Composite microalloyed steel as well as preparation method and application thereof

By adding elements such as Ni, Mn, Cr, Mo, Cu to the alloy steel to form a dense rust layer, the problem of insufficient corrosion resistance of existing alloy steel in high sulfur and high chlorine environments is solved, and efficient corrosion resistance is achieved Performance and excellent mechanical properties, suitable for petrochemical equipment.

CN118932258APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310529822.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing alloy steels are insufficient corrosion resistance in petrochemical environments with high sulfur, high chlorine and high humidity, resulting in serious corrosion problems and cannot meet the corrosion resistance requirements of petroleum refining equipment.

Method used

Compound microalloy steel containing alloy elements such as Ni, Mn, Cr, Mo, Cu, etc. is used to form a dense rust layer through specific chemical composition and process treatment, which inhibits corrosive anions diffusion and improves chlorine- and hydrogen sulfide corrosion resistance.

Benefits of technology

In a wet hydrogen sulfide environment, it significantly reduces the corrosion rate, improves yield strength and tensile strength, and meets the corrosion resistance needs of petrochemical equipment. At the same time, the cost is not high, and it can replace ordinary carbon steel and carbon manganese steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of metal material smelting, and discloses composite microalloyed steel and a preparation method and application thereof. Based on the total weight of the composite microalloyed steel, the composite microalloyed steel comprises the following chemical components in percentage by weight: 2 to 3.1 percent of Ni, 0.8 to 1.8 percent of Mn, 0.5 to 1.5 percent of Cr, 0.1 to 0.8 percent of Mo, 0.05 to 0.6 percent of Cu, 0.03 to 0.12 percent of C, less than or equal to 0.018 percent of P, less than or equal to 0.03 percent of S and the balance of Fe and inevitable impurities. The composite microalloyed steel can form a compact rust layer in a chlorine-containing and hydrogen sulfide-containing environment, corrosive anions are inhibited from diffusing into a metal base material, the chlorine and hydrogen sulfide corrosion resistance of steel is improved, and the service requirement in a wet hydrogen sulfide environment is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal material smelting, and in particular to a composite microalloy steel and a preparation method and application thereof. Background Art

[0002] Ordinary carbon steels such as Q245R, Q345R, 20 steel and carbon-manganese steels such as 16Mn are widely used in petrochemical pipelines, pressure vessels, storage tanks and other oil refining equipment, and have the characteristics of low cost. However, since oil refining equipment often faces highly corrosive environments with high sulfur, high chlorine and high humidity, the above-mentioned ordinary carbon and carbon-manganese steels are far from meeting the corrosion resistance requirements of petrochemical equipment. According to research statistics, the domestic refining industry has more than 1,000 leaks caused by corrosion each year, causing more than 50 unplanned shutdowns, and causing economic losses of hundreds of billions of yuan. In response to serious corrosion problems, the petrochemical industry has begun to use alloy steels with high alloying elements such as Cr, Ni, and Mo to replace ordinary carbon steel and carbon-manganese steel, but the existing design still cannot meet the requirements of corrosion resistance. Therefore, it is urgent to provide a low-alloy steel with good corrosion resistance to replace traditional ordinary carbon steel and carbon-manganese steel. Summary of the invention

[0003] The purpose of the present invention is to overcome the problem of low corrosion resistance of existing alloy steels and to provide a composite micro-alloyed steel and a preparation method and application thereof. The composite micro-alloyed steel can form a relatively dense rust layer in a chlorine-containing and hydrogen sulfide-containing environment, inhibit the diffusion of corrosive anions into the metal substrate, improve the steel's resistance to chlorine and hydrogen sulfide corrosion, and meet the service requirements in a wet hydrogen sulfide environment.

[0004] In order to achieve the above-mentioned object, the present invention provides a composite microalloyed steel on the one hand. The weight percentage of the chemical components contained in the composite microalloyed steel is as follows: Ni: 2-3.1%, Mn: 0.8-1.8%, Cr: 0.5-1.5%, Mo: 0.1-0.8%, Cu: 0.05-0.6%, C: 0.03-0.12%, P: ≤0.018%, S: ≤0.03%, and the balance is Fe and unavoidable impurities.

[0005] Preferably, the weight percentage of the chemical components contained in the composite microalloyed steel is: Ni: 2.5-2.8%, Mn: 1.0-1.5%, Cr: 0.8-1.2%, Mo: 0.3-0.5%, Cu: 0.2-0.3%, C: 0.05-0.1%, P: ≤0.015%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

[0006] Preferably, the corrosion rate of the composite microalloyed steel in the atmospheric and vacuum, coking unit tower top circulation process environment is lower than 0.3 mm / a, wherein the process environment is saturated with chloride ions, 100% humidity, and the hydrogen sulfide content is not lower than 100 ppm.

[0007] Preferably, the yield strength of the composite microalloyed steel is ≥345 MPa, the tensile strength is 470-660 MPa, and the elongation after fracture is ≥23%.

[0008] The second aspect of the present invention provides a method for preparing the composite microalloyed steel according to the first aspect, the method comprising the following steps:

[0009] S1, adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni materials to the converter blowing molten steel for refining, and continuously casting the obtained refined molten steel to obtain a continuously cast billet;

[0010] S2, rolling the continuous casting billet to obtain composite microalloyed steel;

[0011] Wherein, in step S1, the weight percentages of chemical components contained in the refined molten steel are: Ni: 2-3.1%, Mn: 0.8-1.8%, Cr: 0.5-1.5%, Mo: 0.1-0.8%, Cu: 0.05-0.6%, C: 0.03-0.12%, P: ≤0.018%, S: ≤0.03%, and the remainder is Fe and unavoidable impurities.

[0012] Preferably, in step S1, the amount of the Cr alloy block is 1-3% by weight of the molten steel blown in the converter, and the content of Cr in the Cr alloy block is 10-60% by weight.

