Treatment method and application of aluminum alloy anode oxide film hole sealing
Through the coordinated method of water sealing treatment and dry heat treatment, the problem of low sealing degree of aluminum alloy anodized film is solved, significantly improved the sealing quality, achieved a low-cost and efficient sealing effect, and avoided additional sealing of holes Enhancement needs.
Patent Information
- Application Number
- CN202411177388.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the pore sealing degree of aluminum anodized film is poor, resulting in the need to add a pore sealing enhancer to improve quality, but this increases the cost and wastewater treatment burden, and lacks a low-cost and efficient treatment method.
The coordinated method of water sealing treatment and dry heat treatment is adopted to reduce the admission value of the anodic oxide film by combining pretreatment, water sealing and dry heat treatment, significantly improve the sealing quality without the need for additional sealing enhancer.
It realizes efficient sealing of aluminum alloy anodized film, reduces the admission value, is simple in process, easy to control, low cost, and has good development potential.
Smart Images

Figure BDA0005011078580000131 
Figure BDA0005011078580000141
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy anodizing post-treatment, and in particular relates to a processing method and application of aluminum alloy anodizing film sealing. Background Art
[0002] In order to improve the corrosion resistance of aluminum anodized film, it should be sealed, so it is necessary to evaluate the sealing quality of aluminum anodized film. The admittance method is a method for detecting the sealing quality. In the prior art, the sealing degree of the product is mainly improved by adding a sealing enhancer. In addition, deionized water and boiling water are often used for sealing in the prior art, but the sealing degree of boiling water sealing is poor. Therefore, a sealing enhancer is generally added to the deionized water sealing tank liquid. However, after adding the sealing enhancer, the tank liquid needs to be controlled, and the cost of wastewater treatment needs to be increased, which is not conducive to reducing costs and increasing efficiency.
[0003] Therefore, it is urgent to design a low-cost, high-efficiency aluminum alloy anodized film sealing treatment method to reduce the admittance value of the anodized film and significantly improve the sealing quality. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a treatment method and application of aluminum alloy anodized film sealing. The present invention utilizes the synergistic cooperation of water sealing treatment and dry heat treatment, and can reduce the admittance value of the anodized film without adding an additional sealing enhancer, thereby significantly improving the sealing quality of the aluminum alloy anodized film. In addition, the treatment method is simple in process, easy to control, highly efficient and low in cost, and has good development potential.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a method for sealing an anodic oxide film of an aluminum alloy, the method comprising the following steps:
[0007] (1) pre-treating the aluminum alloy and then oxidizing it to form an anodic oxide film;
[0008] (2) placing the aluminum alloy with an anodic oxide film in water for water sealing treatment and then cooling;
[0009] (3) The cooled aluminum alloy is subjected to dry heat treatment to achieve heat sealing.
[0010] The present invention utilizes the synergistic combination of water sealing treatment and dry heat treatment, and can reduce the admittance value of the anodized film without the need to add additional sealing enhancers, thereby significantly improving the sealing quality of the aluminum alloy anodized film. In addition, the treatment method is simple in process, easy to control, highly efficient and low in cost, and has good development potential.
[0011] It should be noted that the present invention does not limit the type of aluminum alloy. For example, it can be 6 series aluminum alloy, etc. 6 series aluminum alloy is an aluminum alloy with magnesium and silicon as main alloying elements and Mg2Si phase as strengthening phase, which belongs to heat treatment strengthenable aluminum alloy, and has the advantages of medium strength, high corrosion resistance, no tendency of stress corrosion cracking, good welding performance, unchanged corrosion performance of welding area, good formability and process performance, etc. The most widely used 6 series aluminum alloys are 6061 and 6063 alloys, which have excellent comprehensive performance.
[0012] As a preferred technical solution of the present invention, the pretreatment step in step (1) comprises:
[0013] The aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing.
[0014] Preferably, the pickling step comprises:
[0015] The aluminum alloy is immersed in an acid solution with a temperature of 5-25°C (for example, 5°C, 10°C, 15°C, 20°C or 25°C, etc.) and a concentration of 5-40% (for example, 5%, 10%, 15%, 20%, 25%, 30%, 35% or 40%, etc.) for 2-20 min (for example, 2 min, 5 min, 10 min, 15 min or 20 min, etc.).
