Preparation method of nitrogen and phosphorus co-doped carbon nanofibers, and product and application of nitrogen and phosphorus co-doped carbon nanofibers

Through the preparation method of nitrogen and phosphorus co-doped carbon nanofibers, the problem of insufficient air electrode reactive activity in zinc-air batteries is solved, and the power density and cycling stability of zinc-air batteries are significantly improved. It is suitable for high-performance zinc-air batteries and flexibility Application of zinc-empty batteries.

CN118932550APending Publication Date: 2024-11-12ZHEJIANG NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078401.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The oxygen reduction reaction and oxygen evolution reaction of the air electrode in zinc-empty batteries are slow, resulting in high overpotential, limiting the practical application of zinc-empty batteries. The dual-functional activity of the existing prepared integrated electrode needs to be further optimized to meet high performance. need.

Method used

A preparation method of nitrogen and phosphorus co-doped carbon nanofibers is adopted to form supramolecular polymer nanosheets through melamine and phytic acid as raw materials. Then polyacrylonitrile and inorganic salt cobalt nitrate are added to the solvent, and aged at room temperature to form Co- ZIF nanofibers were calcined at high temperature to obtain nitrogen-phosphorus co-doped carbon nanofibers supported by Co/Co2P nanoparticles, which were used to enhance oxygen electrocatalytic activity.

Benefits of technology

It significantly improves the power density and cycle stability of zinc-empty batteries, achieves high energy conversion efficiency and long cycle life, and is suitable for practical applications of flexible zinc-empty batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932550A_ABST
    Figure CN118932550A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of nitrogen and phosphorus co-doped carbon nanofibers, which comprises the following steps: stirring melamine and phytic acid as reaction raw materials in a solvent to form a melamine phytic acid supramolecular polymer MPSA nanosheet; mPSA nanosheets and polyacrylonitrile are dispersed in a solvent, and MPSA-coated PAN nanofibers are obtained through electrostatic spinning; the preparation method comprises the following steps: by taking the MPSA-PAN nanofiber as a template, adding 2-methylimidazole and inorganic salt cobalt nitrate into a solvent, and aging at room temperature to form MPSA-PAN-Co-ZIF nanofiber; the MPSA (at) PAN (at) Co-ZIF nanofiber is subjected to high-temperature calcination, and the Co / Co2P nanoparticle loaded nitrogen and phosphorus co-doped carbon nanofiber Co / Co2P (at) PNCF is obtained. The invention also discloses the nitrogen-phosphorus co-doped carbon nanofiber obtained by the preparation method and application of the nitrogen-phosphorus co-doped carbon nanofiber in a zinc-air battery. The nitrogen-phosphorus co-doped carbon nanofiber prepared by the invention has excellent bifunctional activity, and the assembled zinc-air battery has remarkable power density and good cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of zinc-air batteries, and particularly relates to a preparation method of nitrogen-phosphorus co-doped carbon nanofibers and a product and application thereof. Background Art

[0002] Zinc-air batteries have abundant natural reserves and high theoretical specific energy density (1086Wh kg -1 ), environmental friendliness and excellent safety, it is regarded as a highly promising renewable energy device. Among them, the air electrode plays a vital role. As an energy converter, it determines the power density and cycle stability of the zinc-air battery. However, the oxygen reduction reaction (ORR) and oxygen evolution reaction (OER) occurring on the air electrode involve complex four-electron processes with slow kinetics, resulting in a high overpotential during the reaction, which greatly limits the practical application of zinc-air batteries. As the core component of the air electrode, the bifunctional activity of the oxygen electrocatalyst and the precise design of the nanostructure are the key to improving the performance of zinc-air batteries.