[0013] Preferably, in step S1, the amount of the Mn alloy block is 1-3% by weight of the molten steel blown in the converter, and the Mn content in the Mn alloy block is 20-80% by weight.

[0014] Preferably, in step S1, the amount of the Mo alloy block is 0.2-3% by weight of the molten steel blown in the converter, and the content of Mo in the Mo alloy block is 10-60% by weight.

[0015] Preferably, in step S1, the amount of pure Cu material used is 0-1% by weight of the molten steel blown in the converter.

[0016] Preferably, in step S1, the amount of pure Ni material used is 1-4 weight % of the molten steel blown in the converter.

[0017] Preferably, the S1 includes:

[0018] (1) desulfurizing and deslagging molten steel to obtain desulfurized molten steel, wherein the temperature of the molten steel during the desulfurization process is ≥1300° C., and the sulfur content in the desulfurized molten steel is ≤0.007 wt %;

[0019] (2) adding the desulfurized molten steel to a converter for steelmaking, and re-blowing oxygen at the top and bottom of the converter. When the C content in the desulfurized molten steel is ≤0.05 wt % and the P content is ≤0.01 wt %, the blowing is completed to obtain the converter blown molten steel;

[0020] (3) The slag is blocked when the converter is tapped, and Cr alloy blocks, Mn alloy blocks, Mo alloy blocks, pure Cu materials and pure Ni materials are added to the molten steel blown in the converter, and then the molten steel is put into a ladle, argon is blown into the ladle for stirring, and then LF refining is performed, alloys are added, slag is added, the temperature is increased, and the composition is continuously adjusted so that the molten steel meets the target requirements to obtain refined molten steel.

[0021] Preferably, in step (2), the conditions for converter steelmaking include: the converter steelmaking time is 0.1 to 2 hours, and the temperature of the molten steel out of the furnace is 1600 to 1700°C.

[0022] Preferably, in step (2), during the double oxygen blowing process at the top and bottom of the converter, the flow rate of oxygen is 210 to 280 m / s. 3 / ton / h.

[0023] Preferably, in step (3), a deoxidizer is added during the steel tapping process.

[0024] Preferably, the deoxidizer is selected from one or more of Al particles, SiFe particles and MnFe particles.

[0025] Preferably, in step (3), during the argon blowing and stirring process, the flow rate of argon is 0.15 to 0.43 m / s. 3 / ton / h.

[0026] Preferably, in step (3), the conditions for LF refining include: the initial temperature of LF refining of molten steel is 1550-1600° C., and the time of LF refining is 0.6-3 h.

[0027] Preferably, in step S2, the rolling process comprises: cutting the continuous casting billet into a fixed length, feeding it into a heating furnace and heating it to 1220-1250°C, dephosphorizing it with high-pressure water when it leaves the heating furnace, and then rolling and coiling it.

[0028] Preferably, the rolling process includes rough rolling and finish rolling.

[0029] Preferably, the final rolling temperature of the rolling is 840-910°C.

[0030] Preferably, the coiling temperature is 600-720°C.

[0031] Preferably, the rolling process further comprises: cold rolling and annealing the steel obtained after coiling.

[0032] Preferably, the annealing treatment conditions include: an annealing temperature of 750-850° C. and an annealing speed of 80-100 m / min.

[0033] The third aspect of the present invention provides a composite microalloyed steel prepared by the method described in the second aspect.

[0034] A fourth aspect of the present invention provides a use of the composite microalloyed steel described in the first aspect or the composite microalloyed steel described in the third aspect in the manufacture of petroleum refining equipment.

[0035] The present invention adopts specific multiple alloy elements Ni, Mn, Cr, Mo, and Cu for composite microalloying, and the obtained composite microalloyed steel can form a relatively dense rust layer in a chlorine-containing and hydrogen sulfide-containing environment. The rust layer can improve the cation selectivity and inhibit the passage of corrosive anions, so that the steel has super strong corrosion resistance in chlorine and hydrogen sulfide environments, and the corrosion rate in a wet hydrogen sulfide environment is less than 0.25 mm / a.

[0036] At the same time, the yield strength and elongation of the composite microalloyed steel are not lower than those of ordinary 16Mn steel, and the cost is no more than 1.5 times that of 16Mn steel, and it can widely replace ordinary carbon steel and carbon manganese steel in the application of petrochemical wet hydrogen sulfide environment. Specifically, the composite microalloyed steel of the present invention is a corrosion-resistant steel with a yield strength level of 345MPa or more and chlorine and hydrogen sulfide corrosion resistance. The yield strength of the steel is ≥345MPa, the tensile strength is 520-660MPa, and the elongation after fracture is ≥23%. DETAILED DESCRIPTION

[0037] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0038] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0039] The first aspect of the present invention provides a composite microalloyed steel, which contains the following chemical components in weight percentages based on the total weight of the composite microalloyed steel: Ni: 2-3.1%, Mn: 0.8-1.8%, Cr: 0.5-1.5%, Mo: 0.1-0.8%, Cu: 0.05-0.6%, C: 0.03-0.12%, P: ≤0.018%, S: ≤0.03%, and the remainder is Fe and unavoidable impurities.

[0040] After research, the inventors found that composite microalloyed steel containing Ni, Mn, Cr, Mo, Cu and specific contents can form a relatively dense rust layer in a wet hydrogen sulfide environment. The rust layer can improve the selective permeability of cations and inhibit the passage of corrosive anions, thus having super strong corrosion resistance to chlorine and hydrogen sulfide environments.

