Preparation method of chromium nitride PVD (Physical Vapor Deposition) coating and metal workpiece applying coating

By combining etching and sputtering processes in the preparation of chromium nitride PVD plating, ion power supply is added to improve the ionization rate of argon and nitrogen, the problem of poor binding force between chromium nitride and metal substrate is solved, and the coating is realized The denseness and hardness increase simplifies the process and reduces costs.

CN118932303APending Publication Date: 2024-11-12ZHEJIANG SHINTOWN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310529226.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing vapor deposition process of chromium nitride, the bonding force of chromium nitride and metal substrate is poor, resulting in complex and high cost. Composite deposition or transition layer is required to improve the bonding force.

Method used

In the preparation of chromium nitride PVD plating, uneven microporous structures are generated on the metal substrate through etching process, and an ionic power supply is added in the sputtering and deposition process to increase the ionization rate of argon and nitrogen, and increase the band Positive ion weight promotes the deposition and nucleation of CrN plating, forming a dense plating layer.

Benefits of technology

The preparation process of chromium nitride plating is simplified, the bonding force and hardness of the plating layer and metal substrate are improved, the deposition time and cost are reduced, and the firm adhesion and performance of the plating are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004223921340000061
    Figure BDA0004223921340000061
Patent Text Reader

Abstract

The invention discloses a preparation method of a chromium nitride PVD (Physical Vapor Deposition) coating and a metal workpiece applying the coating. The preparation method comprises the following steps: vacuumizing and preheating: putting the metal workpiece into a working furnace chamber, vacuumizing and preheating the metal workpiece; in the heating and low-pressure argon atmosphere, negative bias voltage is applied to the metal workpiece through a bias power supply, and current is applied to the metal workpiece through an ion power supply; in the low-pressure argon atmosphere, negative bias voltage is applied to the metal workpiece through a bias power supply, and current is applied to the metal workpiece through an ion power supply; applying current to the magnetron target material through a sputtering power supply, so that the target material is sputtered and deposited on the metal workpiece; and cooling: cooling the metal workpiece and releasing vacuum to atmospheric pressure. According to the method, deposition of chromium nitride on the surface of the base material can be realized on the premise that the binding force, hardness and non-stickiness of the chromium nitride plating layer and the base material are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of physical vapor deposition, and in particular to a method for preparing a chromium nitride PVD coating and a metal workpiece using the coating. Background Art

[0002] The vapor deposited chromium nitride coating has a low friction coefficient and high surface hardness, as well as good non-stick and corrosion resistance, making it play an important role in industries such as molds and chip cutting tools.

[0003] Since the bonding strength between the chromium nitride deposition layer and the metal substrate is relatively poor, the existing vapor deposition process mostly uses composite deposition of chromium nitride and other materials or adds a transition layer such as Cr, CrTiBN to improve the bonding strength between chromium nitride and the metal substrate. The process is relatively complex and the cost is high. Summary of the invention

[0004] The present application provides a method for preparing a chromium nitride PVD coating and a metal workpiece using the coating, which can effectively simplify the preparation process of the chromium nitride coating and ensure the bonding strength between the chromium nitride coating and the metal substrate.

[0005] In a first aspect, the present application provides a method for preparing a chromium nitride PVD coating, which comprises the following steps: Vacuuming and preheating: Put the metal workpiece into the working furnace chamber, vacuumize and preheat the metal workpiece; Etching: In a heated and low-pressure argon atmosphere, a negative bias is applied to the metal workpiece through a bias power supply, and an electric current is applied to the metal workpiece through an ion power supply; Sputtering deposition: In a low-pressure argon atmosphere, a negative bias is applied to the metal workpiece through a bias power supply, and an electric current is applied to the metal workpiece through an ion power supply; an electric current is applied to the magnetron target through a sputtering power supply, so that the target material is sputtered and deposited on the metal workpiece; Cooling: Cool the metal workpiece and release the vacuum to atmospheric pressure.

[0006] In the preparation method of the present application, the metal workpiece is etched before the sputtering deposition of the chromium nitride coating, and an uneven microporous structure is generated on the metal substrate by etching, which is conducive to improving the physical connection between the chromium nitride and the metal workpiece substrate, which is similar to the mortise and tenon structure, and enhancing the bonding force between the chromium nitride and the substrate. Specifically, in the etching process, compared with the conventional process, the present application adds an ion power supply on the basis of the bias power supply. The ion power supply can ionize the argon gas, increase its ionization rate, increase the content of positively charged argon ions, and accelerate the bombardment of the substrate surface under the action of the ion beam magnetic field force, break through the tiny dust on the surface of the substrate, and free its surface atoms from the substrate, forming an etching morphology containing a denser microporous structure, which is conducive to improving the bonding force between the CrN coating and the metal workpiece substrate.

