Preparation method and application of amorphous FeCoCrNi film catalyst

Preparation of amorphous FeCoCrNi thin film catalyst through electrodeposition technology, solving the problem of kinetics of anodizing reaction in electrolytic water hydrogen production and high cost of precious metal catalysts, realizing low-cost and efficient oxidation reaction catalysis, and improving the production of hydrogen production by electrolytic water hydrogen production Efficiency and stability.

CN118932385APending Publication Date: 2024-11-12TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410925704.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing electrolytic hydrogen production technology, alkaline electrolyte has high corrosion resistance to electrolytic cells and electrodes, and the kinetics of the anode oxidation reaction is difficult, resulting in high voltage of the electrolytic cell to waste energy, and the cost of precious metal catalysts is high and unstable, which limits electrolytic water. The commercial development of anode.

Method used

The amorphous FeCoCrNi film catalyst is prepared by electrodeposition technology, and a catalyst with low overpotential, low Tafel slope and high active electrochemical area is formed through specific electrodeposition fluids and process conditions. The active site is adjusted using the polyvalent state of the Cr element to improve the Oxidation reaction efficiency.

Benefits of technology

It realizes low-cost, stable and efficient oxidation reaction catalysis, reduces the cost of hydrogen production by electrolyzing water, improves the water decomposition rate and catalytic efficiency of electrolyzing water, and has excellent cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932385A_ABST
    Figure CN118932385A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of an amorphous FeCoCrNi film catalyst, belongs to the technical field of water electrolysis catalysis, and develops a stable, efficient and low-cost catalyst in the water electrolysis hydrogen production process, and the preparation method comprises the following steps: mixing chloride-sulfate powder containing main salt elements with deionized water to obtain an electrodeposition solution, the preparation method comprises the following steps: preparing an amorphous FeCoCrNi film on the surface of a copper substrate, putting the pretreated copper substrate into an electro-deposition solution as a cathode for electro-deposition, cleaning and drying the sample after the reaction is completed, and preparing the amorphous FeCoCrNi film catalyst on the surface of the copper substrate, and the catalyst can be applied to the process of producing hydrogen by electrolyzing water. The preparation process is simple, safe and environment-friendly, the production cost can be reduced, and the production efficiency is improved. The amorphous FeCoCrNi thin film catalyst prepared by utilizing an electro-deposition technology has relatively high oxygen evolution reaction catalytic activity and good cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrolytic water catalysis, and specifically relates to a preparation method and application of an amorphous FeCoCrNi thin film catalyst. Background Art

[0002] With the continuous development of industrialization, not only the total amount of non-renewable resources - fossil fuels is gradually decreasing, but also the environmental pollution is aggravated. Human beings are facing serious resource, environmental and energy crises, so the development of various new energy and renewable energy has become a problem that countries around the world attach great importance to. At present, the research hotspots of new energy include solar energy, nuclear energy, geothermal energy, wind energy, tidal energy and hydrogen energy. Among them, hydrogen, as a clean and pollution-free renewable energy, can effectively solve energy and environmental problems. The existing hydrogen production technologies mainly include fossil fuel hydrogen production, nuclear energy hydrogen production, water electrolysis hydrogen production, biomass hydrogen production and photocatalytic hydrogen production. Compared with other hydrogen production technologies, water electrolysis hydrogen production technology has the advantages of simple process, reliable technology, easy to obtain high-purity hydrogen, green and pollution-free, and water is the most abundant resource on the earth, which has prompted researchers to conduct more in-depth research on water electrolysis technology.

[0003] The electrolysis of water is generally carried out in an electrolyzer. A voltage is applied to both ends of the electrolyzer, and a hydrogen evolution reaction (HER) occurs at the cathode, and an oxygen evolution reaction (OER) occurs at the anode. The electrolyte used in the electrolysis of water includes an acidic electrolyte or an alkaline electrolyte, but the acidic electrolyte is more corrosive to the electrolyzer and the electrodes, so alkaline electrolytes are generally used in industry. In the production of hydrogen by alkaline water electrolysis, the actual electrolyzer voltage is much higher than the theoretical voltage due to the influence of the overpotential of O2 and H2, electrolyte resistance and other factors. Moreover, the OER at the anode involves the transfer of four electrons and the formation of OO bonds, which is much more difficult than the hydrogen evolution reaction at the cathode. From a kinetic point of view, when the current increases significantly, HER and OER cause an overpotential (η), which not only wastes a lot of energy, but also reduces the water decomposition rate, which is not conducive to the development of the hydrogen economy. In the early days, the anode materials for water electrolysis were mainly precious metals such as Pt, Ir and Ru and their oxides. However, the reserves of precious metals are limited, the cost is high, and they may be oxidized during the OER process. These factors have greatly restricted the commercial development of precious metal anode oxygen evolution electrodes for water electrolysis. Therefore, the development of stable, efficient and low-cost water splitting catalysts is particularly important to solve the above problems. Summary of the invention