[0041] According to the present invention, in order to further improve the corrosion resistance of the composite microalloyed steel, under preferred conditions, the weight percentages of the chemical components contained in the composite microalloyed steel are: Ni: 2.5-2.8%, Mn: 1.0-1.5%, Cr: 0.8-1.2%, Mo: 0.3-0.5%, Cu: 0.2-0.3%, C: 0.05-0.1%, P: ≤0.015%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

[0042] In the present invention, the action mechanism of each element in the composite microalloyed steel is as follows:

[0043] Carbon (C): Carbon is the most effective and economical strengthening element in steel. It mainly improves the strength of steel through solid solution strengthening and precipitation strengthening, but C will reduce the plasticity and toughness of steel. High C content easily causes C to combine with Cr and precipitate at the grain boundary, resulting in Cr-poor grain boundary, which reduces the steel's resistance to intergranular corrosion and intergranular cracking.

[0044] Nickel (Ni): Nickel can improve the density of the metal rust layer in a high-chlorine and high-hydrogen sulfide environment, the cation selectivity and the rust layer's resistance to the penetration of chloride ions and sulfur-containing anions.

[0045] Manganese (Mn): As a desulfurization and deoxidation element, manganese can reduce the hot brittleness and cold brittleness caused by sulfur. Mn has a solid solution strengthening effect, which can improve the tensile strength of the material, reduce the austenite phase transformation starting temperature Ar3, and moderately improve the hardenability; it can improve the density of the metal rust layer in a high chlorine and high hydrogen sulfide environment.

[0046] Chromium (Cr): Chromium can form a dense oxide film on the surface of the steel plate to improve the passivation ability of the steel plate. It is easy to form enrichment in the rust layer to resist ion penetration and improve the steel's resistance to chlorine corrosion.

[0047] Molybdenum (Mo): Molybdenum can improve the density of the metal rust layer in a high-chlorine and high-hydrogen sulfide environment and the rust layer's resistance to the penetration of chloride ions and sulfur-containing anions.

[0048] Copper (Cu): Copper can improve the density of the metal rust layer in a high-chlorine and high-hydrogen sulfide environment and the rust layer's resistance to the penetration of chloride ions and sulfur-containing anions.

[0049] Phosphorus (P): Phosphorus is easy to segregate, which will reduce the cold brittle toughness and weldability of steel. Generally, P needs to be controlled below 0.10wt%.

[0050] Sulfur (S): Sulfur easily forms MnS inclusions with Mn elements, which deteriorates the mechanical properties of steel. At the same time, large-sized inclusions are prone to form a potential difference with the matrix, which preferentially forms pitting corrosion and deteriorates the corrosion resistance of steel. Generally, the S content should be controlled below 0.1wt%.

[0051] According to the present invention, the composite microalloyed steel can be applied to various highly corrosive process environments with high chlorine content and high humidity in petrochemical industry.

[0052] In a preferred embodiment, the composite micro-alloyed steel is used in a normal pressure reduction, coking unit tower top circulation process environment, wherein the process environment is saturated with chloride ions, 100% humidity, and a hydrogen sulfide content of not less than 100 ppm; further, in this process environment, the corrosion rate of the composite micro-alloyed steel is less than 0.3 mm / a.

[0053] In the present invention, the composite microalloyed steel not only has strong corrosion resistance but also has excellent mechanical properties, and can meet the service requirements in a wet hydrogen sulfide environment.

[0054] In a preferred embodiment, the yield strength of the composite microalloyed steel is ≥345 MPa, the tensile strength is 470-660 MPa, and the elongation after fracture is ≥23%.

[0055] The second aspect of the present invention provides a method for preparing the composite microalloyed steel according to the first aspect, the method comprising the following steps:

[0056] S1, adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni materials to the converter blowing molten steel for refining, and continuously casting the obtained refined molten steel to obtain a continuously cast billet;

[0057] S2, rolling the continuous casting billet to obtain composite microalloyed steel;

[0058] Wherein, in step S1, the weight percentages of chemical components contained in the refined molten steel are: Ni: 2-3.1%, Mn: 0.8-1.8%, Cr: 0.5-1.5%, Mo: 0.1-0.8%, Cu: 0.05-0.6%, C: 0.03-0.12%, P: ≤0.018%, S: ≤0.03%, and the remainder is Fe and unavoidable impurities.

[0059] The method of the present invention can obtain composite microalloy steel with good corrosion resistance and mechanical properties by adding Cr material, Mn material, Mo material and Ni material in a specific step, that is, adding them into molten steel after converter blowing for refining.

[0060] In the present invention, in order to obtain a composite microalloyed steel whose chemical composition and the content of each element meet the target requirements, it is necessary to reasonably control the amount of Cr material, Mn material, Mo material and Ni material added to the converter blowing molten steel.

[0061] The amount of Cr material used in the present invention is determined according to the Cr content in the Cr alloy block; in a preferred embodiment, in step S1, the amount of the Cr alloy block is 1-3% by weight of the molten steel blown in the converter, and the Cr content in the Cr alloy block is 10-60% by weight.

[0062] The amount of Mn material used in the present invention is determined according to the Mn content in the Mn alloy block; in a preferred embodiment, in step S1, the amount of the Mn alloy block is 1-3% by weight of the molten steel blown by the converter, and the Mn content in the Mn alloy block is 20-80% by weight.

[0063] The amount of Mo material used in the present invention is determined according to the Mo content in the Mo alloy block; in a preferred embodiment, in step S1, the amount of the Mo alloy block is 0.2-3% by weight of the molten steel blown in the converter, and the Mo content in the Mo alloy block is 10-60% by weight.

[0064] In a preferred embodiment, in step S1, the amount of pure Cu material used is 0-1% by weight of the molten steel blown in the converter.

[0065] In a preferred embodiment, in step S1, the amount of pure Ni material used is 1-4% by weight of the molten steel blown in the converter.