[0003] With the rapid development of flexible and wearable electronic devices, the market demand for flexible energy storage devices with high energy density and light weight is growing. This requires zinc-air batteries to consider the overall structure of the electrode, the electron transfer between the catalyst and the substrate, and the material transfer between the electrolyte and oxygen molecules. "Adv. Mater." (2024, Vol. 36, p. 2307395) reported an integrated material FeNi2P synthesized using a low-temperature phosphating reduction strategy. v, the material exhibited excellent electrochemical properties. "J.Mater.Chem.A" (2021, Vol. 9, p. 11151) reported that the NCNT@Co-CoP nanowire integrated material constructed on a 3D nickel foam skeleton by in situ catalytic growth and in situ phosphating exhibited excellent electrocatalytic performance. The construction of an integrated air electrode effectively avoids the use of a binder, allowing the active material to be in close contact with the current collector, thereby solving common problems in the traditional air electrode assembly process and opening up a new way to improve the performance of zinc-air batteries. However, the bifunctional activity of the currently prepared integrated electrode still needs to be further optimized to meet the needs of high-performance zinc-air batteries. "Chem. Commun." (2016, Vol. 52, p. 2118) reported that the synergistic effect between N and P can enhance the microstructure of nitrogen-phosphorus co-doped porous carbon, giving it excellent electrocatalytic activity. Adv. Mater. (2020, Vol. 32, p. 2002292) reported that FeP / Fe2O3 nanoparticles were anchored on nitrogen-phosphorus co-doped carbon gels to achieve excellent bifunctional activity. Therefore, nitrogen-phosphorus co-doped carbon nanofibers were synthesized by a simple and effective method and applied to zinc-air batteries to achieve their high power density and long cycle stability, laying a solid foundation for the practical application of flexible solid-state batteries. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing nitrogen-phosphorus co-doped carbon nanofibers. The prepared nitrogen-phosphorus co-doped carbon nanofibers have excellent bifunctional activity, and the assembled zinc-air battery has significant power density and good cycle stability.

[0005] A method for preparing nitrogen and phosphorus co-doped carbon nanofibers, the preparation method comprising:

[0006] (1) Melamine and phytic acid are used as reaction raw materials, and after stirring in a solvent, melamine phytic acid supramolecular polymer MPSA nanosheets are formed;

[0007] (2) Dispersing MPSA nanosheets and polyacrylonitrile in a solvent, and obtaining MPSA@PAN nanofibers by electrospinning;

[0008] (3) Using MPSA@PAN nanofibers as templates, 2-methylimidazole and inorganic salt cobalt nitrate were added to the solvent and aged at room temperature to form MPSA@PAN@Co-ZIF nanofibers;

[0009] (4) MPSA@PAN@Co-ZIF nanofibers were calcined at high temperature to obtain Co / Co2P nanoparticle-loaded nitrogen and phosphorus co-doped carbon nanofibers Co / Co2P@PNCF.

[0010] In step (1), the solvent is water or ethanol. Preferably, the solvent is water.

[0011] Preferably, in step (1), 0.5-3 g of phytic acid is added to a 1-3 g / L melamine aqueous solution and stirred to form MPSA nanosheets.

[0012] Preferably, in step (1), 0.5-1.5 g of phytic acid is added to a 2.5 g / L melamine aqueous solution.

[0013] In the present invention, the Co / Co2P heterostructure in the nitrogen-phosphorus co-doped carbon nanofiber Co / Co2P@PNCF can accelerate electron transport and improve oxygen electrocatalytic activity. Phytic acid is the main source of phosphorus. If too much phytic acid is introduced, the content of Co2P formed will be too high. On the contrary, if too little phytic acid is introduced, the content of Co2P will be too low, and Co will dominate. Therefore, the present invention limits the above-mentioned feed amount to make it more conducive to the oxygen electrocatalytic activity of the product.

[0014] In step (2), the solvent is N,N-dimethylformamide (DMF) or N,N-dimethylacetamide (DMAC). Preferably, the solvent is DMF.

[0015] Preferably, in step (2), 0.3-0.5 g of polyacrylonitrile (PAN) and 50-300 mg of MPSA nanosheets are dispersed in 5-10 mL of N,N-dimethylformamide solvent and stirred to form a uniform solution. The uniform solution is loaded into a 5-10 mL syringe and electrospun using a 20-22 gauge needle and a high voltage of 11-17 kV to obtain MPSA@PAN nanofibers.

[0016] In step (3), the solvent may be an alcohol solvent, including methanol, ethanol, n-pentanol, isopropanol, ethylene glycol, etc., or a water solvent. Different solvents may give different morphologies and sizes of the products. Preferably, anhydrous methanol is used as the solvent.

[0017] Preferably, in step (3), 1-2 g 2-methylimidazole and 0.3-0.9 g cobalt nitrate are respectively dissolved in anhydrous methanol, 100-400 mg MPSA@PAN nanofibers are added, and the nanofibers are completely immersed and aged for 2-6 hours to form MPSA@PAN@Co-ZIF nanofibers.

[0018] The nanoparticle loading amount and particle size can be regulated by adjusting the amount of cobalt nitrate added as a raw material. The particle size can be controlled to be 20 to 100 nm by adjusting the mass range of cobalt nitrate to 0.3 to 0.9 g.

[0019] Preferably, in step (4), 100-300 mg of MPSA@PAN@Co-ZIF nanofibers are calcined at 700-1000°C for 1-3 hours to obtain Co / Co2P nanoparticle-loaded nitrogen and phosphorus co-doped carbon nanofibers Co / Co2P@PNCF.