[0016] Preferably, the acid solution comprises a nitric acid solution.
[0017] Preferably, the alkali washing step comprises:
[0018] The aluminum alloy after one water washing is placed in an alkaline solution with a temperature of 5-25°C (for example, 5°C, 10°C, 15°C, 20°C or 25°C, etc.) and a concentration of 2-15% (for example, 2%, 5%, 7%, 10%, 12% or 15%, etc.) and soaked for 2-5 minutes (for example, 2 minutes, 3 minutes, 4 minutes or 5 minutes, etc.).
[0019] Preferably, the alkaline solution comprises sodium hydroxide solution.
[0020] Preferably, the step of emitting light comprises:
[0021] The aluminum alloy after the secondary water washing is placed in an acid solution with a temperature of 5-25°C (for example, 5°C, 10°C, 15°C, 20°C or 25°C, etc.) and a concentration of 5-40% (for example, 5%, 10%, 15%, 20%, 25%, 30%, 35% or 40%, etc.) and immersed for 2-20 min (for example, 2 min, 5 min, 10 min, 15 min or 20 min, etc.).
[0022] Preferably, in the light extraction process, the acid solution includes a nitric acid solution.
[0023] As a preferred technical solution of the present invention, the oxidation step in step (1) comprises:
[0024] The pretreated aluminum alloy is placed in an oxidant solution for oxidation.
[0025] Preferably, the concentration of the oxidant solution is 100-200 g / L, for example, it can be 100 g / L, 120 g / L, 140 g / L, 160 g / L, 180 g / L or 200 g / L.
[0026] Preferably, the oxidant solution comprises a sulfuric acid solution.
[0027] Preferably, the oxidation temperature is 10-20°C, for example, 10°C, 12°C, 14°C, 16°C, 18°C or 20°C, and the oxidation time is 50-80min, for example, 50min, 60min, 70min or 80min.
[0028] Preferably, the thickness of the anodized film in step (1) is 12-18 μm, for example, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm or 18 μm.
[0029] As a preferred technical solution of the present invention, the water in step (2) is hot pure water.
[0030] Preferably, the hot pure water is deionized water.
[0031] Preferably, the temperature of the water in step (2) is 92-100°C, for example, it can be 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C or 100°C.
[0032] As a preferred technical solution of the present invention, the time for the water sealing hole treatment in step (2) is 20-40 minutes, for example, it can be 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes.
[0033] As a preferred technical solution of the present invention, the dry heat treatment device in step (3) is a heating furnace or a drying oven.
[0034] Preferably, the atmosphere of the dry heat treatment in step (3) is an air atmosphere.
[0035] As a preferred technical solution of the present invention, the temperature of the dry heat treatment in step (3) is 100-140°C, for example, it can be 100°C, 110°C, 120°C, 130°C or 140°C.
[0036] In the present invention, the dry heat treatment is carried out at 100-140°C, and the dry heat sealing effect of the anodized film is the best, and the surface of the anodized film will not crack. If the temperature of the heat treatment is too low, the sealing improvement effect is not obvious; if the temperature of the heat treatment is too high, the surface of the anodized film will crack and the sealing effect will deteriorate.
[0037] As a preferred technical solution of the present invention, the time of the dry heat treatment in step (3) is 2-10 min, for example, it can be 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min.
[0038] In the present invention, if the heat treatment time is too short, the sealing improvement effect is not obvious; if the heat treatment time is too long, the anodized film may have a risk of cracking.
[0039] As a preferred technical solution of the present invention, the processing method comprises the following steps:
[0040] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0041] The specific steps of pickling include: soaking in an acid solution with a concentration of 5-40% for 2-20 minutes at a temperature of 5-25°C; the specific steps of alkali washing include: soaking in an alkali solution with a concentration of 2-15% for 2-5 minutes at a temperature of 5-25°C; the specific steps of light emitting include: soaking in an acid solution with a concentration of 5-40% for 2-20 minutes at a temperature of 5-25°C;
[0042] (2) placing the 6 series aluminum alloy pretreated in step (1) in a 100-200 g / L oxidant solution and oxidizing at a temperature of 10-20° C. for 50-80 min to form an anodic oxide film;
[0043] (3) placing the 6 series aluminum alloy with anodized film in deionized water at 92-100° C. for water sealing treatment for 20-40 minutes, and then cooling naturally;
[0044] (4) The 6 series aluminum alloy cooled in step (3) is placed in a heating furnace or drying oven in an air atmosphere, heated to 100-140° C. for dry heat treatment for 2-10 min, and then cooled naturally.
