Plating solution of high-wear-resistance nickel-tungsten porous plating layer under oil-lacking condition, preparation method and electroplating method
By using the nickel-tungsten porous plating solution formula and DC continuous electroplating method under oil-free conditions, the wear resistance of the nickel-tungsten electroplating layer under oil-free conditions was solved, and a high wear resistance and environmentally friendly nickel-tungsten is achieved. Porous coating preparation simplifies process flow and reduces friction and wear.
Patent Information
- Application Number
- CN202411090533.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has not yet developed a nickel-tungsten porous plating layer suitable for oil-deficient conditions. In traditional chromium plating technology, hexavalent chromium is harmful to the human body and has environmental problems. Moreover, the wear resistance of nickel-tungsten electroplating layer under oil-deficient conditions has not been developed. Be effectively resolved.
The nickel-tungsten porous plating solution formula using aqueous solvents, including nickel sulfate, sodium tungstate, sodium citrate, sodium chloride and ammonium chloride, nickel-tungsten plating layer with porous structure is prepared by DC continuous electroplating method, using tungsten Sodium acid deposits under nickel induction to form holes, and the pH and ammonium chloride are adjusted to improve the stability of the plating solution.
The preparation of a porous nickel-tungsten plating layer with high wear resistance under oil-deficient conditions is realized, the plating solution formulation and preparation process is simplified, high requirements for the parameters of the electroplating equipment are avoided, and the friction coefficient and wear are reduced through the porous structure.
Smart Images

Figure CN118932441A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of a porous plating layer, and specifically discloses a plating solution formula, a preparation method and an electroplating method for a wear-resistant nickel-tungsten porous plating layer under oil-deficient conditions. Background Art
[0002] With the continuous development of industrial technology, electroplating layers are widely used in machinery, energy, catalysis and other fields. In order to meet the performance requirements of electroplating layers in the industrial field, people have designed and developed coatings with various structures. Among them, coatings with porous structures can significantly improve their wear resistance as surface protective layers.
[0003] Loose-porous chrome plating is a special form of wear-resistant chrome plating. Net-like grooves or dot-like gaps are generated on the surface of the loose-porous chrome plating layer, so that a certain amount of lubricating oil can be stored during use, which has the effect of reducing friction and lubrication to improve wear resistance. However, the hexavalent chromium used in the traditional chrome plating process is harmful to the human body and poses environmental problems. The nickel-tungsten electroplating layer has good mechanical properties and can be used as a substitute for hard chrome plating and applied to the surface protective layer of mechanical equipment. However, the preparation process of the nickel-tungsten porous plating layer that can be used in oil-deficient conditions has not yet been developed. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a plating solution, a preparation method and an electroplating method for a highly wear-resistant nickel-tungsten porous coating under oil-deficient conditions, so as to prepare a nickel-tungsten coating with a porous structure by a simple and easy-to-operate direct current, continuous electroplating method.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] The first technical purpose of the present invention is to provide a plating solution for a nickel-tungsten porous plating layer, wherein the mass percentages of the components in the plating solution whose solvent is water are: 0.47-2.81% nickel sulfate, 1.17-7.04% sodium tungstate, 2.62-26.17% sodium citrate, 0.52-0.8% sodium chloride, and 1.43-4.76% ammonium chloride.
[0007] It should be noted that nickel sulfate and sodium tungstate in the plating solution provide metal elements for the coating, and tungsten needs to be co-deposited in the coating under the induction of nickel elements. Tungsten elements have a hydrogen evolution catalytic effect, which is conducive to the formation of holes in the coating through hydrogen evolution. Sodium citrate is a complexing agent that realizes the complexation of metal ions and can adjust the pH of the plating solution. Ammonium chloride can improve the stability of the plating solution, and at the same time play a certain role as a buffer and adjust the pH of the plating solution. The increase in the pH of the plating solution will enhance the hydrogen evolution effect and increase the holes in the coating. Sodium chloride can increase the conductivity of the plating solution and improve the current efficiency.