[0004] The main purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing an amorphous FeCoCrNi thin film catalyst and its application. An efficient oxygen evolution reaction electrocatalyst is obtained by electrodeposition technology, which has excellent characteristics such as low overpotential, low Tafel slope, high active electrochemical area, and long-term stability in water system.

[0005] The present invention is implemented by the following technical scheme: A method for preparing an amorphous FeCoCrNi thin film catalyst comprises the following steps:

[0006] S1. Prepare electrodeposition solution: weigh raw materials according to the following composition and their weight proportions: 7.5 parts of H3BO3, 22.5 parts of KCl, 27.6 parts of C6H8O·7H2O, 14.4 parts of C6H5Na3O7·2H2O, 60 parts of Cr2(SO4)3·6H2O, 1.2 parts of CoSO4·7H2O, 6 parts of NiSO4·6H2O, 0.6 parts of FeSO4·7H2O, and 0.3 parts of NaH2PO·H2O;

[0007] The weighed raw materials were completely dissolved in deionized water, and then NaOH solution was added to adjust the pH value of the mixed solution to 1.5;

[0008] S2, pretreatment of the copper substrate: first, the copper sheet is polished and mechanically polished in sequence to remove the oxide scale and scratches on the surface of the copper sheet; then, the copper sheet is degreased, polished and activated using acetone solution, polishing liquid and activation liquid respectively; finally, deionized water and alcohol ultrasonic cleaning are used in sequence to prepare the copper substrate, which is dried for standby use;

[0009] S3, electrodeposition: immerse the graphite sheet and the copper substrate prepared in step S2 in the electrodeposition solution prepared in step S1, and connect the copper substrate to the cathode and the graphite sheet to the anode. After checking that the circuit connection is correct, turn on the power switch to perform electrodeposition. The deposition temperature is 25°C to 30°C and the current density is 20A / dm 2 ~45A / dm 2 The deposition time is 10 min to 60 min, the stirring rate is 100 r / min to 200 r / min, and an amorphous FeCoCrNi thin film catalyst is prepared on the surface of the copper substrate.

[0010] The elements in the amorphous FeCoCrNi thin film catalyst are all selected from 3d transition metal elements. In the study of the first-row transition metals of OER under alkaline conditions, Cr has a rich valence state (Cr 0 Cr 2+ Cr 3+ and Cr 6+ ), where Cr 3+The Cr-200g / L FeCoCrNi film has the best catalytic performance in the electrolytic oxygen evolution reaction of water, with a 10 mA·cm -2 The overpotential at the current density is 295mV, and the Tafel slope is only 69.52mV·dec -1 , the electrochemical activity and stability are better than those of precious metal catalysts.

[0011] Furthermore, in step S1, the concentration of the NaOH solution is 15 wt.%.

[0012] Furthermore, in step S2, the dimensions of the copper sheet are: length 12 mm×width 12 mm×thickness 1 mm.

[0013] Furthermore, in step S2, the copper sheet is first polished with 1000# sandpaper, and then mechanically polished with 1500# and 2000# sandpapers in sequence.

[0014] Furthermore, in step S2, the copper sheet is immersed in the acetone solution for 2 minutes, the copper sheet is finely polished with the polishing liquid for 30 seconds, and the copper sheet is immersed in the activation solution for 10 minutes; the deionized water and alcohol ultrasonic cleaning times are both 15 minutes.

[0015] Furthermore, in the step S3, the amorphous FeCoCrNi thin film catalyst forms a dense and uniform cellular structure on the surface of the copper substrate, and the average particle size of the cellular structure is 8 μm.