[0045] In a second aspect, the present invention provides an application of the processing method described in the first aspect in the field of sealing technology.
[0046] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] The present invention utilizes the synergistic combination of water sealing treatment and dry heat treatment, and can reduce the admittance value of the anodized film without the need to add additional sealing enhancers, thereby significantly improving the sealing quality of the aluminum alloy anodized film. In addition, the treatment method is simple in process, easy to control, highly efficient and low in cost, and has good development potential. DETAILED DESCRIPTION
[0049] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0050] It should be noted that the room temperature below refers to 25°C.
[0051] Example 1
[0052] This embodiment provides a method for sealing pores of an aluminum alloy anodized film, the method comprising the following steps:
[0053] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0054] The specific steps of pickling include: soaking in a 20% nitric acid solution at a temperature of 15° C. for 10 minutes;
[0055] The specific steps of alkaline washing include: soaking in a sodium hydroxide solution with a concentration of 8% for 3 minutes at a temperature of 15°C;
[0056] The specific steps of emitting light include: soaking in a 20% nitric acid solution at a temperature of 15°C for 10 minutes;
[0057] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 150 g / L sulfuric acid solution, and oxidizing at a temperature of 15° C. for 65 min to form an anodic oxide film;
[0058] (3) The 6 series aluminum alloy with an anodic oxide film was placed in deionized water at 96°C for water sealing for 30 minutes, and then naturally cooled to room temperature;
[0059] (4) The 6 series aluminum alloy cooled in step (3) is placed in a heating furnace in an air atmosphere, heated to 120° C. for 4 minutes of dry heat treatment, and then cooled naturally.
[0060] Example 2
[0061] This embodiment provides a method for sealing pores of an aluminum alloy anodized film, the method comprising the following steps:
[0062] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0063] The specific steps of pickling include: soaking in a 40% nitric acid solution at a temperature of 25° C. for 2 minutes;
[0064] The specific steps of alkaline washing include: soaking in a 15% sodium hydroxide solution at a temperature of 25° C. for 2 minutes;
[0065] The specific steps of emitting light include: soaking in a 40% nitric acid solution at a temperature of 25°C for 2 minutes;
[0066] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 100 g / L sulfuric acid solution, and oxidizing at a temperature of 20° C. for 50 min to form an anodic oxide film;
[0067] (3) The 6 series aluminum alloy with an anodic oxide film was placed in deionized water at 92°C for 40 minutes for water sealing, and then naturally cooled to room temperature;
[0068] (4) The 6 series aluminum alloy cooled in step (3) is placed in a drying oven with air atmosphere, heated to 100° C. for 2 min of dry heat treatment, and then cooled naturally.
[0069] Example 3
[0070] This embodiment provides a method for sealing pores of an aluminum alloy anodized film, the method comprising the following steps:
[0071] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0072] The specific steps of pickling include: soaking in a 5% nitric acid solution at a temperature of 5°C for 20 minutes;
[0073] The specific steps of alkaline washing include: soaking in a 2% sodium hydroxide solution at a temperature of 5° C. for 5 minutes;
[0074] The specific steps of emitting light include: soaking in a 5% nitric acid solution at a temperature of 5°C for 20 minutes;
[0075] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 200 g / L sulfuric acid solution, and oxidizing at a temperature of 10° C. for 80 min to form an anodic oxide film;
[0076] (3) The 6 series aluminum alloy with anodized film was placed in deionized water at 100°C for water sealing for 20 minutes, and then naturally cooled to room temperature;
[0077] (4) The 6 series aluminum alloy cooled in step (3) is placed in a heating furnace in an air atmosphere, heated to 140° C. for 8 min of dry heat treatment, and then cooled naturally.