[0007] Similarly, an ion power supply is also added to the sputtering deposition process of the present application to increase the ionization rate of argon gas, increase the amount of positively charged argon ions and bombard the target material, sputter out more plasma, thereby increasing the ionization rate of nitrogen gas, increasing the amount of positively charged nitrogen ions, and accelerating the deposition of N and Cr atoms in CrN under the action of the ion beam magnetic field force, promoting the growth of CrN grains, increasing the deposition rate of the coating, and shortening the deposition time. At the same time, the acceleration of the ion source can transfer higher energy to the deposited atoms through collision, increase the mobility of the deposited atoms, form more nucleation sites, refine the grains, make the coating denser, and improve the bonding strength and hardness of the coating.

[0008] In summary, by combining the etching process with the sputtering deposition process and adding the above two sets of ion power supplies, it is possible to simplify the CrN deposition process and shorten the deposition time while achieving a firm bond between the CrN coating and the metal workpiece substrate.

[0009] Preferably, in the vacuum preheating step, the preheating temperature is 100-150°C; the vacuum degree is (1-5)×10 -3 Pa.

[0010] Preferably, the preheating time is 5 to 15 minutes, and the preheating time refers to the time taken for the vacuum degree and temperature in the working furnace chamber to reach the target value (preheating temperature).

[0011] Vacuuming during the preheating process can remove the air in the furnace chamber and avoid the deposition of impurities as much as possible.

[0012] Preferably, in the etching process, the argon gas flow rate is 500-1500 sccm; the voltage value of the negative bias is 500-1000 V; and the current value of the ion power supply is 1-10 A.

[0013] In the etching process, the bias power supply cooperates with the ion power supply to help the ionization of argon gas and accelerate the ionized positively charged argon ions, thereby increasing the bombardment intensity and density, thereby forming a denser microporous morphology on the surface of the metal workpiece substrate, which is beneficial to improving the density and bonding strength of the CrN coating.

[0014] Preferably, in the etching process, the vacuum degree is 0.8-5 Pa; and the heating temperature is 100-150°C.

[0015] Preferably, the etching depth is 0.1-0.3 um.

[0016] Preferably, the etching time is 5 to 15 minutes.

[0017] Preferably, in the sputtering deposition process, the current value of the sputtering power supply is 30-100A; the voltage value of the negative bias is 100-300V; the current value of the ion power supply is 1-10A; the argon gas flow rate is 40-160sccm, and the nitrogen gas flow rate is 200-400sccm.

[0018] More preferably, the current value of the sputtering power supply is 60-90A; and the nitrogen flow rate is 150-350sccm.

[0019] In the traditional sputtering process, due to the low ionization rate and low deposition rate, CrN is easy to form a larger grain structure, making the coating surface rough and not dense, and it is also easy to adsorb impurity molecules in the working furnace chamber, causing defects in film bonding and hardness performance. In this application, by coordinating the sputtering power supply, bias power supply and ion power supply, the ionization rate of argon and nitrogen can be accelerated and improved, the sputtering time can be shortened, the deposition density of CrN can be increased, and the grain structure of the coating can be refined, thereby improving the bonding and hardness of the CrN coating and the metal workpiece.

[0020] It should be noted that the voltage and current values ​​of the bias power supply and the ion power supply should not be too high, because this can easily lead to excessive nucleation energy, excessive stress in the coating, and increased defects, which in turn affect properties such as bonding strength and hardness.

[0021] Preferably, in the sputtering deposition process, the vacuum degree is 0.1-1 Pa, more preferably 0.1-0.5 Pa.

[0022] Preferably, the sputtering time is 5 to 15 minutes.

[0023] Preferably, the thickness of the chromium nitride coating of the present application is 0.9-1.5 μm.

[0024] Preferably, in the sputtering deposition process, the distance between the target and the metal workpiece is 50 to 100 mm.

[0025] The above spacing is conducive to forming a uniform and dense CrN coating. Specifically, if the spacing is too large, the deposition speed and density will decrease, which will easily cause coating defects. If the spacing is too small, the deposition uniformity will decrease, which is not conducive to improving the bonding strength.

[0026] Preferably, during the sputtering deposition process, the current value of the ion power supply increases uniformly at a rate of 0.5 to 1.5 A / min.