[0020] Phytic acid decomposes into polyphosphate and H3PO4 at high temperature, promoting the formation of Co2P nanoparticles. If the calcination temperature is too low, phytic acid cannot be fully decomposed. On the contrary, if the calcination temperature is too high, the prepared nitrogen-phosphorus co-doped carbon nanofibers are too brittle, which is not conducive to the assembly and performance of flexible zinc-air batteries. In addition, the pyrolysis temperature has an impact on the electrochemical performance. Too high or too low a temperature is not conducive to the bifunctional activity of the product.

[0021] Preferably, in step (1), 0.5-1 g of phytic acid is added to a 2.5 g / L melamine aqueous solution, and stirred to form MPSA nanosheets; in step (4), the nanosheets are calcined at a high temperature of 800-1000° C. The nitrogen-phosphorus co-doped carbon nanofibers prepared under the above process conditions are applied to zinc-air batteries and have better power density and cycle stability.

[0022] The present invention also provides a nitrogen-phosphorus co-doped carbon nanofiber obtained by the above preparation method.

[0023] The nitrogen-phosphorus co-doped carbon nanofibers are nitrogen-phosphorus co-doped carbon nanofibers loaded with Co / Co2P nanoparticles, the particle size of the Co / Co2P nanoparticles is 20-100nm, and the diameter of the nitrogen-phosphorus co-doped carbon nanofibers is 0.5-1.5μm.

[0024] The present invention can adjust the diameter of nitrogen-phosphorus co-doped carbon nanofibers by adjusting the electrospinning process conditions in step (2) of the preparation method, the addition amounts of the raw materials 2-methylimidazole and cobalt nitrate in step (3), and the immersion aging time and other conditions.

[0025] The present invention also provides an application of the nitrogen-phosphorus co-doped carbon nanofiber in a zinc-air battery.

[0026] Preferably, the nitrogen and phosphorus co-doped carbon nanofibers are used in flexible zinc-air batteries.

[0027] Compared with the prior art, the present invention has the following excellent effects:

[0028] The preparation method of nitrogen-phosphorus co-doped carbon nanofibers provided by the present invention has the advantages of high repeatability, simple synthesis process, and easy control. The nitrogen-phosphorus co-doped carbon nanofibers prepared by the present invention have uniform morphology. The precursor MPSA nanosheets serve as a self-sacrificial template to provide N and P sources while catalyzing the generation of CNTs, thereby increasing the conductivity of the material and making the material have excellent bifunctional activity. The nitrogen-phosphorus co-doped carbon nanofibers provided by the present invention are applied to zinc-air batteries, and the power density is as high as 321mW cm -2 , has remarkable energy conversion efficiency and cycle stability. When used as an integrated air electrode to assemble a flexible zinc-air battery, the power density reaches 161mWcm -2 , the cycle stability is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the XRD spectrum of the nitrogen and phosphorus co-doped carbon nanofibers prepared in Example 1 measured by a D8 X-ray diffractometer from Bruker Corporation, USA, wherein: the abscissa X is the diffraction angle (2θ), and the ordinate Y is the relative diffraction intensity.

[0030] Figure 2 This is a morphology of the nitrogen and phosphorus co-doped carbon nanofibers prepared in Example 1 observed using a Hitachi S-4800 field emission scanning electron microscope (FE-SEM).

[0031] Figure 3 This is a TEM image of the nitrogen and phosphorus co-doped carbon nanofibers prepared in Example 1 measured by a JEM-2100F field emission transmission electron microscope produced by JEOL Corporation of Japan.

[0032] Figure 4 The charge and discharge performance test results of the zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in Example 1 are shown.

[0033] Figure 5 The graph shows the cycle performance test results of the zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in Example 1.

[0034] Figure 6 The specific capacity test results of the zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in Example 1 are shown.

[0035] Figure 7 The charge and discharge performance test results of the flexible zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in Example 1 are shown.

[0036] Figure 8 The graph shows the cycle performance test results of the flexible zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in Example 1. DETAILED DESCRIPTION

[0037] The preparation method and application of the nitrogen-phosphorus co-doped carbon nanofibers of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above content of the present invention belong to the scope of the present invention.

[0038] Example 1

[0039] The preparation method of nitrogen and phosphorus co-doped carbon nanofibers provided in this embodiment comprises the following steps:

[0040] (1) Preparation of MPSA nanosheets: 1 g of phytic acid was added to a 2.5 g / L melamine aqueous solution, and a white precipitate was formed after stirring. The resulting white precipitate was collected by filtration, washed with deionized water, and dried at 80°C.