[0066] According to the present invention, in order to further improve the corrosion resistance of the prepared composite microalloyed steel and reduce the corrosion rate, under preferred conditions, S1 comprises:

[0067] (1) desulfurizing and deslagging molten steel to obtain desulfurized molten steel, wherein the temperature of the molten steel during the desulfurization process is ≥1300° C., and the sulfur content in the desulfurized molten steel is ≤0.007 wt %;

[0068] (2) adding the desulfurized molten steel to a converter for steelmaking, and re-blowing oxygen at the top and bottom of the converter. When the C content in the desulfurized molten steel is ≤0.05 wt % and the P content is ≤0.01 wt %, the blowing is completed to obtain the converter blown molten steel;

[0069] (3) The slag is blocked when the converter is tapped, and Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni materials are added to the molten steel blown in the converter, and then the molten steel is put into a ladle, argon is blown into the ladle for stirring, and then LF refining is performed, alloys are added, slag is added, the temperature is increased, and the composition is continuously adjusted so that the molten steel meets the target requirements to obtain refined molten steel.

[0070] In the present invention, there is no particular limitation on the composition and source of the molten steel, and conventional molten steel can be used. In a specific embodiment, the molten steel in step (1) can be obtained by smelting pure iron or ferroalloy in an electric furnace.

[0071] In step (1), the desulfurization process needs to keep the molten steel at a relatively high temperature, that is, the temperature of the molten steel during the desulfurization process is ≥1300°C; desulfurization can be achieved by spraying lime powder into the molten steel.

[0072] In the present invention, the converter steelmaking can be carried out in a conventional manner in the art. In order to improve the corrosion resistance of the prepared composite microalloyed steel in a wet hydrogen sulfide environment, in a preferred embodiment, in step (2), the converter steelmaking conditions include: the converter steelmaking time is 0.1 to 2 hours, the C and P contents reach the target requirements and the molten steel is discharged from the furnace at a temperature of 1600 to 1700°C, for example, 1600°C, 1650°C or 1700°C.

[0073] According to the present invention, in step (2), the purpose of oxygen blowing at the top and bottom of the converter is to desulfurize and decarbonize; in order to remove as much sulfur and carbon as possible from the molten steel, it is necessary to reasonably control the amount of oxygen introduced. Under preferred conditions, in step (2), during the oxygen blowing at the top and bottom of the converter, the flow rate of oxygen is 210-280 m / s. 3 / ton / h.

[0074] In a specific embodiment, in step (3), a deoxidizer may be added during the steel tapping process. In a preferred embodiment, the deoxidizer is selected from one or more of Al particles, SiFe particles, and MnFe particles.

[0075] According to the present invention, the purpose of argon blowing and stirring the ladle in step (3) is to promote the floating of inclusions, reduce the inclusion content in the molten steel, and thus improve the performance of the composite microalloyed steel. In a preferred embodiment, in step (3), during the argon blowing and stirring process, the flow rate of argon is 0.15-0.43 m / s. 3 / t / h.

[0076] In the present invention, the LF refining process can be carried out according to conventional operations in the art. In order to further improve the mechanical properties of the composite microalloyed steel and its corrosion resistance in a wet hydrogen sulfide environment, under preferred conditions, in step (3), the conditions of the LF refining include: the initial temperature of the molten steel LF refining is 1550-1600°C, that is, the temperature of the molten steel entering the LF furnace is 1550-1600°C; the LF refining time is 0.6-3h. LF refining continuously adjusts the composition, slag, and temperature to achieve the target requirements, and stands for 20 minutes after the argon blowing is completed.

[0077] In the present invention, the rolling process can be performed according to conventional operations in the art. In a preferred embodiment, in step S2, the rolling process includes: cutting the continuous casting billet into a fixed length, feeding it into a heating furnace and heating it to 1220-1250°C, dephosphorizing it with high-pressure water when it leaves the heating furnace, and then rolling and coiling it.

[0078] In a more specific embodiment, the rolling process includes rough rolling and finish rolling. The rolling process can be performed on a rolling mill commonly used in the art.

[0079] According to the present invention, in a preferred embodiment, the initial rolling temperature of the rolling process may be 1200-1250°C.

[0080] According to the present invention, in a preferred embodiment, the final rolling temperature of the rolling may be 840-910°C.

[0081] In the present invention, the coiling operation is not particularly limited as long as it can be operated normally. In a specific embodiment, the coiling temperature of the coiling can be 600-720°C.

[0082] In order to further improve the mechanical properties of the composite microalloyed steel, specifically, the rolling process further includes: cold rolling and annealing the steel obtained after coiling.

[0083] In a preferred embodiment, the annealing conditions include: an annealing temperature of 750-850° C., and an annealing speed of 80-100 m / min. In a more preferred embodiment, the annealing time is 0.1-5 h, preferably 1-5 h.

[0084] The method provided by the invention comprises the processes of molten steel pretreatment, converter blowing, refining, continuous casting and rolling, etc. The method is suitable for low-cost large-scale production and is easy to promote.

[0085] The third aspect of the present invention provides a composite microalloyed steel prepared by the method described in the second aspect.

[0086] In a preferred embodiment, based on the total weight of the composite microalloyed steel, the weight percentages of the chemical components it contains are: Ni: 2-3.1%, Mn: 0.8-1.8%, Cr: 0.5-1.5%, Mo: 0.1-0.8%, Cu: 0.05-0.6%, C: 0.03-0.12%, P: ≤0.018%, S: ≤0.03%, and the balance is Fe and unavoidable impurities.

[0087] In a preferred embodiment, the corrosion rate of the composite microalloyed steel in the atmospheric and vacuum, coking unit top circulation process environment is lower than 0.3 mm / a, wherein the process environment is saturated with chloride ions, 100% humidity, and the hydrogen sulfide content is not lower than 100 ppm.

[0088] In a preferred embodiment, the yield strength of the composite microalloyed steel is ≥345 MPa, the tensile strength is 470-660 MPa, and the elongation after fracture is ≥21%.

[0089] A fourth aspect of the present invention provides a use of the composite microalloyed steel described in the first aspect or the composite microalloyed steel described in the third aspect in the manufacture of petroleum refining equipment.