[0008] The second technical purpose of the present invention is to provide a method for preparing a plating solution for a nickel-tungsten porous plating layer, which specifically comprises the following steps:
[0009] Weigh nickel sulfate, sodium tungstate, sodium citrate, sodium chloride and ammonium chloride respectively, dissolve nickel sulfate and sodium chloride in water to obtain a mixed aqueous solution of nickel sulfate and sodium chloride, dissolve sodium tungstate in water to obtain a sodium tungstate aqueous solution, dissolve sodium citrate in water to obtain a sodium citrate aqueous solution, and dissolve ammonium chloride in water to obtain an ammonium chloride aqueous solution;
[0010] First, a sodium tungstate aqueous solution and a sodium citrate aqueous solution are mixed to obtain a mixed solution, then an ammonium chloride aqueous solution is added to the mixed solution, and finally a mixed aqueous solution of nickel sulfate and sodium chloride is added; water is added to adjust the concentration of the plating solution for depositing a nickel-tungsten porous plating layer as claimed in claim 1, and the plating solution is obtained by mixing evenly.
[0011] It should be noted that the purpose of adding and mixing in batches is to avoid dissolving multiple reagents together to form precipitation, which would affect the use and performance of the plating solution.
[0012] The third technical purpose of the present invention is to provide a method for electroplating a nickel-tungsten porous coating, the specific steps of the method are as follows:
[0013] S1, polish the plated substrate, wash it with water, soak it in a 1 mol / L sodium hydroxide solution at room temperature, take it out, wash it again with water, soak it in a 1 mol / L hydrochloric acid solution at room temperature, take it out, rinse it with deionized water and set it aside;
[0014] S2, using the plated substrate treated in step S1 as the cathode and the pure platinum plate as the anode, immersing them in the plating solution as described above, and electroplating is performed with mechanical stirring. After the electroplating is completed, immersing the plated substrate in deionized water to recover the plating solution on the surface of the plated substrate, and then rinsing with anhydrous ethanol and drying to obtain a nickel-tungsten porous coating.
[0015] It should be noted that mechanical stirring or cathode movement can ensure the uniformity of the composition of the plating solution during the electroplating process; and soaking and rinsing the surface of the plated part after electroplating can ensure that there is no plating solution residue on the surface of the obtained coating.
[0016] Preferably, the soaking time at room temperature using sodium hydroxide is 3 minutes, and the soaking time at room temperature using hydrochloric acid is 15 seconds.
[0017] Preferably, the drying temperature is 25-50° C., the drying time is 2-10 min, and the mechanical stirring rate is 200-250 rpm.
[0018] Preferably, the electroplating adopts constant current, direct current continuous electroplating.
[0019] Furthermore, the current density of the cathode is 6-100 A / dm 2 The electroplating temperature is 40-60 ℃, and the DC continuous electroplating time is 5-600 min.
[0020] Preferably, no surfactant is added in the electroplating method and no pH value of the plating solution needs to be adjusted.
[0021] In summary, the plating solution, preparation method and electroplating method of a highly wear-resistant nickel-tungsten porous plating layer under oil-deficient conditions provided by the present invention have the following advantages:
[0022] The present invention can directly obtain a nickel-tungsten plating layer with a porous structure. Not only is the plating solution formula simple and easy to prepare, but no other surfactant is added to the plating solution, and no additional adjustment of the pH value of the plating solution is required. The present invention adopts constant current and direct current continuous electroplating, and does not require parameters to be changed during the electroplating process, and has low requirements on the power supply used for electroplating. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0024] Figure 1 This is the SEM image of Example 1 of the present invention;
[0025] Figure 2 This is a friction coefficient diagram of Example 1 of the present invention;
[0026] Figure 3 This is an optical photograph of the wear scar of Example 1 of the present invention;
[0027] Figure 4 This is the SEM image of Example 2 of the present invention;
[0028] Figure 5 is a friction coefficient diagram of Example 2 of the present invention;
[0029] Figure 6 This is an optical photograph of the wear scar of Example 2 of the present invention;
[0030] Figure 7 This is the SEM image of Example 3 of the present invention;