[0078] Example 4
[0079] The difference between this embodiment and embodiment 1 is that the temperature of the dry heat treatment in step (4) is 100°C.
[0080] The remaining processing methods and parameters were the same as those in Example 1.
[0081] Example 5
[0082] The difference between this embodiment and embodiment 1 is that the temperature of the dry heat treatment in step (4) is 140°C.
[0083] The remaining processing methods and parameters were the same as those in Example 1.
[0084] Example 6
[0085] This embodiment provides a method for sealing pores of an aluminum alloy anodized film, the method comprising the following steps:
[0086] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0087] The specific steps of pickling include: soaking in a 20% nitric acid solution at a temperature of 15° C. for 10 minutes;
[0088] The specific steps of alkaline washing include: soaking in a sodium hydroxide solution with a concentration of 8% for 3 minutes at a temperature of 15°C;
[0089] The specific steps of emitting light include: soaking in a 20% nitric acid solution at a temperature of 15°C for 10 minutes;
[0090] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 150 g / L sulfuric acid solution, and oxidizing at a temperature of 15° C. for 65 min to form an anodic oxide film;
[0091] (3) The 6 series aluminum alloy with an anodic oxide film was placed in deionized water at 96°C for water sealing for 30 minutes, and then naturally cooled to room temperature;
[0092] (4) The 6 series aluminum alloy cooled in step (3) is placed in a heating furnace in an air atmosphere, heated to 80° C. for 4 minutes of dry heat treatment, and then cooled naturally.
[0093] Example 7
[0094] This embodiment provides a method for sealing pores of an aluminum alloy anodized film, the method comprising the following steps:
[0095] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0096] The specific steps of pickling include: soaking in a 20% nitric acid solution at a temperature of 15° C. for 10 minutes;
[0097] The specific steps of alkaline washing include: soaking in a sodium hydroxide solution with a concentration of 8% for 3 minutes at a temperature of 15°C;
[0098] The specific steps of emitting light include: soaking in a 20% nitric acid solution at a temperature of 15°C for 10 minutes;
[0099] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 150 g / L sulfuric acid solution, and oxidizing at a temperature of 15° C. for 65 min to form an anodic oxide film;
[0100] (3) The 6 series aluminum alloy with an anodic oxide film was placed in deionized water at 96°C for water sealing for 30 minutes, and then naturally cooled to room temperature;
[0101] (4) The 6 series aluminum alloy cooled in step (3) is placed in a heating furnace in an air atmosphere, heated to 150° C. for 4 minutes of dry heat treatment, and then cooled naturally.
[0102] Example 8
[0103] This embodiment provides a method for sealing pores of an aluminum alloy anodized film, the method comprising the following steps:
[0104] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0105] The specific steps of pickling include: soaking in a 20% nitric acid solution at a temperature of 15° C. for 10 minutes;
[0106] The specific steps of alkaline washing include: soaking in a sodium hydroxide solution with a concentration of 8% for 3 minutes at a temperature of 15°C;
[0107] The specific steps of emitting light include: soaking in a 20% nitric acid solution at a temperature of 15°C for 10 minutes;
[0108] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 150 g / L sulfuric acid solution, and oxidizing at a temperature of 15° C. for 65 min to form an anodic oxide film;
[0109] (3) The 6 series aluminum alloy with an anodic oxide film was placed in deionized water at 96°C for water sealing for 30 minutes, and then naturally cooled to room temperature;
[0110] (4) The 6 series aluminum alloy cooled in step (3) is placed in a heating furnace in an air atmosphere, heated to 120° C. for dry heat treatment for 1 min, and then cooled naturally.
