Preparation method and application of rich-grain-boundary ruthenium-based high-entropy oxide catalyst

By introducing 3d transition metal elements into RuO2 lattice and preparing grain boundary-rich ruthenium-based high-entropy oxide catalysts by using molten salt method, the problem of poor performance of ruthenium-based amino synthesis catalysts in the prior art is solved, and high efficiency and low cost are achieved The catalyst preparation significantly improves the catalytic activity and stability of OER and is suitable for electrolyzing hydrogen production.

CN118932377APending Publication Date: 2024-11-12UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411006333.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing high-entropy oxide catalysts have poor performance in ruthenium-based amino synthesis catalysts, and there are fewer high-efficiency and low-cost ruthenium-based high-entropy oxide materials, making it difficult to meet the requirements of catalytic activity and stability.

Method used

Using the fast unequilibrium molten salt method, four 3d transition metal elements are introduced into the RuO2 lattice to form a high-entropy material with entropy stability effect, and alkali metal nitrates are used as solvent-reaction medium to quickly cool water to form Abundant grain boundary and oxygen vacancies, prepare a grain boundary-rich ruthenium-based high-entropy oxide catalyst.

Benefits of technology

It significantly improves the activity and stability of the catalyst, optimizes the oxygen evolution reaction process, reduces the amount of precious metal Ru, improves the catalytic activity of OER, and is suitable for hydrogen production by electrolyzing water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932377A_ABST
    Figure CN118932377A_ABST
Patent Text Reader

Abstract

The invention relates to the field of high-entropy oxide catalysts, and discloses a preparation method and application of a rich-grain-boundary ruthenium-based high-entropy oxide catalyst.The operation includes the steps that ruthenium chloride hydrate, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate with the total amount being 6 mmol are weighed and dissolved in absolute ethyl alcohol, ultrasonic treatment is conducted, and a uniform solution is obtained; putting the mixture into a drying oven until the solvent is completely evaporated, and grinding the obtained material into uniform powder for later use; weighing 0.2 mol of alkali metal nitrate, placing the alkali metal nitrate in a ceramic crucible, heating the ceramic crucible in a muffle furnace until a molten salt transparent solution is formed, rapidly adding the prepared precursor powder, and keeping the constant temperature for 2 hours; after the heat preservation procedure is finished, the crucible is rapidly taken out of the muffle furnace and rapidly cooled with water, a product is collected through suction filtration and washed three times with water and ethyl alcohol respectively, then the product is dried overnight in a vacuum drying oven, and the high-entropy ruthenium-based oxide catalyst with the rich grain boundaries is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of high entropy oxide catalysts, and in particular to a preparation method and application of a grain boundary-rich ruthenium-based high entropy oxide catalyst. Background Art

[0002] High entropy materials are a new type of material composed of five or more metal elements in equimolar ratios or near equimolar ratios. High entropy oxides are regarded as potential candidates for OER catalysts due to their excellent electrochemical properties. They can provide abundant grain boundaries and active sites, thereby significantly improving their catalytic activity and stability.

[0003] In the prior art, there are three catalyst preparation methods, namely, impregnation method, mechanical mixing method and sublimation method, as disclosed in the prior art "[1] Yan Haiyu, Research on Novel High Surface Area Graphite Carbon Supported Ruthenium-based Ammonia Synthesis Catalyst [D], Zhejiang University of Technology, 2014", and the anti-methanation stability of Ba-Ru-K / HSAG ammonia synthesis catalyst was studied.

[0004] However, the performance of the ruthenium-based ammonia synthesis catalyst mentioned in the prior art is poor, and HEOs, due to its diversified element combination and unique structural characteristics, has become an effective method to improve the performance of ruthenium-based catalysts. However, in the existing HEMs field, there are relatively few high-efficiency, low-cost ruthenium-based high-entropy oxide materials. Therefore, a high-efficiency, low-cost high-entropy ruthenium-based oxide is designed. Summary of the invention

[0005] The object of the present invention is to provide a preparation method and application of a grain boundary-rich ruthenium-based high entropy oxide catalyst to solve the problems in the prior art.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst, the preparation method comprises the following steps:

[0008] Step 1: Weigh a total of 6 mmol of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate, dissolve them in anhydrous ethanol, ultrasonicate to obtain a uniform solution, place the solution in an oven until the solvent evaporates completely, and grind the obtained material into a uniform powder for later use.