[0031] Figure 8 This is a friction coefficient diagram of Example 3 of the present invention;
[0032] Fig. 9 This is an optical photograph of the wear scar of Example 3 of the present invention;
[0033] Fig.10 This is the SEM image of Example 4 of the present invention;
[0034] Fig.11 This is a friction coefficient diagram of Example 4 of the present invention;
[0035] Fig.12 This is an optical photograph of the wear scar of Example 4 of the present invention;
[0036] Fig.13 This is the SEM image of Example 5 of the present invention;
[0037] Fig.14 is a friction coefficient diagram of Example 5 of the present invention;
[0038] Fig.15 This is an optical photograph of the wear scar of Example 5 of the present invention;
[0039] Fig.16 This is the SEM image of Example 6 of the present invention;
[0040] Fig.17 This is a friction coefficient diagram of Example 6 of the present invention;
[0041] Fig.18 This is an optical photograph of the wear scar of Example 6 of the present invention;
[0042] Fig.19 This is the SEM image of Example 7 of the present invention;
[0043] Fig. 20 is a friction coefficient diagram of Example 7 of the present invention;
[0044] Fig.21 This is an optical photograph of the wear scar of Example 7 of the present invention;
[0045] Fig. 22 This is the SEM image of Example 8 of the present invention;
[0046] Fig.23 This is a friction coefficient diagram of Example 8 of the present invention;
[0047] Fig.24 This is an optical photograph of the wear scar of Example 8 of the present invention;
[0048] Fig.25 This is the SEM image of Example 9 of the present invention;
[0049] Fig.26 This is a friction coefficient diagram of Example 9 of the present invention;
[0050] Fig. 27 This is an optical photograph of the wear scar of Example 9 of the present invention;
[0051] Fig.28 It is the SEM picture of comparative example;
[0052] Fig.29 The friction coefficient diagram for the comparative example;
[0053] Fig.30 This is an optical photograph of the wear scar of the comparative example. DETAILED DESCRIPTION
[0054] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0056] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0057] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0058] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0059] The invention discloses a plating solution, a preparation method and an electroplating method for a highly wear-resistant nickel-tungsten porous plating layer under oil-deficient conditions.
[0060] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as limiting the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0061] Example 1
[0062] The present embodiment discloses a plating solution for a nickel-tungsten porous plating layer, wherein the mass percentages of the components in the plating solution, in which the solvent is water, are: 1.41% nickel sulfate, 4.11% sodium tungstate, 13.08% sodium citrate, 0.8% sodium chloride, and 2.38% ammonium chloride.
[0063] 1 L of the above composition for preparing a nickel-tungsten porous plating solution, specifically comprising:
[0064] 1) dissolving 15.8 g of nickel sulfate and 9 g of sodium chloride in water to obtain a mixed aqueous solution;
[0065] 2) Dissolve 46.2 g of sodium tungstate in water to obtain a sodium tungstate aqueous solution;
[0066] 3) dissolving 147 g of sodium citrate in water to obtain a sodium citrate aqueous solution;
[0067] 4) dissolving 26.7 g of ammonium chloride in water to obtain an ammonium chloride aqueous solution;
[0068] 5) First, mix the sodium tungstate aqueous solution and the sodium citrate aqueous solution to obtain a mixed solution, then add the ammonium chloride aqueous solution to the mixed solution, and finally add the nickel sulfate and sodium chloride mixed aqueous solution, and add water to 1 L to obtain the final desired plating solution.
[0069] Furthermore, a method for electroplating a plating solution for a nickel-tungsten porous plating layer specifically comprises the following steps:
[0070] S1, polish the plated substrate, wash it with water, put it in a 1 mol / L sodium hydroxide solution, soak it at room temperature for 3 min, take it out, wash it again with water, put it in a 1 mol / L hydrochloric acid solution, soak it at room temperature for 15 s, take it out and rinse it with deionized water for later use;
[0071] S2, the treated plated part is used as cathode and the pure platinum plate is used as anode, immersed in the above electroplating solution, the plating solution temperature is maintained at 50 °C, and the current density is 6 A / dm 2 The DC plating time is 120 min, the mechanical stirring speed is 200-250 rpm, and constant current and DC continuous plating are adopted; after the electroplating is completed, the plated parts are immersed in deionized water to recover the plating solution on the surface of the plated parts. After soaking for 20 s, rinse with anhydrous ethanol for 10 s and then dry.