[0027] In the initial state of sputtering deposition, the Cr atoms produced by the argon gas bombarding the target in the chamber are relatively less than the N atoms, and they are unevenly distributed, which is not conducive to the formation of CrN and uniform deposition, and the strength and non-stick properties of the coating will decrease. If the current value of the ion power supply is too high at the beginning, the ionization rate of Ar gas and N2 is high, which will accelerate the above-mentioned uneven situation. The present application helps to overcome this problem by controlling the uniform increase of the current value of the ion power supply.

[0028] Preferably, in the cooling step, the vacuum is released after the metal workpiece is cooled to 70-100°C.

[0029] In the cooling of the present application, it is achieved through a water circulation system in the sputtering equipment, and the cooling time is usually 5 to 10 minutes.

[0030] In a second aspect, the present application provides a metal workpiece using any of the above-mentioned coatings, wherein the atomic content of Cr in the coating is 55-95%, and the atomic content of N is 5-45%.

[0031] Preferably, the atomic content of Cr in the coating is 80%, and the atomic content of N is 20%.

[0032] Under the above atomic ratio, the balance of heat resistance, corrosion resistance, non-stickiness and hardness of the CrN coating can be guaranteed, which is conducive to the application of the coating in the inner tank of home appliances.

[0033] The above-mentioned metal workpieces include but are not limited to cooking utensils and knives.

[0034] In summary, this application has the following beneficial effects: 1. This application does not need to use the method of setting an intermediate coating or adding other materials to the coating to improve the bonding strength between CrN and the substrate. By adding an ion power supply in the etching and sputtering process, the CrN coating can be firmly attached to the metal substrate, effectively saving the deposition process and shortening the deposition time.

[0035] 2. This application effectively ensures the uniformity of coating deposition and improves the density and bonding strength of the coating by controlling the distance between the metal workpiece and the magnetron target. DETAILED DESCRIPTION Example

[0036] Example 1: A metal workpiece with a chromium nitride PVD coating is prepared according to the following steps: Vacuum preheating: Place the metal workpiece with 304 stainless steel substrate into the working furnace chamber, seal and evacuate to 4×10 -3 Pa, while evacuating the vacuum, the metal workpiece was heated to 130°C within 6.5 min by heating the substrate.

[0037] Etching: Keep the temperature of the metal workpiece at 130°C, introduce argon gas into the working furnace chamber at a rate of 800 sccm, and control the vacuum degree at 3±0.1 Pa. Apply a negative bias voltage of 750V to the metal workpiece through a bias power supply, and apply a current of 6A to the metal workpiece through an ion power supply to etch the surface of the metal workpiece for 10 minutes.

[0038] Sputtering deposition: Argon and nitrogen are introduced into the furnace chamber, with an argon flow rate of 50sccm and a nitrogen flow rate of 300sccm, so that the vacuum degree is controlled at 0.5Pa. Then a negative bias voltage is applied to the metal workpiece through a bias power supply, with a voltage value of 230V; a current is applied to the metal workpiece through an ion power supply, and its current value is 8A. Cr with a purity of 99.8% is used as the target material, and the distance between the target material and the metal workpiece is 60mm. A current is applied to the magnetron target material through a sputtering power supply, and its current size is 55A, so that the target material is sputtered and deposited on the metal workpiece, and the sputtering deposition time is 8min.

[0039] Cooling: The metal workpiece is cooled by water circulation in the furnace chamber. When the temperature drops to 80°C, the vacuum is released to atmospheric pressure and the workpiece is cooled to room temperature to obtain a product with a chromium nitride coating (1 μm thick), in which the N content is 20% and the Cr content is 80%.

[0040] Example 2, a metal workpiece with a chromium nitride PVD coating is prepared according to the following steps: Vacuum preheating: Place the metal workpiece with 304 stainless steel substrate into the working furnace chamber, seal and evacuate to 2×10 -3 Pa, while evacuating the vacuum, the metal workpiece is heated to 130°C within 6.5 minutes by heating the substrate.

[0041] Etching: Keep the temperature of the metal workpiece at 130°C, introduce argon gas into the working furnace chamber at a rate of 1400 sccm, and control the vacuum degree at 4±0.1 Pa. Apply a negative bias voltage of 600 V to the metal workpiece through a bias power supply, and apply a current of 8 A to the metal workpiece through an ion power supply to etch the surface of the metal workpiece for 10 minutes.

[0042] Sputtering deposition: Argon and nitrogen are introduced into the furnace chamber, with an argon flow rate of 60sccm and a nitrogen flow rate of 360sccm, and the vacuum degree is controlled at 0.3Pa. Then a negative bias voltage is applied to the metal workpiece through a bias power supply, with a voltage value of 300V; a current is applied to the metal workpiece through an ion power supply, and its current value is 8A. Cr with a purity of 99.8% is used as the target material, and the distance between the target material and the metal workpiece is 60mm. A current is applied to the magnetron target material through a sputtering power supply, and its current size is 80A; the target material is sputtered and deposited on the metal workpiece; the sputtering deposition time is 10min.