[0009] Step 2: Weigh 0.2 mol of alkali metal nitrate and place it in a ceramic crucible. Heat the ceramic crucible in a muffle furnace until a transparent molten salt solution is formed. Rapidly add the precursor powder prepared in step 1 and maintain a constant temperature for 2 hours.

[0010] Step 3. At the end of the insulation program, the crucible is quickly taken out of the muffle furnace and quickly cooled with water. The product is collected by filtration, washed three times with water and ethanol respectively, and then dried in a vacuum drying oven overnight to obtain a high-entropy ruthenium-based oxide catalyst with rich grain boundaries.

[0011] Furthermore, the raw materials of the high entropy ruthenium-based oxide catalyst are as follows:

[0012] Ruthenium chloride hydrate, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate, manganese chloride tetrahydrate, anhydrous ethanol, alkali metal nitrate, water.

[0013] Furthermore, in step 1, the molar ratio of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate is 2:1:1:1:1, and the content of anhydrous ethanol for dissolving the raw materials is 5-10 mL.

[0014] When weighing the raw materials in step 1, ruthenium chloride hydrate, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate, manganese chloride tetrahydrate and alkali metal nitrate are all weighed at room temperature and weighed using weighing paper.

[0015] Furthermore, the ultrasonic time in step 1 is 15-20 min, and the temperature of the oven is 70-80°C.

[0016] Furthermore, in step 2, the alkali metal nitrate includes KNO3 and NaNO3.

[0017] Furthermore, in step 2, the heating is performed at a rate of 5-10°C per minute to 350-380°C, and the constant temperature is 350-380°C.

[0018] Furthermore, in step 3, the temperature in the vacuum drying oven is 70-80°C.

[0019] Furthermore, in step 3, the crucible is rapidly cooled with rapid water to achieve a material having a large number of oxygen vacancies and abundant grain boundaries.

[0020] A grain boundary-rich ruthenium-based high entropy oxide catalyst is prepared by the preparation method of the grain boundary-rich ruthenium-based high entropy oxide catalyst.

[0021] Furthermore, a grain boundary-rich ruthenium-based high entropy oxide catalyst is used as an OER catalyst.

[0022] Beneficial effects of the present invention:

[0023] 1. The preparation method of the present invention prepares a ruthenium-based high-entropy oxide material with abundant grain boundaries by utilizing a rapid non-equilibrium molten salt method, and introduces four 3d transition metal elements with activity enhancement into the RuO2 lattice to form a high-entropy material with an entropy stabilization effect, which not only improves the activity and stability of the catalyst, but also effectively reduces the amount of precious metal Ru. The abundant grain boundaries and a large number of oxygen vacancies make the material have a lower metal oxidation state and more coordinated unsaturated Ru active centers, thereby optimizing the adsorption of key intermediates in the oxygen evolution reaction process and producing a more excellent OER catalytic activity;

[0024] 2. The preparation method of the present invention is not only simple in process and easy to operate, but also can provide a large amount of oxidizing ions O by using molten alkali metal nitrate (sodium nitrate, potassium nitrate) as a solvent and reaction medium. 2- Reacting with metal precursors to generate metal oxides can accelerate the reaction kinetics. Subsequent rapid water cooling is conducive to the formation of a large number of oxygen vacancies and abundant grain boundaries, thus making the material exhibit excellent electrocatalytic OER performance;

[0025] 3. The preparation method of the present invention can not only significantly improve its OER catalytic activity and stability, but also reduce the amount of ruthenium used, and is suitable for hydrogen production by water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention will be further described below in conjunction with the accompanying drawings.