[0041] (2) Preparation of MPSA@PAN nanofibers: 0.5 g of polyacrylonitrile (PAN) and 50 mg of MPSA nanosheets obtained in step (1) were dispersed in 5 mL of N,N-dimethylformamide (DMF) solvent and stirred for 12 h to form a uniform solution. The mixture solution was loaded into a 5 mL syringe and electrospun using a 20-gauge needle, 13 kV high voltage, a spray speed of 0.05 mm / min, and a spray distance of 15 cm.

[0042] (3) Preparation of MPSA@PAN@Co-ZIF nanofibers: 1.32 g 2-methylimidazole (2-MIM) and 0.582 g cobalt nitrate (Co(NO3)2·6H2O) were dissolved in 40 mL anhydrous methanol, respectively, and mixed after ultrasonic homogenization. The mixture was stirred magnetically for 1 min, and 300 mg MPSA@PAN nanofibers obtained in step (2) were added. The nanofibers were completely immersed and aged for 4 h. The MPSA@PAN nanofibers wrapped with Co-ZIF were taken out, rinsed with anhydrous ethanol several times, and dried in a vacuum oven at 80°C.

[0043] (4) Preparation of Co / Co2P@PNCF nanofibers: 200 mg of MPSA@PAN@Co-ZIF nanofibers were placed in a tubular furnace and calcined at 900 °C for 2 h (heating rate of 5 °C / min).

[0044] The XRD test results in this embodiment show that: Figure 1 As shown, the abscissa X is the diffraction angle (2θ), the ordinate Y is the relative diffraction intensity, and the diffraction peaks correspond to elemental cobalt and cobalt phosphide.

[0045] The nitrogen and phosphorus co-doped carbon nanofibers prepared in this example were analyzed by field emission scanning electron microscopy (SEM), and the obtained electron microscope photographs are as follows: Figure 2As shown, it can be seen that the surface of the nanofibers is uniformly loaded with nanoparticles and carbon nanotubes are generated. The nitrogen and phosphorus co-doped carbon nanofibers prepared in this embodiment have uniform morphology and a diameter range of about 1 μm.

[0046] The nitrogen and phosphorus co-doped carbon nanofibers prepared in this example were analyzed by field emission transmission electron microscopy (TEM), and the obtained electron microscopy photographs are as follows: Figure 3 As shown, it can be observed that the particle size of Co / Co2P nanoparticles is about 50 nm.

[0047] Take the nitrogen and phosphorus co-doped carbon nanofibers prepared in this example, grind them into powder, add deionized water, ethanol, and naphthol solution in sequence, and then ultrasonically mix for 20 to 40 minutes to obtain catalyst ink, and drop the catalyst ink into the middle of the hydrophobic carbon paper with a wetting area of ​​1 square centimeter. Dry at 60°C to obtain an air cathode electrode.

[0048] The air cathode electrode and the zinc sheet anode electrode are fixed in the plexiglass mold respectively, and the air cathode electrode and the zinc sheet anode electrode are separated by a rubber ring. An electrolyte solution made of 6 mol / L potassium hydroxide and 0.2 mol / L zinc acetate is injected into the plexiglass mold to obtain a zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers.

[0049] The prepared zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers was tested for charge and discharge performance. The air electrode was used as the positive electrode and the zinc sheet was used as the negative electrode. The zinc-air battery discharge test was first performed to obtain the discharge curve, and then the charge test was performed. The results are as follows: Figure 4 As shown, its charging and discharging functions are normal, and the maximum power density reaches 321mW / cm 2 , indicating that the zinc-air battery assembled with nitrogen-phosphorus co-doped carbon nanofibers prepared by the method of the present invention has a higher energy conversion efficiency.

[0050] The cycle performance of the prepared zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers was tested, and the assembled zinc-air battery was subjected to cyclic charge and discharge. The results are as follows Figure 5 As shown, the battery performance remains stable after 700 hours of continuous operation, indicating that the zinc-air battery assembled with nitrogen-phosphorus co-doped carbon nanofibers prepared by the method of the present invention has good battery cycle stability.

[0051] The specific capacity of the prepared zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers was tested. The air electrode was the positive electrode and the zinc sheet was the negative electrode. The constant current discharge test was performed until the voltage was less than 0V. The results are as follows: Figure 6 As shown, at a current density of 20 mA / cm 2 Under constant current discharge conditions, the battery specific capacity is 801mAh / g.