[0090] In the present invention, specifically, the oil refining equipment can be oil refining equipment such as pipelines, pressure vessels, storage tanks, etc. for petrochemical industry.

[0091] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.

[0092] In the following examples, the Cr content in the Cr alloy block is 10 wt %; the Mn content in the Mn alloy block is 65.0 wt %; and the Mo content in the Mo alloy block is 12 wt %.

[0093] The following examples are used to illustrate the composite microalloyed steel and its preparation process according to the present invention.

[0094] Example 1

[0095] 1) spraying lime powder (spraying amount is 8.2kg / ton) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.007 weight%;

[0096] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 220m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 1h and the temperature of the molten steel out of the furnace is 1650°C;

[0097] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.81 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.85% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.056% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.52% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.52% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.15m 3 / tons / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, increase temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time of LF refining is 1h;

[0098] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0099] 5) Cut the continuous casting billet into slabs with a thickness of 250 mm, send it into a heating furnace and heat it to 1220° C., use high-pressure water to dephosphorize it when it comes out of the heating furnace, and then send it into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1200° C., the final rolling temperature is 850° C., and the coiling temperature is 600° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 750° C., the annealing speed is 90 m / min, and the annealing time is 2 h, to obtain a composite micro-alloyed steel with a thickness of 22 mm.

[0100] The composite microalloyed steel prepared in Example 1 contains the following chemical components in weight percentage: Ni: 2.52%, Mn: 1.34%, Cr: 1.12%, Mo: 0.45%, Cu: 0.23%, C: 0.065%, P: 0.013%, S: 0.007%, and the balance is Fe and unavoidable impurities.

[0101] Example 2

[0102] 1) spraying lime powder (spraying amount is 7.5 / ton) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.007 weight%;

[0103] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 225m 3 / ton / h), remove P and C, when the C content in the desulfurized molten steel is ≤ 0.05% by weight and the P content is ≤ 0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 1 hour and the temperature of the molten steel out of the furnace is 1600°C;

[0104] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.78 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.78% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.195% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.78% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.78% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.32 m 3 / tons / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, increase temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1600℃, and the time of LF refining is 1.5h;

[0105] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0106] 5) Cut the continuous casting billet into slabs with a thickness of 280 mm, send it into a heating furnace and heat it to 1250° C., use high-pressure water to dephosphorize it when it comes out of the heating furnace, and then send it into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1220° C., the final rolling temperature is 860° C., and the coiling temperature is 650° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 830° C., the annealing speed is 90 m / min, and the annealing time is 1.5 h, to obtain a composite micro-alloyed steel with a thickness of 12 mm.

[0107] The composite microalloyed steel prepared in Example 2 contains the following chemical components in percentage by weight: Ni: 2.78%, Mn: 1.02%, Cr: 1.08%, Mo: 0.68%, Cu: 0.22%, C: 0.093%, P: 0.012%, S: 0.009%, and the remainder is Fe and unavoidable impurities.

[0108] Example 3

[0109] 1) spraying lime powder (spraying amount is 8.0 kg / ton) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.006 weight%;

[0110] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 228m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 1.5h and the temperature of the molten steel out of the furnace is 1650°C;

[0111] 3) slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.82 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.9% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.246% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.64% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.64% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.25m 3 / tons / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, increase temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time of LF refining is 1h;

[0112] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0113] 5) Cut the continuous casting billet into slabs with a thickness of 160 mm, send it into a heating furnace and heat it to 1220° C., use high-pressure water to dephosphorize it when it comes out of the heating furnace, and then send it into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1200° C., the final rolling temperature is 870° C., and the coiling temperature is 710° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 750° C., the annealing speed is 90 m / min, and the annealing time is 2 h, to obtain a composite micro-alloyed steel with a thickness of 22 mm.

[0114] The composite microalloyed steel prepared in Example 3 contains the following chemical components in percentage by weight: Ni: 2.64%, Mn: 1.29%, Cr: 1.16%, Mo: 0.42%, Cu: 0.23%, C: 0.075%, P: 0.015%, S: 0.009%, and the remainder is Fe and unavoidable impurities.

[0115] Example 4

[0116] 1) spraying lime powder (spraying amount is 10kg / t) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.007 weight%;

[0117] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 214m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 1.5h and the temperature of the molten steel out of the furnace is 1620°C;

[0118] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.68 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.91% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.246% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.50% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.79% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.22m 3 / tons / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, increase temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time of LF refining is 2h;

[0119] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0120] 5) Cut the continuous casting billet into slabs with a thickness of 250 mm, send them into a heating furnace and heat them to 1240° C., use high-pressure water to dephosphorize them when they come out of the heating furnace, and then send them into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1200° C., the final rolling temperature is 875° C., and the coiling temperature is 710° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 750° C., the annealing speed is 90 m / min, and the annealing time is 1.5 h, to obtain a composite microalloyed steel with a thickness of 10 mm.

[0121] The composite microalloyed steel prepared in Example 4 contains the following chemical components in percentage by weight: Ni: 2.50%, Mn: 1.29%, Cr: 1.16%, Mo: 0.42%, Cu: 0.23%, C: 0.075%, P: 0.015%, S: 0.009%, and the remainder is Fe and unavoidable impurities.

[0122] Example 5

[0123] 1) spraying lime powder (spraying amount is 8.2kg / t) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.006% by weight;

[0124] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 224m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 0.6h and the temperature of the molten steel out of the furnace is 1652°C;

[0125] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.82 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.91% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.246% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.50% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.79% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.42 m 3 / t / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, raise temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time of LF refining is 2h;

[0126] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0127] 5) Cut the continuous casting billet into slabs with a thickness of 160 mm, send them into a heating furnace and heat them to 1235° C., use high-pressure water to dephosphorize them when they come out of the heating furnace, and then send them into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1225° C., the final rolling temperature is 860° C., and the coiling temperature is 620° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 780° C., the annealing speed is 90 m / min, and the annealing time is 2 h, to obtain a composite microalloyed steel with a thickness of 4 mm.