[0027] Figure 1 is a SEM image of the high entropy ruthenium-based oxide catalyst of the present invention;

[0028] Figure 2 is a TEM image of the high entropy ruthenium-based oxide catalyst of the present invention;

[0029] Figure 3 It is a mapping diagram of the high entropy ruthenium-based oxide catalyst of the present invention;

[0030] Figure 4 It is a XAS comparison diagram of the high entropy ruthenium-based oxide catalyst of the present invention and ruthenium dioxide;

[0031] Figure 5 It is a XAS comparison diagram of the high entropy ruthenium-based oxide catalyst of the present invention and ruthenium dioxide;

[0032] Figure 6 is an XPS graph of the high entropy ruthenium-based oxide catalyst of the present invention;

[0033] Figure 7 is an XPS graph of the high entropy ruthenium-based oxide catalyst of the present invention;

[0034] Figure 8It is an OER performance diagram of the high entropy ruthenium-based oxide catalyst of the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] A preparation method and application of a ruthenium-based high-entropy oxide catalyst rich in grain boundaries. A ruthenium-based high-entropy oxide material with rich grain boundaries is prepared by a rapid non-equilibrium molten salt method. Four 3d transition metal elements with activity enhancement effects are introduced into the RuO2 lattice to form a high-entropy material with an entropy stabilization effect.

[0037] A method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst. The raw materials required for preparing the catalyst are as follows:

[0038] Ruthenium chloride hydrate, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate, manganese chloride tetrahydrate, anhydrous ethanol, alkali metal nitrate, water.

[0039] The steps of the preparation method are as follows:

[0040] Step 1. Weigh 6 mmol of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate in a molar ratio of 2:1:1:1:1 and dissolve them in 5-10 mL of anhydrous ethanol. Ultrasonicate for 15-20 min to obtain a uniform solution, place it in an oven at 70-80° C. until the solvent is completely evaporated, and grind the obtained material into a uniform powder for later use.

[0041] Among them, when weighing the five raw materials, ruthenium chloride hydrate, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate, manganese chloride tetrahydrate and alkali metal nitrates need to be weighed at room temperature and with weighing paper, and should not be weighed in an overly humid environment to prevent the materials from absorbing moisture.

[0042] Step 2: Weigh 0.2 mol of alkali metal nitrate and place it in a ceramic crucible. Heat the ceramic crucible in a muffle furnace at a rate of 5-10°C per minute to 350-380°C until a transparent molten salt solution is formed. Rapidly add the precursor powder prepared in step 1 and keep it at 350-380°C for 2 hours.

[0043] The alkali metal nitrate used in step 2 is prepared by using a molten alkali metal nitrate (sodium nitrate, potassium nitrate) as a solvent and reaction medium, which can provide a large amount of oxidizing ions O 2- Reacting with metal precursors to form metal oxides can accelerate the reaction kinetics.

[0044] Step 3. At the end of the insulation program, the crucible is quickly removed from the muffle furnace and quickly cooled with water. The product is collected by filtration, washed three times with water and ethanol respectively, and then dried in a vacuum drying oven at 70-80°C overnight to obtain a high-entropy ruthenium-based oxide catalyst with rich grain boundaries.

[0045] The rapid water cooling used in step 3 is to achieve a material with a large number of oxygen vacancies and abundant grain boundaries.

[0046] Example 1

[0047] A method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst, the steps of the preparation method are as follows:

[0048] Step 1, weighing a total of 6 mmol of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate in a molar ratio of 2:1:1:1:1, dissolving them in 5 mL of anhydrous ethanol, ultrasonicating for 15 min to obtain a uniform solution, placing the solution in an oven at 80° C. until the solvent is completely evaporated, and grinding the obtained material into a uniform powder for later use;

[0049] Step 2, weigh 0.2 mol of NaNO3 and place it in a ceramic crucible, heat the ceramic crucible in a muffle furnace to 350°C at a rate of 5°C per minute until a transparent molten salt solution is formed, quickly add the precursor powder prepared in step 1, and keep it at 350°C for 2h;

[0050] Step 3. At the end of the insulation program, the crucible is quickly taken out of the muffle furnace and quickly cooled with water. The product is collected by filtration, washed three times with water and ethanol respectively, and then dried in a vacuum drying oven at 80°C overnight to obtain a high-entropy ruthenium-based oxide catalyst with rich grain boundaries.