[0043] Cooling: The furnace chamber and the metal workpiece are cooled by water circulation in the furnace chamber. When the temperature drops to 80°C, the vacuum is released to atmospheric pressure and the product is cooled to room temperature to obtain a product with a chromium nitride coating (1 μm thick), in which the N content is 30% and the chromium content is 70%.

[0044] Example 3, a metal workpiece with a chromium nitride PVD coating is prepared according to the following steps: Vacuum preheating: Place the metal workpiece with 304 stainless steel substrate into the working furnace chamber, seal and evacuate to 4×10 -3 Pa, while evacuating the vacuum, the metal workpiece is heated to 150°C within 10 minutes by heating the substrate.

[0045] Etching: Keep the temperature of the metal workpiece at 150°C, introduce argon gas into the working furnace chamber, the amount of argon gas introduced is 1000sccm, and the vacuum degree is controlled at 3±0.1Pa. Apply a negative bias voltage to the metal workpiece through a bias power supply, the voltage value is 750V, and apply a current to the metal workpiece through an ion power supply, the current size is 4A, so as to etch the surface of the metal workpiece, and the etching time is 12min.

[0046] Sputtering deposition: Argon and nitrogen are introduced into the furnace chamber, with an argon flow rate of 250sccm and a nitrogen flow rate of 400sccm, and the vacuum degree is controlled at 0.5Pa. Then a negative bias voltage of 200V is applied to the metal workpiece through a bias power supply; a current of 8A is applied to the metal workpiece through an ion power supply. Cr with a purity of 99.8% is used as the target material, and the distance between the target material and the metal workpiece is 100mm. A current of 100A is applied to the magnetron target material through a sputtering power supply; the target material is sputtered and deposited on the metal workpiece; the sputtering deposition time is 6min.

[0047] Cooling: The furnace chamber and the metal workpiece are cooled by water circulation in the furnace chamber. When the temperature drops to 80°C, the vacuum is released to atmospheric pressure and the temperature is further cooled to room temperature to obtain a product with a chromium nitride coating (1 μm thick) with an N content of 10% and a chromium content of 90%.

[0048] Example 4: A metal workpiece with a chromium nitride PVD coating is prepared according to the following steps: Vacuum preheating: Place the metal workpiece with 304 stainless steel substrate into the working furnace chamber, seal and evacuate to 4×10 -3 Pa, while evacuating the vacuum, the metal workpiece was heated to 130°C within 6.5 min by heating the substrate.

[0049] Etching: Keep the temperature of the metal workpiece at 130°C, introduce argon gas into the working furnace chamber at a rate of 800 sccm, and control the vacuum degree at 3±0.1 Pa. Apply a negative bias voltage of 750V to the metal workpiece through a bias power supply, and apply a current of 6A to the metal workpiece through an ion power supply to etch the surface of the metal workpiece for 10 minutes.

[0050] Sputtering deposition: Argon and nitrogen are introduced into the furnace chamber, with an argon flow rate of 60sccm and a nitrogen flow rate of 400sccm, so that the vacuum degree is controlled at 0.5Pa. Then a negative bias voltage is applied to the metal workpiece through a bias power supply, with a voltage value of 230V; a current is applied to the metal workpiece through an ion power supply, and its current value is 8A. Cr with a purity of 99.8% is used as the target material, and the distance between the target material and the metal workpiece is 60mm. A current is applied to the magnetron target material through a sputtering power supply, and its current size is 55A, so that the target material is sputtered and deposited on the metal workpiece, and the sputtering deposition time is 8min.

[0051] Cooling: The metal workpiece is cooled by water circulation in the furnace chamber. When the temperature drops to 80°C, the vacuum is released to atmospheric pressure and the workpiece is cooled to room temperature to obtain a product with a chromium nitride coating (1 μm thick), in which the N content is 45% and the chromium content is 55%.

[0052] Example 5, a metal workpiece with chromium nitride PVD coating, is different from Example 1 in that the distance between the target and the metal workpiece is 35 mm.

[0053] Example 6, a metal workpiece with chromium nitride PVD coating, is different from Example 1 in that the distance between the target and the metal workpiece is 110 mm.

[0054] Example 7, a metal workpiece with a chromium nitride PVD coating, differs from Example 1 in that, during the sputtering deposition process, the initial current of the ion power supply is 0 and increases at a rate of 1 A / min. When the current reaches 8 A, the power is maintained, and the sputtering deposition time is 10 minutes.