[0128] The composite microalloyed steel prepared in Example 5 contains the following chemical components in percentage by weight: Ni: 2.90%, Mn: 1.35%, Cr: 1.26%, Mo: 0.47%, Cu: 0.52%, C: 0.08%, P: 0.012%, S: 0.007%, and the remainder is Fe and unavoidable impurities.

[0129] Example 6

[0130] 1) spraying lime powder (spraying amount is 8.5 kg / t) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.005 weight%;

[0131] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 220m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 0.4h and the temperature of the molten steel out of the furnace is 1660°C;

[0132] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.83 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.91% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.246% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.50% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.79% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.35 m 3 / t / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, raise temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time of LF refining is 2h;

[0133] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0134] 5) Cut the continuous casting billet into slabs with a thickness of 200 mm, send them into a heating furnace and heat them to 1225° C., use high-pressure water to dephosphorize them when they come out of the heating furnace, and then send them into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1220° C., the final rolling temperature is 860° C., and the coiling temperature is 680° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 7600° C., the annealing speed is 90 m / min, and the annealing time is 2 h, to obtain a composite micro-alloyed steel with a thickness of 15 mm.

[0135] The composite microalloyed steel prepared in Example 6 contains the following chemical components in percentage by weight: Ni: 2.1%, Mn: 1.12%, Cr: 0.72%, Mo: 0.42%, Cu: 0.08%, C: 0.11%, P: 0.012%, S: 0.007%, and the remainder is Fe and unavoidable impurities.

[0136] Example 7

[0137] 1) spraying lime powder (spraying amount is 10kg / t) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.007 weight%;

[0138] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 226m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 0.2h and the temperature of the molten steel out of the furnace is 1680°C;

[0139] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.82 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.91% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.246% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.50% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.79% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.25m 3 / t / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, raise temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time of LF refining is 2h;

[0140] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0141] 5) Cut the continuous casting billet into slabs with a thickness of 300 mm, send it into a heating furnace and heat it to 1250° C., use high-pressure water to dephosphorize it when it comes out of the heating furnace, and then send it into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1250° C., the final rolling temperature is 890° C., and the coiling temperature is 720° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 850° C., the annealing speed is 90 m / min, and the annealing time is 2 h, to obtain a composite micro-alloyed steel with a thickness of 25 mm.

[0142] The composite microalloyed steel prepared in Example 7 contains the following chemical components in weight percentage: Ni: 2.50%, Mn: 1.29%, Cr: 1.16%, Mo: 0.42%, Cu: 0.23%, C: 0.075%, P: 0.015%, S: 0.009%, and the remainder is Fe and unavoidable impurities.

[0143] Example 8

[0144] 1) spraying lime powder (spraying amount is 7.9 kg / t) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.007 weight%;

[0145] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 228m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 1.5h, and the temperature of the molten steel out of the furnace is 1640°C;

[0146] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.80 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.91% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.246% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.50% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.79% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.40 m 3 / t / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, raise temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time of LF refining is 2h;

[0147] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0148] 5) Cut the continuous casting billet into slabs with a thickness of 250 mm, send them into a heating furnace and heat them to 1250° C., use high-pressure water to dephosphorize them when they come out of the heating furnace, and then send them into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1250° C., the final rolling temperature is 880° C., and the coiling temperature is 700° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 820° C., the annealing speed is 90 m / min, and the annealing time is 2 h, to obtain a composite microalloyed steel with a thickness of 22 mm.

[0149] The composite microalloyed steel prepared in Example 8 contains the following chemical components in weight percentage: Ni: 2.50%, Mn: 1.29%, Cr: 1.16%, Mo: 0.42%, Cu: 0.23%, C: 0.075%, P: 0.015%, S: 0.009%, and the remainder is Fe and unavoidable impurities.

[0150] Example 9

[0151] 1) spraying lime powder (spraying amount is 8.0 kg / t) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.007 weight%;

[0152] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 215m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is completed to obtain the converter blown molten steel, wherein the converter steelmaking time is 1.5h and the temperature of the molten steel out of the furnace is 1650°C;

[0153] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.80 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.91% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.246% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.50% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.79% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.38 m 3 / t / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, raise temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time of LF refining is 2h;

[0154] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0155] 5) Cut the continuous casting billet into slabs with a thickness of 250 mm, send them into a heating furnace and heat them to 1240° C., use high-pressure water to dephosphorize them when they come out of the heating furnace, and then send them into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1220° C., the final rolling temperature is 880° C., and the coiling temperature is 690° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 760° C., the annealing speed is 90 m / min, and the annealing time is 4.5 h, to obtain a composite microalloyed steel with a thickness of 22 mm.

[0156] The composite microalloyed steel prepared in Example 9 contains the following chemical components in weight percentage: Ni: 3.1%, Mn: 1.29%, Cr: 1.23%, Mo: 0.72%, Cu: 0.04%, C: 0.055%, P: 0.014%, S: 0.008%, and the remainder is Fe and unavoidable impurities.

