Graphitization furnace, high-strength high-modulus carbon fiber and preparation method of high-strength high-modulus carbon fiber

By designing an induction heating graphitization furnace, using multi-temperature zone design and electromagnetic shielding structure, the graphitization furnace has been solved in the short life and high energy consumption in high temperature environments, and the efficient polyacrylonitrile-based high-strength high-mode carbon fiber is achieved. Continuous preparation meets the needs of the aerospace field.

CN118932554APending Publication Date: 2024-11-12INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411151662.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing graphitization furnace has a short life, high energy consumption and slow heating rate in high temperature environments, and cannot meet the preparation needs of large-scale and continuous polyacrylonitrile-based high-strength high-mode carbon fibers.

Method used

An induction heating graphitization furnace is designed. The furnace cavity includes multiple continuous temperature sections. The induction coil is arranged around the furnace. An electromagnetic shielding structure is set between any adjacent induction coil segments. The furnace can be spliced ​​into a structure to accommodate width. The furnace material and thickness are optimized for improved stability and economy.

Benefits of technology

The life of the graphitization furnace is extended, energy consumption is reduced, and the heating rate is improved, meeting the preparation needs of large-scale and continuous polyacrylonitrile-based high-strength high-mode carbon fibers. The fiber tensile strength and modulus are improved, and the stability is good, suitable for High-end fields such as aerospace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932554A_ABST
    Figure CN118932554A_ABST
Patent Text Reader

Abstract

The invention relates to a graphitization furnace, a high-strength and high-modulus carbon fiber and a preparation method thereof, and relates to the technical field of carbon fibers. Wherein the graphitization furnace is an induction heating type graphitization furnace; the graphitization furnace comprises a hearth and an induction coil; an inner cavity of the hearth comprises a plurality of continuous temperature sections in sequence; the induction coil is arranged around the periphery of the hearth and is used for generating induction current to the hearth so as to heat the hearth; wherein the induction coil comprises a plurality of induction coil sections; wherein the number of the induction coil sections is consistent with that of the temperature zone sections, and each induction coil section is arranged around the corresponding temperature zone section; wherein an electromagnetic shielding structure is arranged between any two adjacent induction coil sections, so that mutual influence between magnetic induction lines of any two adjacent induction coil sections is avoided. The method is mainly used for prolonging the service life of the graphitization furnace, and meanwhile, the graphitization furnace can further meet the large-scale and continuous polyacrylonitrile-based high-strength and high-modulus carbon fiber preparation requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon fiber, in particular to a graphitization furnace, and a high-strength and high-modulus carbon fiber and a preparation method thereof. Background Art

[0002] Polyacrylonitrile-based high-strength and high-modulus carbon fiber refers to carbon fiber with a carbon content of more than 99%. Polyacrylonitrile-based high-strength and high-modulus carbon fiber not only has the characteristics of high specific modulus and high specific strength, but also has excellent properties such as small thermal expansion coefficient, good thermal stability, and dimensional stability. It is widely used in spacecraft, aerospace and other fields.

[0003] Polyacrylonitrile-based high-strength and high-modulus carbon fibers are made by high-temperature graphitization of carbon fibers. The highest tensile modulus of the high-strength and high-modulus carbon fibers currently prepared is far from the theoretical modulus, and there are problems such as difficulty in simultaneously improving tensile strength and tensile modulus performance, excessive fiber fuzz, and poor stability, which cannot meet the needs of high-end fields such as aerospace.

[0004] The preparation of polyacrylonitrile-based high-strength and high-modulus carbon fibers is an integration of high-temperature equipment (i.e., ultra-high temperature graphitization furnace) and high-temperature technology. The continuous graphitization furnace commonly used in the industrial production of polyacrylonitrile-based high-strength and high-modulus carbon fibers is a resistance furnace, whose structure includes a furnace shell, a graphite heating element, a furnace chamber, and thermal insulation materials. However, there are many problems in its use, and it cannot meet the needs of industrial continuous production. The existing resistive graphitization furnace has at least the following technical problems: ① In a high-temperature graphitization environment, the graphite heating element is continuously consumed due to oxidation and sublimation, and can operate stably for 1 year at a temperature of 2650°C. When the graphitization temperature exceeds 2800°C, the loss of the graphite heating element rises sharply, and the life of the heating element is significantly reduced. Its stable operation time is less than 7 days (it should be noted here that the furnace chamber reaches the set temperature by heating the graphite body. When the furnace chamber reaches the set temperature, the temperature of the graphite body is higher than the set temperature, and it is easy to exceed 2800°C). ② The width of the continuous ultra-high temperature graphitization furnace used in the industrial production process is less than 1m, and the width of the continuous graphitization furnace used by most companies is 0.1-0.6m. The main reason is that in the high-temperature graphitization environment, as the width of the furnace mouth increases, the graphite furnace is prone to breakage due to the increase in span. ③ The energy consumption of resistive heating is high and the heating rate is slow.

