Forming method for prefabricated furnace wall of aluminum electrolysis cell
By using prefabricated furnaces in aluminum electrolytic cells, the problems of unstable formation of tanks and sliding of electrolyte blocks are solved, efficient and stable furnace formation is achieved, and the electrolytic current efficiency and electrolytic cell life are improved.
Patent Information
- Application Number
- CN202410989724.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing aluminum electrolytic cell pre-baked tanks form unstable, resulting in early damage, affecting the life and production efficiency of the electrolyte blocks of the commonly used methods are prone to slide and hindering the lifting and lowering of the anode, resulting in unfavorable production.
The prefabricated furnace method is used to build a weir wall around the furnace with a prefabricated furnace made of ice crystal and soda ash before starting the electrolytic tank. The molecular ratio is 2.7~3.1, and the powdered mixture is filled to form a polymer ratio for quicker furnace. Establish a regular furnace to protect artificial legs.
It achieves rapid formation of stable furnaces, shortens the electrolytic cell start management cycle, improves electrolytic current efficiency, reduces the risk of early damage, can withstand high-temperature environment without melting, and improves production stability.
Smart Images

Figure CN118932428A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum electrolysis production, and in particular relates to a molding method for a prefabricated furnace wall of an aluminum electrolysis cell. Background Art
[0002] The aluminum electrolysis process is not only a simple electrolytic production process, but also a dynamic equilibrium process including crust formation and melting. If the aluminum electrolytic cell is damaged, it will affect production. Generally speaking, the damage of the electrolytic cell is related to many factors, mainly depending on the quality of the cathode material, the cell structure design and the production operation.
[0003] The main factors that affect the normal life of aluminum electrolytic cells and their proportion in the life of the cell are roughly as follows: cell structure design accounts for 20%, furnace construction technology accounts for 20%, quality of raw materials for cell lining accounts for 10%, roasting start-up method accounts for 25%, and production operation management accounts for 25%. Of course, serious mistakes in any of the above factors can cause early damage to the cell lining. It can be seen that early damage is mostly the result of the combined influence of various factors. Among them, whether the naturally formed high molecular ratio regular furnace inside the electrolytic cell can be established and maintained can not only improve the current efficiency of the electrolytic cell, but also protect the cell lining to extend the life of the electrolytic cell. The quality of the cell wall is the top priority of electrolysis management and will directly affect the production during the cell life.
[0004] The existing pre-baked aluminum electrolytic cell's slot sidewall is mainly an unstable structural layer that is automatically formed in the early stage of electrolysis. Generally, it takes at least 3 months of abnormal period management after the electrolytic cell is roasted and started to form a regular slot sidewall. The purpose of abnormal period management after startup is to establish everything necessary for normal production of the cell and create good innate conditions so that management can be handy and achieve efficient and low-consumption production of the electrolytic cell. Once this opportunity is missed, it will be difficult to form a slot sidewall again in future production. Although edge processing is also carried out, the role is different and the work is passive, which will bring great disadvantages to future production management.
[0005] Before the electrolytic cell is loaded, a weir wall is built around the tank chamber with solid electrolyte blocks to protect the artificial legs. However, with this method, the electrolyte blocks can easily slide under the anode when and after the electrolytic cell is started, hindering the anode from being lifted or even damaging the lead screw of the anode lifting mechanism.
[0006] Secondly, the commonly used method is: first, place 2~3cm of cryolite around the tank, close to the edge of the anode bottom, then evenly spread calcium fluoride on the "artificial legs", then add cryolite to 10cm, then add cryolite and soda ash mixture on top, and then add cryolite all over to fill the tank (5~7cm above the upper surface of the anode group). The middle seam between the two rows of anodes is filled with cryolite, of which the cryolite around the tank is high molecular weight cryolite, and the middle seam is added with ordinary cryolite.
[0007] The above methods all have the problems of slow melting, easy to cause precipitation to form on the edges, and hinder the formation of high-quality grooves. Summary of the invention
[0008] The present invention provides a method for forming a prefabricated furnace wall of an aluminum electrolytic cell, which takes the construction of a good high-molecular ratio furnace wall as a starting point and quickly establishes an electrolytic cell furnace to achieve the purpose of improving the electrolytic current efficiency and reducing early damage to the electrolytic cell.
[0009] The technical solution adopted by the present invention is a method for forming a prefabricated furnace side of an aluminum electrolytic cell. Before the electrolytic cell is started for roasting and loading, a circle of weir walls is built around the furnace of the electrolytic cell with the prefabricated furnace side, so that the electrolytic cell can quickly form a good furnace side and protect the artificial legs when the roasting is started. The prefabricated furnace side is prepared by cryolite and soda ash, and is made into a standardized prefabricated furnace side according to the requirements of the excellent furnace side shape of the aluminum electrolytic cell, and its molecular ratio is 2.7~3.1.
[0010] Furthermore, the molecular ratio of the prefabricated furnace sidewall is greater than 2.8.
[0011] Furthermore, when prefabricated furnace walls are built around the furnace of the electrolytic cell, gaps between the prefabricated furnace walls are filled with a powdered mixture, the mixture including cryolite and soda ash, and the mass proportion of soda ash in the mixture is 5-15%.
[0012] Furthermore, the height of the prefabricated furnace sidewalls matches the furnace of the electrolytic cell and fits with the artificial legs of the electrolytic cell; each prefabricated furnace sidewall has a width of 200-600 mm and a thickness of 5-15 cm.