[0157] Example 10

[0158] 1) spraying lime powder (spraying amount is 8.6 kg / t) into the ladle for desulfurization, and then slag treatment to obtain desulfurized molten steel, wherein the molten steel temperature during the desulfurization process is ≥1300°C, and the S content in the obtained desulfurized molten steel is ≤0.007 weight%;

[0159] 2) Add desulfurized molten steel into the converter for steelmaking, and blow oxygen at the top and bottom of the converter (the oxygen flow rate is 280m 3 / t / h), removing P and C, when the C content in the desulfurized molten steel is ≤0.05% by weight and the P content is ≤0.01% by weight, the blowing is finished to obtain the converter blown molten steel, wherein the converter steelmaking time is 2h and the temperature of the molten steel out of the furnace is 1690°C;

[0160] 3) Slag blocking during converter steel tapping, adding deoxidizer (Al particles, added in an amount of 0.83 kg / t) for deoxidation during the steel tapping process, and then adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks and pure Ni to the converter blown steel water, wherein the addition amount of Cr alloy blocks is 1.91% by weight of the converter blown steel water, the addition amount of Mn alloy blocks is 1.246% by weight of the converter blown steel water, the addition amount of Mo alloy blocks is 2.50% by weight of the converter blown steel water, the amount of pure Cu material is 0.1% by weight of the converter blown steel water, the addition amount of pure Ni is 2.79% by weight of the converter blown steel water, and then putting into a ladle, blowing argon into the ladle for stirring (the flow rate of argon is 0.41m 3 / t / h), promote the floating of inclusions, then carry out LF refining, add alloy, add slag, raise temperature, and continuously adjust the composition of molten steel to meet the target requirements to obtain refined molten steel, wherein the initial temperature of LF refining of molten steel is 1580℃, and the time is 2h;

[0161] 4) The ladle enters the continuous casting workshop for continuous casting to obtain continuous casting billets;

[0162] 5) Cut the continuous casting billet into slabs with a thickness of 260 mm, send them into a heating furnace and heat them to 1240° C., use high-pressure water to dephosphorize them when they come out of the heating furnace, and then send them into a rolling unit for rough rolling, finish rolling, and coiling, wherein the rough rolling end temperature is 1240° C., the final rolling temperature is 870° C., and the coiling temperature is 690° C., and then the steel obtained after coiling is cold rolled and annealed, wherein the annealing temperature is 750° C., the annealing speed is 90 m / min, and the annealing time is 2 h, to obtain a composite microalloyed steel with a thickness of 21 mm.

[0163] The composite microalloyed steel prepared in Example 10 contains the following chemical components in weight percentage: Ni: 3.10%, Mn: 1.12%, Cr: 1.26%, Mo: 0.31%, Cu: 0.58%, C: 0.064%, P: 0.018%, S: 0.03%, and the remainder is Fe and unavoidable impurities.

[0164] Comparative Example 1

[0165] The method of Example 1 is followed, except that in step 3), no Cr alloy block is added, and the amount of Mo alloy block is increased, so that the prepared composite microalloyed steel does not contain Cr, and the Mo content is 1.57%, that is, the Mo content is the sum of the contents of Cr and Mo in Example 1, and the contents of the remaining components are basically the same as in Example 1.

[0166] Comparative Example 2

[0167] The method of Example 1 is followed, except that in step 3), pure Ni is not added, so that the prepared composite microalloyed steel does not contain Ni, and the contents of other components are substantially the same as those in Example 1.

[0168] Comparative Example 3

[0169] The method of Example 1 is followed, except that in step 3), no Cr alloy block is added, so that the prepared composite microalloyed steel does not contain Cr, and the contents of other components are substantially the same as those in Example 1.

[0170] Comparative Example 4

[0171] The method of Example 1 is followed, except that in step 3), no Mo alloy block is added, so that the prepared composite microalloyed steel does not contain Mo, and the contents of other components are substantially the same as those in Example 1.

[0172] Comparative Example 5

[0173] The method of Example 1 is followed, except that in step 3), no Mn alloy block is added, so that the prepared composite microalloyed steel does not contain Mn, and the contents of other components are substantially the same as those in Example 1.

[0174] Test Example 1

[0175] The composite micro-alloyed steels prepared in Examples 1-10 and Comparative Examples 1-5, and ordinary 16Mn steel were subjected to corrosion resistance tests. The test method is: the composite micro-alloyed steels and 16Mn steels were placed in a top circulation line environment of a coking unit mixed with waste oil (chloride ion saturation, humidity 100%, hydrogen sulfide content not less than 100 ppm), taken out after 180 days, and their corrosion rates were detected and calculated. The results are shown in Table 1 below.

[0176] Table 1

[0177] Example No. Uniform corrosion rate (mm / a) Relative reduction ratio of 16Mn Example 1 0.26 84.6% Example 2 0.23 86.4% Example 3 0.25 85.3% Example 4 0.29 82.3% Example 5 0.23 86.4% Example 6 0.29 82.8% Example 7 0.25 85.2% Example 8 0.24 85.8% Example 9 0.25 85.2% Example 10 0.27 84.0% Comparative Example 1 0.74 56.2% Comparative Example 2 0.52 69.2% Comparative Example 3 0.79 53.3% Comparative Example 4 0.65 61.5% Comparative Example 5 0.82 51.5% 16Mn Steel 1.69 0

[0178] It can be seen from Table 1 that the corrosion rate of the composite microalloyed steel prepared in the present invention in a wet hydrogen sulfide environment is significantly lower than that of the composite microalloyed steel and 16Mn steel prepared in the comparative example.

[0179] Test Example 2

[0180] The yield strength, tensile strength and elongation of the composite microalloyed steels prepared in Examples 1-10 and Comparative Examples 1-5, and ordinary 16Mn steel were tested according to GB / T 228.1 standard, using a slow strain rate tensile test. The results are shown in Table 2 below.

[0181] Table 2

[0182] Example No. Yield strength (MPa) Tensile strength(MPa) Elongation after break (%) Example 1 365 560 25.5 Example 2 355 537 26.7 Example 3 345 562 23.7 Example 4 374 564 24.4 Example 5 357 533 29.6 Example 6 372 520 25.8 Example 7 387 582 24.5 Example 8 358 525 28.4 Example 9 345 530 29.2 Example 10 349 550 26.2 Comparative Example 1 315 509 21.4 Comparative Example 2 287 504 21.9 Comparative Example 3 298 461 20.7 Comparative Example 4 295 492 20.1 Comparative Example 5 314 458 25.2 16Mn Steel Requirements 275~345 470~660 ≥21%

[0183] It can be seen from Table 2 that the composite microalloyed steel prepared in the present invention has higher yield strength, tensile strength and elongation after fracture.