[0051] Example 2

[0052] A method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst, the steps of the preparation method are as follows:

[0053] Step 1, weighing a total of 6 mmol of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate in a molar ratio of 2:1:1:1:1, dissolving them in 10 mL of anhydrous ethanol, ultrasonicating for 20 min to obtain a uniform solution, placing the solution in an oven at 80° C. until the solvent is completely evaporated, and grinding the obtained material into a uniform powder for later use;

[0054] Step 2, weigh 0.2 mol of KNO3 and place it in a ceramic crucible, heat the ceramic crucible to 380°C in a muffle furnace at a rate of 10°C per minute until a transparent molten salt solution is formed, quickly add the precursor powder prepared in step 1, and keep the temperature at 380°C for 2h;

[0055] Step 3. At the end of the insulation program, the crucible is quickly taken out of the muffle furnace and quickly cooled with water. The product is collected by filtration, washed three times with water and ethanol respectively, and then dried in a vacuum drying oven at 80°C overnight to obtain a high-entropy ruthenium-based oxide catalyst with rich grain boundaries.

[0056] Example 3

[0057] A method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst, the steps of the preparation method are as follows:

[0058] Step 1, weighing a total of 6 mmol of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate in a molar ratio of 2:1:1:1:1, dissolving them in 5 mL of anhydrous ethanol, ultrasonicating for 15 min to obtain a uniform solution, placing the solution in an oven at 70° C. until the solvent is completely evaporated, and grinding the obtained material into a uniform powder for later use;

[0059] Step 2, weigh 0.2 mol of NaNO3 and place it in a ceramic crucible, heat the ceramic crucible to 360°C in a muffle furnace at a rate of 5°C per minute until a transparent molten salt solution is formed, quickly add the precursor powder prepared in step 1, and keep the temperature at 360°C for 2h;

[0060] Step 3. At the end of the insulation program, the crucible is quickly taken out of the muffle furnace and quickly cooled with water. The product is collected by filtration, washed three times with water and ethanol respectively, and then dried in a vacuum drying oven at 70°C overnight to obtain a high-entropy ruthenium-based oxide catalyst with rich grain boundaries.

[0061] Example 4

[0062] A method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst, the steps of the preparation method are as follows:

[0063] Step 1, weighing a total of 6 mmol of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate in a molar ratio of 2:1:1:1:1, dissolving them in 7 mL of anhydrous ethanol, ultrasonicating for 17 min to obtain a uniform solution, placing the solution in an oven at 75° C. until the solvent is completely evaporated, and grinding the obtained material into a uniform powder for later use;

[0064] Step 2, weigh 0.2 mol of KNO3 and place it in a ceramic crucible, heat the ceramic crucible to 370°C in a muffle furnace at a rate of 7°C per minute until a transparent molten salt solution is formed, quickly add the precursor powder prepared in step 1, and keep the temperature at 370°C for 2h;

[0065] Step 3. At the end of the insulation program, the crucible is quickly taken out of the muffle furnace and quickly cooled with water. The product is collected by filtration, washed three times with water and ethanol respectively, and then dried in a vacuum drying oven at 75°C overnight to obtain a high-entropy ruthenium-based oxide catalyst with rich grain boundaries.

[0066] In step 2, the alkali metal nitrate used can be replaced by NaNO3 (>350℃) or KNO3 (>380℃), and then the material is made to have a large number of oxygen vacancies and abundant grain boundaries through rapid water cooling in step 3.

[0067] See also Figure 1-4 , the morphology characterization and OER performance of the high entropy ruthenium-based oxide catalyst RuFeCoNiMn-HEO were tested, and the test data are as follows:

[0068] like Figure 1-3 As shown, the SEM, TEM and Mapping images of the high-entropy ruthenium-based oxide material (RuFeCoNiMn-HEO) with rich grain boundaries prepared by the molten salt method indicate that its morphology is a two-dimensional nanosheet structure composed of countless nanoparticles, and the five metal elements are evenly dispersed in the entire catalyst structure. This preparation method can be applied to the preparation of the high-entropy ruthenium-based oxide material with rich grain boundaries.

[0069] like Figure 4 , Figure 5 As shown, the XAS pattern of the K-edge of Ru in the grain-boundary rich high-entropy ruthenium-based oxide material found that compared with the ruthenium dioxide (C-RuO2) in the prior art, the metallic oxidation state of Ru in RuFeCoNiMn-HEO is lower and has more coordinately unsaturated Ru centers.

[0070] like Figure 6 , Figure 7 As shown, the 3dXPS image of Ru in the grain-boundary rich high-entropy ruthenium-based oxide catalyst shows that the oxidation state of Ru metal in RuFeCoNiMn-HEO is lower than that in ruthenium dioxide (C-RuO2).