[0072] Example 2
[0073] The current density is 100 A / dm 2 , the DC plating time is 5 min, and other conditions are the same as those in Example 1.
[0074] Example 3
[0075] The mass percentages of the components in the plating solution are: nickel sulfate 1.41%, sodium tungstate 7.04%, sodium citrate 13.08%, sodium chloride 0.8%, and ammonium chloride 2.38%. The current density is 30 A / dm 2 , the DC plating time is 30 min, and other conditions are the same as those in Example 1.
[0076] Example 4
[0077] The mass percentages of the components in the plating solution are: 0.47% nickel sulfate, 4.11% sodium tungstate, 13.08% sodium citrate, 0.8% sodium chloride, and 2.38% ammonium chloride. Other conditions are the same as those in Example 3.
[0078] Example 5
[0079] The mass percentages of the components in the plating solution are: 2.81% nickel sulfate, 4.11% sodium tungstate, 13.08% sodium citrate, 0.8% sodium chloride, and 2.38% ammonium chloride. Other conditions are the same as those in Example 3.
[0080] Example 6
[0081] The mass percentages of the components in the plating solution are: 1.41% nickel sulfate, 4.11% sodium tungstate, 13.08% sodium citrate, 0.8% sodium chloride, and 1.43% ammonium chloride. Other conditions are the same as those in Example 3.
[0082] Example 7
[0083] The mass percentages of the components in the plating solution are: 1.41% nickel sulfate, 4.11% sodium tungstate, 13.08% sodium citrate, 0.8% sodium chloride, and 4.76% ammonium chloride. Other conditions are the same as those in Example 3.
[0084] Example 8
[0085] The mass percentages of the components in the plating solution are: 1.41% nickel sulfate, 4.11% sodium tungstate, 26.17% sodium citrate, 0.8% sodium chloride, and 2.38% ammonium chloride. Other conditions are the same as those in Example 3.
[0086] Example 9
[0087] The current density is 30 A / dm 2 , the DC plating time is 30 min, and other conditions are the same as those in Example 1.
[0088] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following experimental examples and comparative examples are used to further illustrate the technical features disclosed in the present invention, but they should not be understood as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without creative work are also considered to fall within the scope of protection of the present invention.
[0089] Comparative Example
[0090] The current density is 5 A / dm 2 , the DC plating time is 120 min, and other conditions are the same as those in Example 1.
[0091] Experimental example
[0092] (1) Wear resistance test under oil-starved conditions:
[0093] Friction and wear tests were conducted on the coatings prepared and treated in Examples 1-9 and the comparative examples. Before the friction and wear test, in order to simulate the oil-starved condition, all the prepared coating samples were immersed in lubricating oil for 10 min, and then the samples were taken out and wiped with sanitary napkins to remove the residual oil on the surface, and then the friction and wear test was carried out. The friction and wear parameters were: load 5 N; rate 500 t / min; time 20 min, wear scar length 5 mm, and the grinding ball was a GCr15 steel ball. The friction coefficient was automatically recorded by the friction and wear equipment, and the wear scar width was observed with a metallographic microscope after the friction and wear test.
[0094] As can be seen from the accompanying drawings, the nickel-tungsten coating with a porous structure can be obtained by electroplating using the conditions of the present invention. The prepared coating can effectively reduce the friction coefficient under oil-deficient conditions and reduce the width of the wear scar, thereby achieving the effect of reducing friction and wear. Comparing the width of the wear scar under different electroplating parameters, the wear scar of the coating becomes wider as the current density increases. Compared with Example 9, increasing the content of sodium tungstate, reducing the content of nickel sulfate, and increasing or decreasing the content of ammonium chloride narrows the wear scar width; increasing the content of nickel sulfate and sodium citrate widens the wear scar width. The friction coefficients of the various embodiments are not much different.
[0095] (2) Scanning electron microscopy (SEM) testing of the surface of the prepared coating showed that the surface of the coating presented a porous distribution structure.