[0055] Comparative Example Comparative Example 1 is a metal workpiece coated with chromium nitride PVD. The difference from Example 1 is that no ion power source is used in the etching process.

[0056] Comparative Example 2 is a metal workpiece with a chromium nitride PVD coating. The difference from Example 1 is that the workpiece is not etched, and sputtering deposition is directly performed after vacuuming and preheating.

[0057] Comparative Example 3 is a metal workpiece coated with chromium nitride PVD. The difference from Example 1 is that no ion power source is used in the sputtering deposition process.

[0058] Performance testing 1. Friction coefficient: The test was conducted using a friction and wear tester (CETR, model UMT-3).

[0059] 2. Hardness: A nano indentation hardness tester is used with a load of 400 mN. The hardness test result is calculated through a curve of force and indentation depth, and the test value is converted based on 1 GPa = 102.04 HV.

[0060] 3. Adhesion strength of chromium nitride coating: tested by Rockwell indentation method with a load of 60KG.

[0061] Table 1. Test results Analysis of test results: It can be seen from the combination of Examples 1 to 6 and Comparative Examples 1 to 3 and Table 1 that the present application can significantly improve the bonding force, hardness and non-stick performance (low friction coefficient) of the chromium nitride coating by adding an ion power supply in the etching process and the sputtering deposition process. The reason may be that the ion power supply can increase the ionization rate of argon gas, increase the amount of positively charged argon ions and bombard the target material, sputter out more plasma, thereby increasing the ionization rate of nitrogen gas, increasing the amount of positively charged nitrogen ions, and accelerating the deposition of N and Cr atoms in CrN under the action of the ion beam magnetic field force, promoting the growth of CrN grains, increasing the deposition rate of the coating, and shortening the deposition time. At the same time, the acceleration of the ion source can transfer higher energy to the deposited atoms through collision, increase the mobility of the deposited atoms, form more nucleation sites, and refine the grains, which can make the coating denser and improve the bonding force and hardness of the coating.

[0062] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing a chromium nitride PVD coating, characterized in that: The steps include: Vacuuming and preheating: Put the metal workpiece into the working furnace chamber, vacuumize and preheat the metal workpiece; Etching: In a heated and low-pressure argon atmosphere, a negative bias is applied to the metal workpiece through a bias power supply, and an electric current is applied to the metal workpiece through an ion power supply; Sputtering deposition: In a low-pressure argon atmosphere, a negative bias is applied to the metal workpiece through a bias power supply, and a current is applied to the metal workpiece through an ion power supply; a current is applied to the magnetron target through a sputtering power supply, so that the target material is sputtered and deposited on the metal workpiece; Cooling: Cool the metal workpiece and release the vacuum to atmospheric pressure.

2. The method for preparing a chromium nitride PVD coating according to claim 1, characterized in that: In the vacuum preheating step, the preheating temperature is 100-150°C; the vacuum degree is (1-5) × 10 -3 Pa.

3. The method for preparing a chromium nitride PVD coating according to claim 1, characterized in that: In the etching process, the amount of argon gas introduced is 500-1500 sccm; the voltage value of the negative bias is 500-1000 V; and the current value of the ion power supply is 1-10 A.

4. The method for preparing a chromium nitride PVD coating according to claim 1, characterized in that: In the etching process, the vacuum degree is 0.8-5 Pa; the heating temperature is 100-150°C.

5. The method for preparing a chromium nitride PVD coating according to claim 1, characterized in that: In the sputtering deposition process, the current value of the sputtering power supply is 30-100A; the voltage value of the negative bias is 100-300V; the current value of the ion power supply is 1-10A; the argon gas flow rate is 40-160sccm, and the nitrogen gas flow rate is 200-400sccm.

6. The method for preparing a chromium nitride PVD coating according to claim 1, characterized in that: In the sputtering deposition process, the vacuum degree is 0.1-1Pa.

7. The method for preparing a chromium nitride PVD coating according to claim 1, characterized in that: During the sputtering deposition process, the distance between the target and the metal workpiece is 50 to 100 mm.

8. The method for preparing a chromium nitride PVD coating according to claim 1, characterized in that: In the cooling step, the vacuum is released after the metal workpiece is cooled to 70-100°C.

9. A metal workpiece coated with any one of claims 1 to 8, characterized in that: The atomic content of Cr in the coating is 55-95%, and the atomic content of N is 5-45%.

10. The metal workpiece according to claim 9, characterized in that The atomic content of Cr in the coating is 80%, and the atomic content of N is 20%.