[0013] Compared with the prior art, the beneficial effect of the present invention is that a good polymer furnace side and furnace shape are constructed before the roasting is started, forming a furnace with uniform composition or uniform composition change and integrity, solving the uncontrollable factors such as composition, quality, shape, time, etc. in the furnace side formation process in the prior art, shortening the startup management cycle of the electrolytic cell, and improving the furnace management of the electrolytic cell. In addition, the initial melting temperature of the formed furnace side is high, which can withstand the melting effect of the electrolyte working temperature of 940°C to 970°C on the crust, so that the crystallization process does not proceed in the melting direction, thereby achieving the purpose of improving the electrolytic current efficiency and reducing the early damage of the electrolytic cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 A schematic diagram of the structure of the prefabricated furnace side of the electrolytic cell; Figure 2 A top view of a prefabricated furnace wall for an electrolytic cell; Figure 3 It is a partial schematic diagram of the connection between the prefabricated furnace side and the electrolytic cell; Figure 4 for Figure 2 Enlarged view of local A. DETAILED DESCRIPTION
[0015] The present invention will be further explained below in conjunction with the accompanying drawings to facilitate better understanding by those skilled in the art.
[0016] Example 1 A method for forming a prefabricated furnace wall of an aluminum electrolytic cell, before the electrolytic cell is roasted and loaded, a circle of weir walls is built around the furnace of the electrolytic cell with the prefabricated furnace wall, so that the electrolytic cell can quickly form a good furnace wall when roasting and starting and protect the artificial legs; the prefabricated furnace wall is prepared by mixing cryolite and soda ash, and is made into a fixed prefabricated furnace wall according to the requirements of the excellent furnace wall shape of the aluminum electrolytic cell, and its molecular ratio is 2.7~3.1 Furthermore, the molecular ratio of the above-mentioned prefabricated furnace sides is greater than 2.8. When the prefabricated furnace sides are built around the furnace of the electrolytic cell, the gaps between the prefabricated furnace sides are filled with a powdered mixture, which includes cryolite and soda ash, and the mass proportion of soda ash in the mixture is 5-15%.
[0017] Example 2 like Figure 1-4 As shown, a prefabricated furnace side of an aluminum electrolytic cell includes a furnace side single block 1. The furnace side single block 1 is made of multiple pieces, which are spliced and built around the bottom of the furnace of the electrolytic cell 2 to form a weir wall structure 3. The weir wall structure 3 fits the artificial legs of the electrolytic cell 2. Each furnace side single block 1 has a width of 200-600 mm and a thickness of 5-15 cm.
[0018] The furnace side monoblock 1 includes a corner section monoblock 101 and a splicing section monoblock 102. The corner section monoblock 101 is L-shaped to match the furnace corner of the electrolytic cell 2. The splicing section monoblock 102 is long and has T-shaped slots 103 and T-shaped platforms 104 at both ends of the corner section monoblock 101 and the splicing section monoblock 102. Two adjacent furnace side monoblocks 101 are spliced and fixed by the T-shaped slots 103 and the T-shaped platforms 104. The furnace side monoblocks are inlaid with matching concave and convex structures, which can not only be quickly connected and assembled, but also have good connection stability.
[0019] In order to improve the connection stability between the furnace side block 1 and the electrolytic cell 2, a circle of slots 201 are provided at the bottom of the electrolytic cell 2, and a boss 105 is provided at the bottom end of the furnace side block 1 at the bottom of the prefabricated furnace side corresponding to the slot 201. The furnace side block 1 is embedded in the slot 201 through the boss 105 and is connected to the electrolytic cell 2.
[0020] The present invention adopts polymer prefabricated groove sidewalls to improve the molecular ratio of the electrolytic cell and the final NaF / AlF3 molecular ratio (molar ratio, CR) reaches 2.9-3.1. A good furnace sidewall can promote better separation of carbon slag and electrolyte. Under the premise of high molecular ratio, the groove sidewalls established in this way will be more solid, the groove chamber will be more regular, and can withstand temperature fluctuations during normal production in the future.
[0021] The above-described embodiments are only for describing the preferred implementation of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit and principles of the present invention, various modifications and improvements made by those skilled in the art to the technical solution of the present invention should all fall within the scope of protection determined by the claims of the present invention.
Claims
1. A method for forming a prefabricated furnace wall of an aluminum electrolytic cell, characterized in that: Before the electrolytic cell is started for roasting and loading, a circle of weir walls is built around the furnace of the electrolytic cell with prefabricated furnace walls, so that the electrolytic cell can quickly form a good furnace wall and protect the artificial legs when roasting is started. The prefabricated furnace wall is prepared by cryolite and soda ash and is made into a fixed prefabricated furnace wall according to the furnace wall shape requirements of the aluminum electrolytic cell, and its molecular ratio is 2.7~3.
1.
2. The method for forming a prefabricated ridge of an aluminum electrolytic cell according to claim 1, characterized in that: The molecular ratio of the prefabricated furnace sidewall is greater than 2.
8.
3. The method for forming a prefabricated ridge of an aluminum electrolytic cell according to claim 1, characterized in that: When prefabricated furnace walls are built around the furnace of the electrolytic cell, the gaps between the prefabricated furnace walls are filled with a powdered mixture. The mixture includes cryolite and soda ash, and the mass proportion of soda ash in the mixture is 5-15%.
4. The method for forming a prefabricated ridge of an aluminum electrolytic cell according to claim 1, characterized in that: The height of the prefabricated furnace sidewall matches the furnace of the electrolytic cell and fits with the artificial legs of the electrolytic cell; the width of each prefabricated furnace sidewall is 200-600mm and the thickness is 5-15cm.