[0096] Examples 1, 2 and 9 only change the cathode current density and the electroplating time, and do not change the composition of the plating solution. According to the SEM images, as the current density increases, the number of micropores on the surface of the coating increases and the distribution becomes denser, and the surface structure of the coating becomes looser. According to the SEM images of Examples 3 and 9, increasing the content of sodium tungstate increases the pH of the plating solution, which is conducive to the formation of micropores in the coating. According to Examples 4, 5 and 9, since nickel sulfate and sodium tungstate in the plating solution provide metal ions for the coating and tungsten needs to be co-deposited under the induction of the nickel element, when the nickel sulfate content is low, it is not conducive to the formation and growth of the coating. Among Examples 4, 5 and 9, the coating of Example 4 is the thinnest. According to Examples 8 and 9, sodium citrate is used as a complexing agent, which combines with nickel ions and tungsten ions during the electroplating process to prevent the precipitation of metal ions in the plating solution. Increasing the content of sodium citrate increases the pH of the plating solution, which is conducive to the formation of micropores in the coating. According to Examples 6, 7 and 9, as the ammonium chloride content increases, the pH of the plating solution decreases, and the number of micropores in the coating decreases. A lower pH in an alkaline environment is not conducive to the formation of micropores.
[0097] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A plating solution for a nickel-tungsten porous plating layer, characterized in that: The mass percentages of the components in the plating solution with water as the solvent are as follows: Nickel sulfate 0.47-2.81%, sodium tungstate 1.17-7.04%, sodium citrate 2.62-26.17%, sodium chloride 0.52-0.8%, ammonium chloride 1.43-4.76%.
2. A method for preparing a plating solution for a nickel-tungsten porous plating layer, characterized in that: The specific steps include: Weigh nickel sulfate, sodium tungstate, sodium citrate, sodium chloride and ammonium chloride respectively, dissolve nickel sulfate and sodium chloride in water to obtain a mixed aqueous solution of nickel sulfate and sodium chloride, dissolve sodium tungstate in water to obtain a sodium tungstate aqueous solution, dissolve sodium citrate in water to obtain a sodium citrate aqueous solution, and dissolve ammonium chloride in water to obtain an ammonium chloride aqueous solution; first mix the sodium tungstate aqueous solution and the sodium citrate aqueous solution to obtain a mixed solution, then add the ammonium chloride aqueous solution to the mixed solution, and finally add the nickel sulfate and sodium chloride mixed aqueous solution; add water to adjust the concentration of the plating solution for depositing a nickel-tungsten porous plating layer as claimed in claim 1, and mix evenly to obtain a plating solution.
3. A method for electroplating a nickel-tungsten porous coating, characterized in that: The specific steps of the method are as follows: S1, polish the plated substrate, wash it with water, soak it in a 1 mol / L sodium hydroxide solution at room temperature, take it out, wash it again with water, soak it in a 1 mol / L hydrochloric acid solution at room temperature, take it out, rinse it with deionized water and set it aside; S2, using the plated substrate treated in step S1 as a cathode and a pure platinum plate as an anode, immersing them in the plating solution as described in claim 1 or the plating solution prepared by the method as described in claim 2, and electroplating is performed with mechanical stirring. After the electroplating is completed, immersing the plated substrate in deionized water to recover the plating solution on the surface of the plated substrate, and then rinsing with anhydrous ethanol and drying to obtain a nickel-tungsten porous coating.
4. The electroplating method of nickel-tungsten porous plating layer according to claim 3, characterized in that: The immersion time at room temperature was 3 min using sodium hydroxide, and 15 s using hydrochloric acid.
5. The electroplating method of nickel-tungsten porous plating layer according to claim 3, characterized in that: The drying temperature is 25-50°C, the drying time is 2-10 min, and the mechanical stirring rate is 200-250 rpm.
6. The electroplating method of nickel-tungsten porous plating layer according to claim 3, characterized in that: The electroplating adopts constant current and direct current continuous electroplating.
7. The electroplating method of nickel-tungsten porous plating layer according to claim 6, characterized in that: The current density of the cathode is 6-100 A / dm 2 The electroplating temperature is 40-60 ℃ and the DC continuous electroplating time is 5-600 min.