[0016] The invention discloses an application of an amorphous FeCoCrNi thin film catalyst prepared by the method as described above in a process of producing hydrogen by electrolysis of water, comprising the following steps: using a Hg or HgO electrode as a reference electrode, a platinum sheet as a counter electrode, and a copper-based amorphous FeCoCrNi thin film catalyst as a working electrode, which are respectively connected to an electrochemical detection device, and using an alkaline solution saturated with H2 as an electrolyte to produce hydrogen by electrolysis of water.

[0017] The beneficial effects of the present invention are:

[0018] 1. The present invention utilizes electrodeposition technology to prepare an efficient amorphous FeCoCrNi thin film catalyst. During the electrodeposition process, specific metal ions in the electrodeposition solution obtain electrons under the action of an external electric field and are reduced and deposited on the cathode surface. By controlling the ion concentration, a thin film catalyst having a uniform and dense cellular structure that is beneficial to the electrocatalytic oxygen evolution reaction is obtained. The preparation process is simple, can reduce production costs, increase deposition rate, is environmentally friendly, and greatly reduces the cost of hydrogen production by alkaline water electrolysis.

[0019] 2. The present invention adopts electrodeposition technology to prepare amorphous FeCoCrNi thin film catalyst. Compared with crystalline catalysts, the prepared amorphous Cr-200g / L FeCoCrNi thin film has the most excellent OER performance. Its disordered atomic arrangement causes a large number of structural defects, which is beneficial to the diffusion and reaction of electrolyte ions, forms a large number of active sites, increases the reaction sites of the catalytic reaction, and improves the catalytic efficiency of water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Schematic diagram of the structure of the electrodeposition device; in the figure, 1 is a power supply, 2 is a cathode sample, 3 is an anode graphite sheet, 4 is an electrodeposition tank, and 5 is a constant temperature water bath;

[0021] Figure 2 The X-ray diffraction pattern of the amorphous Cr-200g / L FeCoCrNi thin film catalyst prepared in Example 1;

[0022] Figure 3 The scanning electron microscope images of the surface and cross section of the amorphous Cr-200g / L FeCoCrNi thin film catalyst prepared in Example 1; wherein (a) is a surface morphology image, and (b) is a cross-sectional morphology image;

[0023] Figure 4 This is a LSV comparison diagram of the amorphous Cr-200g / L FeCoCrNi thin film catalyst prepared in Example 1 and other FeCoCrNi thin film catalysts with different Cr contents;

[0024] Figure 5 It is a comparison diagram of the Tafel slope curves of the amorphous Cr-200g / L FeCoCrNi thin film catalyst prepared in Example 1 and other FeCoCrNi thin film catalysts with different Cr contents;

[0025] Figure 6 This is a cyclic stability test curve of the amorphous Cr-200g / L FeCoCrNi thin film catalyst prepared in Example 1 in the oxygen evolution reaction. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0027] The structure of the electrodeposition device used in this specific embodiment is as follows Figure 1 As shown, the power supply 1 is a constant current power supply, the cathode sample 2 and the anode graphite sheet 3 are connected to the positive and negative electrodes of the power supply 1 respectively, the electrodeposition tank 4 is a beaker with a volume of 500 mL, and the electrodeposition liquid in the beaker is heated in a water bath by a constant temperature water bath pot 5. The specific preparation process is as follows.

[0028] Example 1

[0029] A method for preparing an amorphous FeCoCrNi thin film catalyst comprises the following steps:

[0030] S1. Preparation of electrodeposition solution:

[0031] First, use an electronic balance to weigh the raw materials according to the following composition and their weight fractions: 7.5g H3BO3, 22.5g KCl, 27.6g C6H8O·7H2O, 14.4g C6H5Na3O7·2H2O, add the above raw materials to a beaker, add 300mL deionized water to the beaker, and place the beaker in a water bath and stir until dissolved; then, after the raw materials in the beaker are completely dissolved, use an electronic balance again to weigh the remaining raw materials according to the following composition and their weight fractions: 60g Cr2(SO4)3·6H2O, 1.2g CoSO4·7H2O, 6g NiSO4·6H2O, 0.6g FeSO4·7H2O, 0.3g NaH2PO·H2O, add the remaining raw materials weighed twice to the mixed solution, and continue stirring for 2h after the raw materials are completely dissolved; finally, add a NaOH solution with a concentration of 15wt.% to adjust the pH value of the mixed solution to 1.5;