[0052] The prepared nitrogen-phosphorus co-doped carbon nanofibers are directly used as the air cathode electrode, the zinc sheet is used as the anode electrode, and the electrolyte gel is made of 6 mol / L potassium hydroxide and 0.2 mol / L zinc acetate to obtain a flexible zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers.

[0053] The prepared flexible zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers was tested for charge and discharge performance. The air electrode was used as the positive electrode and the zinc sheet was used as the negative electrode. The zinc-air battery discharge test was first performed to obtain the discharge curve, and then the charge test was performed. The results are as follows: Figure 7 Its charge and discharge functions are normal, and the maximum power density reaches 161mW / cm 2 , indicating that the flexible zinc-air battery assembled with nitrogen-phosphorus co-doped carbon nanofibers prepared by the method of the present invention has a higher energy conversion efficiency.

[0054] The cycle performance of the prepared flexible zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers was tested, and the assembled zinc-air battery was subjected to cyclic charge and discharge. The results are as follows Figure 8 As shown, the battery performance remains stable after working continuously for 20 hours, indicating that the flexible zinc-air battery assembled with nitrogen-phosphorus co-doped carbon nanofibers prepared by the method of the present invention has good battery cycle stability.

[0055] Example 2

[0056] The preparation method of nitrogen and phosphorus co-doped carbon nanofibers provided in this embodiment comprises the following steps:

[0057] (1) Preparation of MPSA nanosheets: 0.5 g of phytic acid was added to a 2.5 g / L melamine aqueous solution, and a white precipitate was formed after stirring. The resulting white precipitate was collected by filtration, washed with deionized water, and dried at 80°C.

[0058] (2) Preparation of MPSA@PAN nanofibers: 0.5 g of polyacrylonitrile (PAN) and 50 mg of MPSA nanosheets obtained in step (1) were dispersed in 5 mL of N,N-dimethylformamide (DMF) solvent and stirred for 12 h to form a uniform solution. The mixture solution was loaded into a 5 mL syringe and electrospun using a 20-gauge needle, 13 kV high voltage, a spray speed of 0.05 mm / min, and a spray distance of 15 cm.

[0059] (3) Preparation of MPSA@PAN@Co-ZIF nanofibers: 1.32 g 2-methylimidazole (2-MIM) and 0.582 g cobalt nitrate (Co(NO3)2·6H2O) were dissolved in 40 mL anhydrous methanol, respectively, and mixed after ultrasonic homogenization. The mixture was stirred magnetically for 1 min, and 300 mg MPSA@PAN nanofibers obtained in step (2) were added. The nanofibers were completely immersed and aged for 4 h. The MPSA@PAN nanofibers wrapped with Co-ZIF were taken out, rinsed with anhydrous ethanol several times, and dried in a vacuum oven at 80°C.

[0060] (4) Preparation of Co / Co2P@PNCF nanofibers: 200 mg of MPSA@PAN@Co-ZIF nanofibers were placed in a tubular furnace and calcined at 900 °C for 2 h (heating rate of 5 °C / min).

[0061] The charge and discharge performance of the zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers prepared in this example was tested, and the maximum power density reached 271 mW / cm 2 .

[0062] The cycle performance of the zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers prepared in this example was tested. The battery performance remained stable after working continuously for 600 hours.

[0063] Example 3

[0064] The preparation method of nitrogen and phosphorus co-doped carbon nanofibers provided in this embodiment comprises the following steps:

[0065] (1) Preparation of MPSA nanosheets: 1.5 g of phytic acid was added to a 2.5 g / L melamine aqueous solution, and a white precipitate was formed after stirring. The resulting white precipitate was collected by filtration, washed with deionized water, and dried at 80°C.

[0066] (2) Preparation of MPSA@PAN nanofibers: 0.5 g of polyacrylonitrile (PAN) and 50 mg of MPSA nanosheets obtained in step (1) were dispersed in 5 mL of N,N-dimethylformamide (DMF) solvent and stirred for 12 h to form a uniform solution. The mixture solution was loaded into a 5 mL syringe and electrospun using a 20-gauge needle, 13 kV high voltage, a spray speed of 0.05 mm / min, and a spray distance of 15 cm.

[0067] (3) Preparation of MPSA@PAN@Co-ZIF nanofibers: 1.32 g 2-methylimidazole (2-MIM) and 0.582 g cobalt nitrate (Co(NO3)2·6H2O) were dissolved in 40 mL anhydrous methanol, respectively, and mixed after ultrasonic homogenization. The mixture was stirred magnetically for 1 min, and 300 mg MPSA@PAN nanofibers obtained in step (2) were added. The nanofibers were completely immersed and aged for 4 h. The MPSA@PAN nanofibers wrapped with Co-ZIF were taken out, rinsed with anhydrous ethanol several times, and dried in a vacuum oven at 80°C.