[0005] In addition, when polyacrylonitrile-based high-strength and high-modulus carbon fibers are prepared in the laboratory, an induction graphitization furnace that generates eddy current heating by induction is used. However, most graphitization furnaces with this type of heat source are intermittent graphitization furnaces or single-tube continuous graphitization furnaces, and one graphitization furnace can only achieve one temperature zone; during the graphitization process, multiple graphitization furnaces need to be connected in series to achieve the multi-temperature zone graphitization process requirements. However, in this way, different temperature zones are not continuous, and there will be cold zones between them (from one graphitization furnace to another graphitization furnace, the interval formed by the cold zone), so it cannot meet the large-scale and continuous preparation requirements of polyacrylonitrile-based high-strength and high-modulus carbon fibers.

[0006] In summary, there is an urgent need for a graphitization furnace with a long service life that can meet the needs of large-scale and continuous preparation of polyacrylonitrile-based high-strength and high-modulus carbon fibers. Summary of the invention

[0007] In view of this, the present invention provides a graphitization furnace, a high-strength and high-modulus carbon fiber and a preparation method thereof, the main purpose of which is to increase the service life of the graphitization furnace, while enabling the graphitization furnace to meet the needs of large-scale and continuous preparation of polyacrylonitrile-based high-strength and high-modulus carbon fibers.

[0008] In order to achieve the above object, the present invention mainly provides the following technical solutions:

[0009] On the one hand, an embodiment of the present invention provides a graphitization furnace, wherein the graphitization furnace is an induction heating graphitization furnace; wherein the graphitization furnace comprises:

[0010] A furnace, wherein the inner cavity of the furnace comprises a plurality of temperature sections arranged in sequence;

[0011] an induction coil, the induction coil being arranged around the outer circumference of the furnace and being used for generating an induced current in the furnace to heat the furnace;

[0012] The induction coil includes a plurality of induction coil segments; wherein the number of the induction coil segments is consistent with the number of the temperature zones, and each of the induction coil segments is arranged around the corresponding temperature zone to heat the corresponding temperature zone;

[0013] Wherein, an electromagnetic shielding structure is arranged between any two adjacent induction coil segments to avoid mutual influence between the magnetic flux lines of any two adjacent temperature zones.

[0014] Preferably, the inner cavity of the furnace has a wire passage so that the fibers to be graphitized can pass through a plurality of temperature sections in sequence and continuously.

[0015] Preferably, the material of the electromagnetic shielding structure is a set material; wherein, under an inert atmosphere, the set material can withstand a temperature of ≥3000°C; and / or the electromagnetic shielding structure is formed by stacking at least two layers of carbon fiber cloth; or the electromagnetic shielding structure is formed by alternately stacking carbon fiber cloth and tungsten mesh in sequence, and further preferably, the outer layers of the electromagnetic shielding structure are all carbon fiber cloth.

[0016] Preferably, the electromagnetic shielding structure is an electromagnetic shielding plate.

[0017] Preferably, the width W of the furnace mouth of the furnace is 0.1-4.0m; when the width W of the furnace mouth is ≤1m, the furnace is an integrated structure; when the width W of the furnace mouth is greater than 1m, the furnace is an integrated structure or a spliced ​​structure.

[0018] Preferably, the furnace is composed of a plurality of furnace sections spliced ​​in sequence; wherein the number of furnace sections is consistent with the number of temperature zones and corresponds one to one; preferably, an electromagnetic shielding structure is provided between any two adjacent furnace sections; and a through hole for allowing the fiber to pass through is provided on the electromagnetic shielding structure.

[0019] Preferably, each of the furnace sections is an integrated structure, and preferably, a cross section of the furnace section forms a flat annular structure.