[0032] S2, copper substrate pretreatment: First, the size of the copper sheet is: length 12mm×width 12mm×thickness 1mm, first use 1000# sandpaper to polish the copper sheet, and then use 1500# and 2000# sandpaper to mechanically polish the copper sheet in turn to remove the oxide scale and scratches on the surface of the copper sheet; then, use acetone solution, polishing liquid and activation liquid in turn to degrease, fine polish and activate the copper sheet respectively, the copper sheet is immersed in the acetone solution for 2 minutes, the copper sheet is finely polished with the polishing liquid for 30 seconds, and the copper sheet is immersed in the activation liquid for 10 minutes; finally, deionized water and alcohol ultrasonic cleaning are used in turn, the deionized water and alcohol ultrasonic cleaning time are 15 minutes, and the copper substrate is dried for standby use;

[0033] S3, electrodeposition: immerse the graphite sheet and the copper substrate prepared in step S2 into the electrodeposition solution prepared in step S1, and connect the copper substrate to the cathode and the graphite sheet to the anode. After checking that the circuit connection is correct, turn on the power switch to perform electrodeposition. The deposition temperature is 30°C and the current density is 25A / dm 2 , deposition time was 30 min, stirring rate was 200 r / min, and an amorphous FeCoCrNi thin film catalyst was prepared on the surface of the copper substrate.

[0034] On this basis, the concentration of chromium sulfate in the electrodeposition solution was changed, and other conditions remained unchanged. Amorphous FeCoCrNi thin film catalysts with different Cr contents were obtained by electrodeposition. The structure and performance of the obtained thin film catalysts were tested, and the results are shown below.

[0035] Depend on Figure 2 It can be seen that the amorphous FeCoCrNi thin film catalyst prepared on the copper substrate surface contains not only the diffraction peak of the copper substrate, but also a broad and gentle steamed bun peak near 2θ≈45°, indicating that all elements are dissolved in the same lattice and the FeCoCrNi film obtained by electrodeposition is amorphous.

[0036] Depend on Figure 3 It can be seen that the amorphous Cr-200g / L FeCoCrNi film has a typical cellular structure with an average particle size of 8 μm. The cracks on the film surface are evenly distributed, and the cells are uneven but uniform in size.

[0037] Example 2

[0038] An application of an amorphous FeCoCrNi thin film catalyst prepared by the method described in Example 1 in a process of producing hydrogen by electrolysis of water comprises the following steps: using a Hg or HgO electrode as a reference electrode, a platinum sheet as a counter electrode, and a copper-based amorphous FeCoCrNi thin film catalyst as a working electrode, which are respectively connected to an electrochemical detection device, and using an alkaline solution saturated with H2 as an electrolyte to produce hydrogen by electrolysis of water.

[0039] The results of water electrolysis to produce hydrogen are as follows Figure 4 As shown in the figure, the amorphous Cr-200g / L FeCoCrNi thin film catalyst has a current density of 10mA·cm -2 The overpotential of oxygen evolution reaction is 295 mA, which is significantly lower than that of FeCoCrNi thin film catalysts with other Cr contents.

[0040] Depend on Figure 5 It can be seen that the Tafel slope of the amorphous Cr-200g / L FeCoCrNi thin film catalyst during the oxygen evolution reaction is significantly lower than that of the FeCoCrNi thin film catalysts with other Cr contents (only 69.52 mV·dec -1 ). In the catalytic process, the lower the Tafel slope, the faster the rate of oxygen evolution reaction increases, which has better OER reaction kinetic properties.

[0041] Depend on Figure 6 It can be seen that after 1000 cycles, the LSV curve of the thin film catalyst after the cycle is not significantly different from the LSV curve of the initial catalyst, indicating that the amorphous Cr-200g FeCoCrNi film has good long-term cycle stability.

[0042] Example 3

[0043] A method for preparing an amorphous FeCoCrNi thin film catalyst. Step S1 and step S2 in this embodiment 3 are the same as those in embodiment 1, except that the electrodeposition parameters in step S3 are different: the deposition temperature is 25°C, the current density is 20A / dm 2 , deposition time was 10 min, stirring rate was 100 r / min, and an amorphous FeCoCrNi thin film catalyst was prepared on the surface of the copper substrate.