[0068] (4) Preparation of Co / Co2P@PNCF nanofibers: 200 mg of MPSA@PAN@Co-ZIF nanofibers were placed in a tubular furnace and calcined at 900 °C for 2 h (heating rate of 5 °C / min).

[0069] The charge and discharge performance of the zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers prepared in this example was tested, and the maximum power density reached 220 mW / cm 2 .

[0070] The cycle performance of the zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers prepared in this example was tested. The battery performance remained stable after working continuously for 400 hours.

[0071] The performance of the nitrogen-phosphorus co-doped carbon nanofibers prepared in Examples 2-3 was verified, and the results showed that the products all exhibited excellent electrochemical performance. When the mass of phytic acid was 1g, the material had a more excellent bifunctional activity, so that the assembled zinc-air battery had a higher power density and better cycle stability.

[0072] Example 4

[0073] The preparation method of nitrogen and phosphorus co-doped carbon nanofibers provided in this embodiment comprises the following steps:

[0074] (1) Preparation of MPSA nanosheets: 1 g of phytic acid was added to a 2.5 g / L melamine aqueous solution, and a white precipitate was formed after stirring. The resulting white precipitate was collected by filtration, washed with deionized water, and dried at 80°C.

[0075] (2) Preparation of MPSA@PAN nanofibers: 0.5 g of polyacrylonitrile (PAN) and 50 mg of MPSA nanosheets obtained in step (1) were dispersed in 5 mL of N,N-dimethylformamide (DMF) solvent and stirred for 12 h to form a uniform solution. The mixture solution was loaded into a 5 mL syringe and electrospun using a 20-gauge needle, 13 kV high voltage, a spray speed of 0.05 mm / min, and a spray distance of 15 cm.

[0076] (3) Preparation of MPSA@PAN@Co-ZIF nanofibers: 1.32 g 2-methylimidazole (2-MIM) and 0.582 g cobalt nitrate (Co(NO3)2·6H2O) were dissolved in 40 mL anhydrous methanol, respectively, and mixed after ultrasonic homogenization. The mixture was stirred magnetically for 1 min, and 300 mg MPSA@PAN nanofibers obtained in step (2) were added. The nanofibers were completely immersed and aged for 4 h. The MPSA@PAN nanofibers wrapped with Co-ZIF were taken out, rinsed with anhydrous ethanol several times, and dried in a vacuum oven at 80°C.

[0077] (4) Preparation of Co / Co2P@PNCF nanofibers: 200 mg of MPSA@PAN@Co-ZIF nanofibers were placed in a tubular furnace and calcined at 700 °C for 2 h (heating rate of 5 °C / min).

[0078] The charge and discharge performance of the zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers prepared in this example was tested, and the maximum power density reached 224 mW / cm 2 .

[0079] The cycle performance of the zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in this example was tested, and the battery performance remained stable after working continuously for 470 hours.

[0080] Example 5

[0081] The preparation method of nitrogen and phosphorus co-doped carbon nanofibers provided in this embodiment comprises the following steps:

[0082] (1) Preparation of MPSA nanosheets: 1 g of phytic acid was added to a 2.5 g / L melamine aqueous solution, and a white precipitate was formed after stirring. The resulting white precipitate was collected by filtration, washed with deionized water, and dried at 80°C.

[0083] (2) Preparation of MPSA@PAN nanofibers: 0.5 g of polyacrylonitrile (PAN) and 50 mg of MPSA nanosheets obtained in step (1) were dispersed in 5 mL of N,N-dimethylformamide (DMF) solvent and stirred for 12 h to form a uniform solution. The mixture solution was loaded into a 5 mL syringe and electrospun using a 20-gauge needle, 13 kV high voltage, a spray speed of 0.05 mm / min, and a spray distance of 15 cm.

[0084] (3) Preparation of MPSA@PAN@Co-ZIF nanofibers: 1.32 g 2-methylimidazole (2-MIM) and 0.582 g cobalt nitrate (Co(NO3)2·6H2O) were dissolved in 40 mL anhydrous methanol, respectively, and mixed after ultrasonic homogenization. The mixture was stirred magnetically for 1 min, and 300 mg MPSA@PAN nanofibers obtained in step (2) were added. The nanofibers were completely immersed and aged for 4 h. The MPSA@PAN nanofibers wrapped with Co-ZIF were taken out, rinsed with anhydrous ethanol several times, and dried in a vacuum oven at 80°C.