[0111] Example 9
[0112] This embodiment provides a method for sealing pores of an aluminum alloy anodized film, the method comprising the following steps:
[0113] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0114] The specific steps of pickling include: soaking in a 20% nitric acid solution at a temperature of 15° C. for 10 minutes;
[0115] The specific steps of alkaline washing include: soaking in a sodium hydroxide solution with a concentration of 8% for 3 minutes at a temperature of 15°C;
[0116] The specific steps of emitting light include: soaking in a 20% nitric acid solution at a temperature of 15°C for 10 minutes;
[0117] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 150 g / L sulfuric acid solution, and oxidizing at a temperature of 15° C. for 65 min to form an anodic oxide film;
[0118] (3) The 6 series aluminum alloy with an anodic oxide film was placed in deionized water at 96°C for water sealing for 30 minutes, and then naturally cooled to room temperature;
[0119] (4) The 6 series aluminum alloy cooled in step (3) is placed in a heating furnace with air atmosphere, heated to 120° C. for 20 min of dry heat treatment, and then cooled naturally.
[0120] Comparative Example 1
[0121] This comparative example provides a method for sealing the pores of an aluminum alloy anodized film, and the method comprises the following steps:
[0122] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0123] The specific steps of pickling include: soaking in a 20% nitric acid solution at a temperature of 15° C. for 10 minutes;
[0124] The specific steps of alkaline washing include: soaking in a sodium hydroxide solution with a concentration of 8% for 3 minutes at a temperature of 15°C;
[0125] The specific steps of emitting light include: soaking in a 20% nitric acid solution at a temperature of 15°C for 10 minutes;
[0126] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 150 g / L sulfuric acid solution, and oxidizing at a temperature of 15° C. for 65 min to form an anodic oxide film;
[0127] (3) The 6 series aluminum alloy with anodized film was placed in deionized water at 96°C for water sealing treatment for 30 minutes, and then naturally cooled to room temperature.
[0128] Comparative Example 2
[0129] This comparative example provides a method for sealing the pores of an aluminum alloy anodized film, and the method comprises the following steps:
[0130] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0131] The specific steps of pickling include: soaking in a 20% nitric acid solution at a temperature of 15° C. for 10 minutes;
[0132] The specific steps of alkaline washing include: soaking in a sodium hydroxide solution with a concentration of 8% for 3 minutes at a temperature of 15°C;
[0133] The specific steps of emitting light include: soaking in a 20% nitric acid solution at a temperature of 15°C for 10 minutes;
[0134] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 150 g / L sulfuric acid solution, and oxidizing at a temperature of 15° C. for 65 min to form an anodic oxide film;
[0135] (3) The 6 series aluminum alloy with an anodic oxide film is placed in a heating furnace in an air atmosphere, heated to 120° C. for 4 min of dry heat treatment, and then naturally cooled.
[0136] Comparative Example 3
[0137] This embodiment provides a method for sealing pores of an aluminum alloy anodized film, the method comprising the following steps:
[0138] (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment;
[0139] The specific steps of pickling include: soaking in a 20% nitric acid solution at a temperature of 15° C. for 10 minutes;
[0140] The specific steps of alkaline washing include: soaking in a sodium hydroxide solution with a concentration of 8% for 3 minutes at a temperature of 15°C;
[0141] The specific steps of emitting light include: soaking in a 20% nitric acid solution at a temperature of 15°C for 10 minutes;
[0142] (2) placing the 6 series aluminum alloy pretreated in step (1) in a sulfuric acid tank containing 150 g / L sulfuric acid solution, and oxidizing at a temperature of 15° C. for 65 min to form an anodic oxide film;
[0143] (3) The 6 series aluminum alloy with an anodic oxide film was placed in a sealing solution with a pH value of 4.5±0.5 for sealing at a temperature of 35°C for 10 min, then washed with deionized water and naturally cooled to room temperature;
[0144] The sealing liquid contains 1.5 g / L chromium nitrate, 0.8 g / L fluorozirconic acid, 0.6 g / L trisodium citrate and 0.03 g / L nickel sulfate.
[0145] Performance Testing
[0146] The admittance value of the aluminum alloy anodized film provided in the above embodiments and comparative examples was measured using an admittance meter (Fischer ANOTEST YMP30-S).
[0147] The test results are shown in Table 1.
[0148] Table 1
[0149]
[0150]
[0151] analyze:
[0152] It can be seen from the above table that the present invention utilizes the synergistic combination of water sealing treatment and dry heat treatment, and can reduce the conductance value of the anodized film without the need to add additional sealing enhancers, thereby significantly improving the sealing quality of the aluminum alloy anodized film. In addition, the treatment method is simple in process, easy to control, highly efficient and low in cost, and has good development potential.