[0184] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A composite microalloyed steel, characterized in that: Based on the total weight of the composite microalloyed steel, the weight percentages of the chemical components it contains are: Ni: 2-3.1%, Mn: 0.8-1.8%, Cr: 0.5-1.5%, Mo: 0.1-0.8%, Cu: 0.05-0.6%, C: 0.03-0.12%, P: ≤0.018%, S: ≤0.03%, and the balance is Fe and unavoidable impurities.

2. The composite microalloyed steel according to claim 1, characterized in that: The weight percentage of the chemical components contained in the composite microalloyed steel is: Ni: 2.5-2.8%, Mn: 1.0-1.5%, Cr: 0.8-1.2%, Mo: 0.3-0.5%, Cu: 0.2-0.3%, C: 0.05-0.1%, P: ≤0.015%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

3. The composite microalloyed steel according to claim 1 or 2, characterized in that: The corrosion rate of the composite microalloyed steel in the atmospheric and vacuum pressure and coking device tower top circulation process environment is lower than 0.3 mm / a, wherein the process environment is saturated with chloride ions, 100% humidity, and the hydrogen sulfide content is not lower than 100 ppm.

4. The composite microalloyed steel according to any one of claims 1 to 3, characterized in that: The yield strength of the composite microalloy steel is ≥345MPa, the tensile strength is 470-660MPa, and the elongation after fracture is ≥23%.

5. A method for preparing composite microalloyed steel, characterized in that: The method comprises the following steps: S1, adding Cr alloy blocks, Mn alloy blocks, Mo alloy blocks, pure Cu materials and pure Ni materials into the converter blowing molten steel for refining, and continuously casting the obtained refined molten steel to obtain a continuously cast billet; S2, rolling the continuous casting billet to obtain composite microalloyed steel; Wherein, in step S1, the weight percentages of chemical components contained in the refined molten steel are: Ni: 2-3.1%, Mn: 0.8-1.8%, Cr: 0.5-1.5%, Mo: 0.1-0.8%, Cu: 0.05-0.6%, C: 0.03-0.12%, P: ≤0.018%, S: ≤0.03%, and the remainder is Fe and unavoidable impurities.

6. The method according to claim 5, characterized in that In step S1, the amount of the Cr alloy block is 1-3% by weight of the molten steel produced by the converter, and the Cr content in the Cr alloy block is 10-60% by weight; Preferably, in step S1, the amount of the Mn alloy block is 1-3% by weight of the molten steel produced by the converter, and the Mn content in the Mn alloy block is 20-80% by weight; Preferably, in step S1, the amount of the Mo alloy block is 0.2-3% by weight of the molten steel blown by the converter, and the content of Mo in the Mo alloy block is 10-60% by weight; Preferably, in step S1, the amount of pure Cu material used is 0-1% by weight of the molten steel blown in the converter; Preferably, in step S1, the amount of pure Ni material used is 1-4 weight % of the molten steel blown in the converter.

7. The method according to claim 5 or 6, characterized in that: The S1 includes: (1) desulfurizing and deslagging molten steel to obtain desulfurized molten steel, wherein the temperature of the molten steel during the desulfurization process is ≥1300° C., and the sulfur content in the desulfurized molten steel is ≤0.007 wt %; (2) adding the desulfurized molten steel to a converter for steelmaking, and re-blowing oxygen at the top and bottom of the converter. When the C content in the desulfurized molten steel is ≤0.05 wt % and the P content is ≤0.01 wt %, the blowing is completed to obtain the converter blown molten steel; (3) The slag is blocked when the converter is tapped, and Cr alloy blocks, Mn alloy blocks, Mo alloy blocks, pure Cu materials and pure Ni materials are added to the molten steel blown in the converter, and then the molten steel is put into a ladle, argon is blown into the ladle for stirring, and then LF refining is performed, alloys are added, slag is added, the temperature is increased, and the composition is continuously adjusted so that the molten steel meets the target requirements to obtain refined molten steel.

8. The method according to claim 7, characterized in that In step (2), the conditions for converter steelmaking include: the converter steelmaking time is 0.1 to 2 hours, and the temperature of the molten steel out of the furnace is 1600 to 1700°C.

9. The method according to claim 7 or 8, characterized in that: In step (2), during the double oxygen blowing process at the top and bottom of the converter, the oxygen flow rate is 210-280m 3 / ton / h.

10. The method according to any one of claims 7 to 9, characterized in that: In step (3), a deoxidizer is added during the steel tapping process; Preferably, the deoxidizer is selected from one or more of Al particles, SiFe particles and MnFe particles.

11. The method according to any one of claims 7 to 10, characterized in that: In step (3), during the argon blowing and stirring process, the flow rate of argon is 0.15 to 0.43 m 3 / ton / h.

12. The method according to any one of claims 7 to 11, characterized in that: In step (3), the conditions for LF refining include: the initial temperature of LF refining of molten steel is 1550-1600°C, and the time of LF refining is 0.6-3h.

13. The method according to claim 5, characterized in that In step S2, the rolling process includes: cutting the continuous casting billet into a fixed length, sending it into a heating furnace and heating it to 1220-1250°C, dephosphorizing it with high-pressure water when it leaves the heating furnace, and then rolling and coiling it.

14. The method according to claim 13, characterized in that The rolling process includes rough rolling and finish rolling; Preferably, the final rolling temperature of the rolling is 840-910°C.

15. The method according to claim 13 or 14, characterized in that The coiling temperature of the coiling is 600-720°C.

16. The method according to claim 13 or 14, characterized in that The rolling process also includes: cold rolling and annealing the steel obtained after coiling.

17. The method according to claim 16, characterized in that The annealing conditions include: an annealing temperature of 750-850° C. and an annealing speed of 80-100 m / min.

18. Composite microalloyed steel prepared by the method according to any one of claims 5 to 17.