[0044] Example 4

[0045] A method for preparing an amorphous FeCoCrNi thin film catalyst. Step S1 and step S2 in this embodiment 4 are the same as those in embodiment 1, except that the electrodeposition parameters in step S3 are different: the deposition temperature is 27°C, the current density is 45A / dm 2 , deposition time was 60 min, stirring rate was 150 r / min, and an amorphous FeCoCrNi thin film catalyst was prepared on the surface of the copper substrate.

[0046] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for preparing an amorphous FeCoCrNi thin film catalyst, It is characterized in that The following steps are involved: S1. Preparation of electrodeposition solution: Weigh the raw materials according to the following composition and their weight parts: 7.5 parts H 3 BO 3 , 22.5 parts KCl, 27.6 parts C 6 H 8 O·7H 2 O, 14.4 parts C 6 H 5 Na 3 O 7 ·2H 2 O, 60 parts Cr 2 (SO 4 ) 3 6H 2 O, 1.2 parts CoSO 4 7H 2 O, 6 parts NiSO 4 6H 2 O, 0.6 parts FeSO 4 7H 2 O, 0.3 parts NaH 2 PO·H 2 O; The weighed raw materials were completely dissolved in deionized water, and then NaOH solution was added to adjust the pH value of the mixed solution to 1.5; S2, pretreatment of the copper substrate: first, the copper sheet is polished and mechanically polished in sequence to remove the oxide scale and scratches on the surface of the copper sheet; then, the copper sheet is degreased, polished and activated using acetone solution, polishing liquid and activation liquid respectively; finally, deionized water and alcohol ultrasonic cleaning are used in sequence to prepare the copper substrate, which is dried for standby use; S3, electrodeposition: immerse the graphite sheet and the copper substrate prepared in step S2 in the electrodeposition solution prepared in step S1, and connect the copper substrate to the cathode and the graphite sheet to the anode. After checking that the circuit connection is correct, turn on the power switch to perform electrodeposition. The deposition temperature is 25°C to 30°C and the current density is 20A / dm 2 ~45A / dm 2 The deposition time was 10 min ~ 60 min, the stirring rate was 100 r / min ~ 200 r / min, and an amorphous FeCoCrNi thin film catalyst was prepared on the surface of the copper substrate.

2. The method for preparing an amorphous FeCoCrNi thin film catalyst according to claim 1, Features: In step S1, the concentration of the NaOH solution is 15 wt.%.

3. The method for preparing an amorphous FeCoCrNi thin film catalyst according to claim 1, Features: In step S2, the size of the copper sheet is: length 12 mm×width 12 mm×thickness 1 mm.

4. A method for preparing an amorphous FeCoCrNi thin film catalyst according to claim 1 or 3, Features: In step S2, the copper sheet is firstly polished with 1000# sandpaper, and then mechanically polished with 1500# and 2000# sandpapers in sequence.

5. A method for preparing an amorphous FeCoCrNi thin film catalyst according to claim 1 or 3, Features: In step S2, the copper sheet is immersed in the acetone solution for 2 minutes, the copper sheet is finely polished with the polishing liquid for 30 seconds, and the copper sheet is immersed in the activation solution for 10 minutes; the deionized water and alcohol ultrasonic cleaning times are both 15 minutes.

6. The method for preparing an amorphous FeCoCrNi thin film catalyst according to claim 1, Features: In the step S3, the amorphous FeCoCrNi thin film catalyst forms a dense and uniform cellular structure on the surface of the copper substrate, and the average particle size of the cellular structure is 8 μm.

7. Use of an amorphous FeCoCrNi thin film catalyst prepared by the method as claimed in claim 1 in a process of producing hydrogen by electrolysis of water, It is characterized in that The following steps are involved: Hg or HgO electrode was used as reference electrode, platinum sheet was used as counter electrode, and copper-based amorphous FeCoCrNi thin film catalyst was used as working electrode. They were connected to electrochemical detection equipment respectively. 2 A saturated alkaline solution is used as the electrolyte to electrolyze water to produce hydrogen.