[0071] The oxygen evolution reaction performance of the samples was tested using a standard three-electrode electrochemical test method. Figure 8 As shown in Figure 2, it was found that the grain-boundary-rich high-entropy ruthenium-based oxide (RuFeCoNiMn-HEO) exhibited the best electrocatalytic OER activity at 10 mA / cm2 The overpotential is only 190mV at a current density of 200mA / cm 2 The overpotential at a current density of is also as low as 336 mV, which is superior to the catalysts in the prior art.

[0072] Compared with the related art, the preparation method of the high entropy ruthenium-based oxide catalyst with rich grain boundaries of the present invention has the following beneficial effects:

[0073] 1. A high-entropy ruthenium-based oxide catalyst material with rich grain boundaries was prepared using a rapid nonequilibrium molten salt method. The material has a large number of oxygen vacancies and abundant grain boundaries. The metal elements in the material have a lower metal oxidation state and a large number of coordinatively unsaturated Ru centers, thereby optimizing the adsorption energy of key intermediates in the oxygen evolution reaction and producing a more excellent electrocatalytic oxygen evolution reaction activity.

[0074] Second, the preparation process is not only simple and easy to operate, but also can provide a large amount of oxidizing ions O through the use of molten alkali metal nitrate as solvent and reaction medium. 2- Reacting with metal precursors to generate metal oxides can accelerate the reaction kinetics, and the subsequent rapid water cooling is conducive to the formation of a large number of oxygen vacancies and abundant grain boundaries, thus making the material exhibit excellent electrocatalytic OER performance.

[0075] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst, characterized in that: The operation steps of the preparation method are as follows: Step 1, weighing a total of 6 mmol of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate, dissolving them in anhydrous ethanol, ultrasonicating to obtain a uniform solution, placing the solution in an oven until the solvent is completely evaporated, and grinding the obtained material into a uniform powder for later use; Step 2, weigh 0.2 mol of alkali metal nitrate and place it in a ceramic crucible, heat the ceramic crucible in a muffle furnace until a transparent molten salt solution is formed, quickly add the precursor powder prepared in step 1, and keep the constant temperature for 2 hours; Step 3. At the end of the insulation program, the crucible is quickly taken out of the muffle furnace and quickly cooled with water. The product is collected by filtration, washed three times with water and ethanol respectively, and then dried in a vacuum drying oven overnight to obtain a high-entropy ruthenium-based oxide catalyst with rich grain boundaries.

2. The method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst according to claim 1, characterized in that: The raw materials of the high entropy ruthenium-based oxide catalyst are as follows: Ruthenium chloride hydrate, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate, manganese chloride tetrahydrate, anhydrous ethanol, alkali metal nitrate, water.

3. The method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst according to claim 2, characterized in that: In the step 1, the molar ratio of hydrated ruthenium chloride, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate and manganese chloride tetrahydrate is 2:1:1:1:1, and the content of anhydrous ethanol for dissolving the raw materials is 5-10 mL; When weighing the raw materials in step 1, ruthenium chloride hydrate, ferric chloride hexahydrate, cobalt chloride hexahydrate, nickel chloride hexahydrate, manganese chloride tetrahydrate and alkali metal nitrate are all weighed at room temperature and weighed using weighing paper.

4. The method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst according to claim 1, characterized in that: The ultrasonic time in step 1 is 15-20 min, and the temperature of the oven is 70-80°C.

5. The method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst according to claim 1, characterized in that: The alkali metal nitrate in step 2 includes KNO3 and NaNO3.

6. The method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst according to claim 5, characterized in that: In step 2, the temperature is heated to 350-380°C at a rate of 5-10°C per minute, and the constant temperature is 350-380°C.

7. The method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst according to claim 1, characterized in that: The temperature in the vacuum drying oven in step 3 is 70-80°C.

8. The method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst according to claim 7, characterized in that: In step 3, the crucible is rapidly cooled with rapid water to achieve a material having a large number of oxygen vacancies and abundant grain boundaries.

9. A grain boundary-rich ruthenium-based high entropy oxide catalyst, characterized in that: The catalyst is prepared by the method for preparing a grain boundary-rich ruthenium-based high entropy oxide catalyst according to any one of claims 1 to 8.

10. Use of a grain boundary-rich ruthenium-based high entropy oxide catalyst according to claim 9 as an OER catalyst.