[0085] (4) Preparation of Co / Co2P@PNCF nanofibers: 200 mg of MPSA@PAN@Co-ZIF nanofibers were placed in a tubular furnace and calcined at 800 °C for 2 h (heating rate of 5 °C / min).

[0086] The charge and discharge performance of the zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers prepared in this example was tested, and the maximum power density reached 250mW / cm 2 .

[0087] The cycle performance of the zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in this example was tested, and the battery performance remained stable after working continuously for 530 hours.

[0088] Example 6

[0089] The preparation method of nitrogen and phosphorus co-doped carbon nanofibers provided in this embodiment comprises the following steps:

[0090] (1) Preparation of MPSA nanosheets: 1 g of phytic acid was added to a 2.5 g / L melamine aqueous solution, and a white precipitate was formed after stirring. The resulting white precipitate was collected by filtration, washed with deionized water, and dried at 80°C.

[0091] (2) Preparation of MPSA@PAN nanofibers: 0.5 g of polyacrylonitrile (PAN) and 50 mg of MPSA nanosheets obtained in step (1) were dispersed in 5 mL of N,N-dimethylformamide (DMF) solvent and stirred for 12 h to form a uniform solution. The mixture solution was loaded into a 5 mL syringe and electrospun using a 20-gauge needle, 13 kV high voltage, a spray speed of 0.05 mm / min, and a spray distance of 15 cm.

[0092] (3) Preparation of MPSA@PAN@Co-ZIF nanofibers: 1.32 g 2-methylimidazole (2-MIM) and 0.582 g cobalt nitrate (Co(NO3)2·6H2O) were dissolved in 40 mL anhydrous methanol, respectively, and mixed after ultrasonic homogenization. The mixture was stirred magnetically for 1 min, and 300 mg MPSA@PAN nanofibers obtained in step (2) were added. The nanofibers were completely immersed and aged for 4 h. The MPSA@PAN nanofibers wrapped with Co-ZIF were taken out, rinsed with anhydrous ethanol several times, and dried in a vacuum oven at 80°C.

[0093] (4) Preparation of Co / Co2P@PNCF nanofibers: 200 mg of MPSA@PAN@Co-ZIF nanofibers were placed in a tubular furnace and calcined at 1000 °C for 2 h (heating rate of 5 °C / min).

[0094] The charge and discharge performance of the zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers prepared in this example was tested, and the maximum power density reached 242 mW / cm 2 .

[0095] The cycle performance of the zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in this example was tested. The battery performance remained stable after working continuously for 480 hours.

[0096] The performance of the nitrogen-phosphorus co-doped carbon nanofibers prepared in Examples 4-6 was verified, and the results showed that the products all exhibited excellent electrochemical performance. When the calcination temperature was 900°C, the material had better bifunctional activity, so that the assembled zinc-air battery had higher power density and better cycle stability.

[0097] Example 7

[0098] The preparation method of nitrogen and phosphorus co-doped carbon nanofibers provided in this embodiment comprises the following steps:

[0099] (1) Preparation of MPSA nanosheets: 1 g of phytic acid was added to a 2.5 g / L melamine aqueous solution, and a white precipitate was formed after stirring. The resulting white precipitate was collected by filtration, washed with deionized water, and dried at 80°C.

[0100] (2) Preparation of MPSA@PAN nanofibers: 0.5 g of polyacrylonitrile (PAN) and 50 mg of MPSA nanosheets obtained in step (1) were dispersed in 5 mL of N,N-dimethylformamide (DMF) solvent and stirred for 12 h to form a uniform solution. The mixture solution was loaded into a 5 mL syringe and electrospun using a 20-gauge needle, 13 kV high voltage, a spray speed of 0.05 mm / min, and a spray distance of 15 cm.

[0101] (3) Preparation of MPSA@PAN@Co-ZIF nanofibers: 1.32 g 2-methylimidazole (2-MIM) and 0.873 g cobalt nitrate (Co(NO3)2·6H2O) were dissolved in 40 mL anhydrous methanol, respectively, and mixed after ultrasonic homogenization. The mixture was stirred magnetically for 1 min, and 300 mg MPSA@PAN nanofibers obtained in step (2) were added. The nanofibers were completely immersed and aged for 4 h. The MPSA@PAN nanofibers wrapped with Co-ZIF were taken out, rinsed with anhydrous ethanol several times, and dried in a vacuum oven at 80°C.

