet is 6-7ppm, the maximum size of the inclusions in the casting billet is 15-18μm, and the D and Ds inclusions in the rolled material are both less than 1.0 grade. When the LF of the comparative example leaves the station, the TS content in the steel is 115ppm, the T.Ca content in the steel is controlled at 12ppm, the TO content in the continuous casting billet is 12ppm, the maximum size of the inclusions in the casting billet is 35μm, the D inclusions in the rolled material are 1.0 grade, and the Ds inclusions are 2.5 grade. The cleanliness in the steel of Examples 1 and 2 is significantly better than that of the comparative example, and the flaw detection pass rate of Examples 1 and 2 is higher than that of the comparative example.
[0146] The process parameters (such as temperature, time, etc.) of the present invention can realize the method by taking upper and lower limits and interval values, and the embodiments are not listed one by one here.
[0147] Any contents not described in detail in the present invention can be based on the conventional technical knowledge in the art.
[0148] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the embodiments, it should be understood by those skilled in the art that any modification or equivalent replacement of the technical solutions of the present invention does not depart from the spirit and scope of the technical solutions of the present invention and should be included in the scope of the claims of the present invention.
Claims
1. A Q690D high-strength steel plate, characterized in that: The chemical composition of the Q690D high-strength steel plate includes, by weight percentage, C: 0.14-0.2%, Si: 0.2-0.4%, Mn: 1.1-1.6%, P≤0.015%, S≤0.005%, Cr: 0.1-0.4%, Nb: 0.01-0.04%, Ti: 0.01-0.03%, Mo: 0.1-0.4%, Als: 0.01-0.045%, B: 0.001-0.003%, CEV≤0.62, and the balance is iron and unavoidable impurities.
2. A method for preparing the Q690D high-strength steel plate according to claim 1, comprising the following steps: 1) Converter smelting: The C content at the end of smelting is controlled at 0.05-0.09%, the tapping temperature is controlled at 1630-1650℃, and the final slag basicity is controlled within the range of 3.0-4.0; Molybdenum oxide briquettes are placed in front of the scrap steel bucket and added together with the scrap steel; 2) LF refining: The final slag basicity is controlled at 5-6, the refined slag CaO / Al2O3 is controlled at 1.8-2.0, and the slag thickness is 110-120mm; 3)RH refining: After RH treatment, feed nano high calcium wire 70-80m / furnace, soft blowing time is 10-12min, slag thickness is 100-120mm, and T.Ca content in steel is controlled at 8-10ppm; 4) Continuous casting: The crystallizer adopts non-sinusoidal vibration, the liquidus temperature is 1510-1520℃, the superheat of the tundish is controlled at 20-30℃, and the pulling speed is 1.1-1.4m / min; 5) Rolling: Continuous casting billet heating: tapping temperature is 1180-1210℃, heating rate is 8-10min / cm, and furnace time is 210-230min; Rough rolling: the starting rolling temperature of rough rolling is 1140-1170℃, and the final rolling temperature of rough rolling is 1050-1120℃; Finishing rolling: the starting temperature of finishing rolling is 890-950℃, and the final rolling temperature of finishing rolling is 810-860℃; Cooling: cooling inlet temperature 770-820℃, cooling outlet temperature 670-700℃, cooling speed controlled at 5-10℃ / s; 6) Heat treatment: The quenching heating temperature is 900-920℃, the holding time is 7-13min, the tempering heating temperature is 510-530℃, and the holding time is 15-25min.
3. The preparation method according to claim 2, characterized in that: In step 1), silicon manganese, high carbon ferromanganese, medium carbon ferrochrome and ferroniobium are used for alloying, and the added amounts are 14.15-16.18 kg / t steel, 2.65-4.65 kg / t steel, 2.6-3.5 kg / t steel and 0.23-0.31 kg / t steel respectively. The addition is completed when one-fifth to three-quarters of the steel is released, and the alloy is added to the impact zone of the steel flow.
4. The preparation method according to claim 2, characterized in that: The chemical composition weight ratio of the molybdenum oxide compact is: Mo: 48%-55%, Si≤0.1%, P≤0.05%.
5. The preparation method according to claim 2, characterized in that: In step 2), LF refining adopts bottom blowing argon stirring throughout the whole process. The argon flow rate in the early strong stirring and shell breaking stage is 500-750L / min, and the argon blowing stirring time is 2-3min; the argon flow rate in the power-on slag adding and white slag making stage is 100-200L / min; the argon flow rate in the white slag refining and fine-tuning composition stage is 100-180L / min; before leaving the station, low-pressure soft blowing is adopted, the argon flow rate is 50-70L / min, and the soft blowing time is 5-7min.
6. The preparation method according to claim 2, characterized in that: In step 3), RH adopts the present treatment operation mode, during which the immersion tube is inserted to a depth of 400 mm, the vacuum degree is 120-133 Pa and maintained for 15-20 min, and the pure degassing time is 10-15 min.
7. The preparation method according to claim 2, characterized in that: In step 4), during the continuous casting process, full-process protective pouring is adopted, the argon sealing flow rate of the large ladle is 90-100L / min, and the liquid surface of the tundish is covered with carbonized rice husks, and the added amount is 1-1.5kg / t steel.
8. The preparation method according to claim 2, characterized in that: In step 4), the continuous casting billet is slowly cooled off the production line and pile-cooled to below 400°C.
9. The preparation method according to claim 2, characterized in that: In step 5), the total rolling passes are 12-16 passes, the total rolling passes of rough rolling are 5-7 passes, the total rolling passes of finish rolling are 7-9 passes, and the rolling thickness is 24.7-25.05 mm.
10. The preparation method according to claim 2, characterized in that: The yield strength of the obtained steel plate is 720-790MPa, the tensile strength is 770-940MPa, the elongation after fracture is 14.5-19.5%, the impact energy at -20°C is 114-252J, and the D and Ds inclusions in the rolled material are both less than 1.0 grade.
Citation Information
Patent Citations
Manufacturing technology of steel containing molybdenum
CN103074543A
Thick specification Q690D high-strength high-toughness steel plate and production method thereof
CN104018085A
Low-compression-ratio super-thick Q690D tempered high-strength steel plate and production method thereof
CN111088467A
690MPa easy-to-weld corrosion-resisting high-strength steel and manufacturing method thereof
CN111455256A
Economical 690MPa-grade high-strength steel plate and preparation method thereof
CN113235009A