[0153] It can be seen from Example 1 and Examples 6-7 that if the temperature of some heat treatments is too low, the sealing improvement effect is not obvious; if the temperature of some heat treatments is too high, the surface of the anodized film will crack and the sealing effect will deteriorate.
[0154] It can be seen from Example 1 and Examples 8-9 that if the heat treatment time is too short, the sealing improvement effect is not obvious; if the heat treatment time is too long, there is a risk of cracking on the surface of the anodized film.
[0155] It can be seen from Example 1 and Comparative Example 1 that if only deionized water at a certain temperature is used for water sealing, the sealing effect is poor.
[0156] It can be seen from Example 1 and Comparative Example 2 that if the pore sealing is achieved by only performing dry heat treatment at a certain temperature, the pore sealing effect is poor.
[0157] It can be seen from Example 1 and Comparative Example 3 that if the existing technology described in Comparative Example 3 is used for sealing, the sealing effect is poor.
[0158] The applicant declares that the present invention illustrates the process of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for sealing pores of anodized aluminum alloy films, characterized in that: The processing method comprises the following steps: (1) pre-treating the aluminum alloy and then oxidizing it to form an anodic oxide film; (2) placing the aluminum alloy with an anodic oxide film in water for water sealing treatment and then cooling; (3) The cooled aluminum alloy is subjected to dry heat treatment to achieve heat sealing.
2. The processing method according to claim 1, characterized in that: The pretreatment step in step (1) comprises: The aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing.
3. The processing method according to claim 1 or 2, characterized in that: The oxidation step in step (1) comprises: placing the pretreated aluminum alloy in an oxidant solution for oxidation; Preferably, the concentration of the oxidant solution is 100-200 g / L; Preferably, the oxidation temperature is 10-20° C., and the oxidation time is 50-80 min.
4. The processing method according to any one of claims 1 to 3, characterized in that: The water in step (2) is hot pure water; Preferably, the hot pure water is deionized water; Preferably, the temperature of the water in step (2) is 92-100°C.
5. The processing method according to any one of claims 1 to 4, characterized in that: The time for the water sealing hole treatment in step (2) is 20-40 minutes.
6. The processing method according to any one of claims 1 to 5, characterized in that: The dry heat treatment device in step (3) is a heating furnace or a drying oven; Preferably, the atmosphere of the dry heat treatment in step (3) is an air atmosphere.
7. The processing method according to any one of claims 1 to 6, characterized in that: The temperature of the dry heat treatment in step (3) is 100-140°C.
8. The processing method according to any one of claims 1 to 7, characterized in that: The dry heat treatment time in step (3) is 2-10 minutes.
9. The processing method according to any one of claims 1 to 8, characterized in that: The processing method comprises the following steps: (1) The polished 6 series aluminum alloy is sequentially subjected to pickling, primary water washing, alkali washing, secondary water washing, polishing and tertiary water washing to complete pretreatment; The specific steps of pickling include: soaking in an acid solution with a concentration of 5-40% for 2-20 minutes at a temperature of 5-25°C; the specific steps of alkali washing include: soaking in an alkali solution with a concentration of 2-15% for 2-5 minutes at a temperature of 5-25°C; the specific steps of light emitting include: soaking in an acid solution with a concentration of 5-40% for 2-20 minutes at a temperature of 5-25°C; (2) placing the 6 series aluminum alloy pretreated in step (1) in a 100-200 g / L oxidant solution and oxidizing at a temperature of 10-20° C. for 50-80 min to form an anodic oxide film; (3) placing the 6 series aluminum alloy with anodized film in deionized water at 92-100° C. for water sealing treatment for 20-40 minutes, and then cooling naturally; (4) The 6 series aluminum alloy cooled in step (3) is placed in a heating furnace or drying oven in an air atmosphere, heated to 100-140° C. for dry heat treatment for 2-10 min, and then cooled naturally.
10. Application of the treatment method according to any one of claims 1 to 9 in the field of sealing technology.
Citation Information
Cited By
Selective exchange film closed concentrated solution based on layered double hydroxides as well as preparation method and application of selective exchange film closed concentrated solution