[0102] (4) Preparation of Co / Co2P@PNCF nanofibers: 200 mg of MPSA@PAN@Co-ZIF nanofibers were placed in a tubular furnace and calcined at 900 °C for 2 h (heating rate of 5 °C / min).

[0103] Field emission transmission electron microscopy analysis of the nitrogen and phosphorus co-doped carbon nanofibers prepared in this example showed that the particle size of the Co / Co2P nanoparticles was about 100 nm.

[0104] The charge and discharge performance of the zinc-air battery based on nitrogen-phosphorus co-doped carbon nanofibers prepared in this example was tested, and the maximum power density reached 233 mW / cm 2 .

[0105] The cycle performance of the zinc-air battery based on nitrogen and phosphorus co-doped carbon nanofibers prepared in this example was tested. The battery performance remained stable after working continuously for 410 hours.

[0106] After the same experimental verification as Example 1, the results show that the batteries assembled with the materials prepared in Examples 2-7 all exhibit excellent power density and good cycle stability. The above results show that the nitrogen-phosphorus co-doped carbon nanofibers prepared by the method of the present invention are suitable for zinc-air batteries including integrated flexible zinc-air batteries, and have excellent zinc-air battery performance. The present invention has brought significant impetus to the research of high-performance multifunctional carbon materials, provided a new idea for improving the performance of zinc-air batteries, and laid a technical foundation for the further promotion of flexible solid-state batteries in practical applications.

Claims

1. A method for preparing nitrogen-phosphorus co-doped carbon nanofibers, It is characterized in that The preparation method comprises: (1) Melamine and phytic acid are used as reaction raw materials, and melamine phytic acid supramolecular polymer MPSA nanosheets are formed after stirring in a solvent; (2) Dispersing MPSA nanosheets and polyacrylonitrile in a solvent, and obtaining MPSA@PAN nanofibers by electrospinning; (3) Using MPSA@PAN nanofibers as templates, 2-methylimidazole and inorganic salt cobalt nitrate were added to the solvent and aged at room temperature to form MPSA@PAN@Co-ZIF nanofibers; (4) MPSA@PAN@Co-ZIF nanofibers were calcined at high temperature to obtain Co / Co 2 Nitrogen and phosphorus co-doped carbon nanofibers Co / Co supported by P nanoparticles 2 P@PNCF.

2. The method for preparing nitrogen-phosphorus co-doped carbon nanofibers according to claim 1, It is characterized in that In step (1), 0.5-3 g of phytic acid is added to a 1-3 g / L melamine aqueous solution and stirred to form MPSA nanosheets.

3. The method for preparing nitrogen-phosphorus co-doped carbon nanofibers according to claim 1, It is characterized in that In step (2), 0.3-0.5 g of polyacrylonitrile and 50-300 mg of MPSA nanosheets are dispersed in 5-10 mL of N,N-dimethylformamide solvent and stirred to form a uniform solution. The uniform solution is loaded into a 5-10 mL syringe and electrospun using a 20-22 gauge needle and a high voltage of 11-17 kV to obtain MPSA@PAN nanofibers.

4. The method for preparing nitrogen-phosphorus co-doped carbon nanofibers according to claim 1, It is characterized in that In step (3), 1-2 g of 2-methylimidazole and 0.3-0.9 g of cobalt nitrate are dissolved in anhydrous methanol, 100-400 mg of MPSA@PAN nanofibers are added, and the nanofibers are aged for 2-6 hours after being completely immersed to form MPSA@PAN@Co-ZIF nanofibers.

5. The method for preparing nitrogen-phosphorus co-doped carbon nanofibers according to claim 1, It is characterized in that In step (4), 100-300 mg of MPSA@PAN@Co-ZIF nanofibers are calcined at 700-1000°C for 1-3 hours to obtain Co / Co 2 Nitrogen and phosphorus co-doped carbon nanofibers Co / Co supported by P nanoparticles 2 P@PNCF.

6. Nitrogen and phosphorus co-doped carbon nanofibers obtained according to the preparation method according to any one of claims 1 to 5.

7. The nitrogen-phosphorus co-doped carbon nanofiber according to claim 6, It is characterized in that The nitrogen-phosphorus co-doped carbon nanofiber-supported Co / Co 2 The particle size of the P nanoparticles is 20-100 nm, and the diameter of the nitrogen-phosphorus co-doped carbon nanofibers is 0.5-1.5 μm.

8. Use of the nitrogen-phosphorus co-doped carbon nanofibers according to claim 6 in zinc-air batteries.

9. The use according to claim 8, It is characterized in that Application of the nitrogen-phosphorus co-doped carbon nanofibers in flexible zinc-air batteries.