[0020] Preferably, each of the furnace sections comprises:

[0021] roof;

[0022] A bottom plate, wherein the bottom plate and the top plate are arranged opposite to each other;

[0023] a first arc-shaped side plate, wherein a first side of the first arc-shaped side plate is butted against a first side of the top plate, and a second side of the first arc-shaped side plate is butted against a first side of the bottom plate;

[0024] a second curved side plate, wherein a first side of the second curved side plate is butted against a second side of the top plate, and a second side of the second curved side plate is butted against a second side of the bottom plate;

[0025] Wherein, the first side and the second side are two sides arranged opposite to each other;

[0026] Preferably, the cross section of the furnace section forms a flat annular structure through the top plate, the bottom plate, the first arc-shaped side plate and the second arc-shaped side plate;

[0027] Preferably, the first arc-shaped side plate is a U-shaped plate;

[0028] Preferably, the second arc-shaped side plate is a U-shaped plate;

[0029] Preferably, the first side of the first curved side panel is connected to the first side of the top panel via a first connecting plate, and the second side of the first curved side panel is connected to the first side of the bottom panel via a second connecting plate; the first side of the second curved side panel is connected to the second side of the top panel via a third connecting plate, and the second side of the second curved side panel is connected to the second side of the bottom panel via a fourth connecting plate.

[0030] Preferably, the furnace mouth of the furnace is in the shape of a flat annular mouth; and / or the induction coil segment is wound around the outer circumference of the furnace; preferably, the induction coil segment is in a flat annular structure; and / or the furnace is made of graphite, preferably isostatic graphite.

[0031] Preferably, the thickness K of the furnace and the design temperature T of the highest temperature zone of the graphitization furnace satisfy the following relationship:

[0032] When T<2800℃, K=30-45mm;

[0033] When 2800℃≤T≤3200℃, K=0.2593×e 0.0019×T ;

[0034] The unit of K is mm, and the unit of T is °C.

[0035] Preferably, a heat insulating material is filled between the furnace and the induction coil; preferably, the heat insulating material is high temperature resistant graphite carbon felt; and / or the induction coil is installed on an insulating frame; preferably, the insulating frame is made of refractory clay; preferably, soft magnetic materials are evenly distributed in the insulating frame to play a magnetic role; and / or the graphitization furnace includes a furnace shell; the furnace and the induction coil are both located in the furnace shell; the gap between the furnace shell and the furnace and the induction coil is filled with heat insulating material; and / or the graphitization furnace further includes: a controller and a temperature measuring device; wherein the controller and the temperature measuring device The number is consistent with the number of the temperature sections and corresponds one to one; preferably, the temperature measuring device is used to measure the temperature of the temperature section corresponding to it; the controller is connected to the temperature measuring device and the induction coil section corresponding to it; and / or the inlet and outlet of the graphitization furnace are both provided with removable plugs to prevent heat radiation; and / or the number of the temperature sections is greater than 1 and less than or equal to 9; and / or along the wire feeding direction, an electromagnetic shielding structure is also provided on one side of the first induction coil section close to the inlet of the graphitization furnace; an electromagnetic shielding structure is also provided on one side of the last induction coil section close to the outlet of the graphitization furnace.

[0036] On the other hand, an embodiment of the present invention provides a method for preparing high-strength and high-modulus carbon fiber, which comprises the following steps:

[0037] Graphitization treatment: Graphitization treatment is performed on the fibers after high-temperature carbonization treatment to obtain high-strength and high-modulus carbon fibers;

[0038] Wherein, the fiber after high temperature carbonization treatment is graphitized by using any of the graphitization furnaces described above;

[0039] The polyacrylonitrile precursor is subjected to a pre-oxidation treatment, a low-temperature carbonization treatment, and a high-temperature carbonization treatment in sequence to obtain the fiber subjected to the high-temperature carbonization treatment;

[0040] Preferably, the fiber after high-temperature carbonization has a bulk density of 1.79-1.81 g / cm3, a tensile strength of 6.1-6.4 GPa, and a tensile modulus of 280-300 GPa.

[0041] Preferably, in the step of graphitization treatment: the temperature of the highest temperature zone of the graphitization treatment is 2050-3200°C, preferably 2100-3100°C; and / or the sealing gas in the graphitization furnace is selected from one or more of argon, nitrogen and helium; and / or the carrier gas in the graphitization furnace is selected from one or more of argon, nitrogen and helium; and / or the pressure in the graphitization furnace is 0-500Pa, preferably 30-100Pa; and / or the rotation speed of the roller before the graphitization furnace and the rotation speed of the roller after the graphitization furnace meet the following conditions: 1≤V2 / V1≤1.3, preferably 1.05≤V2 / V1≤1.2; In the figure, V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; and / or the time t of the graphitization treatment satisfies the following conditions: t=L×(V1+V2) / (2×V1×V2); 4D≤t≤20D, preferably 5D≤t≤10D; wherein t represents the time of the graphitization treatment, in s; L represents the length of the furnace, in m; V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; D is the diameter of the fiber after high-temperature carbonization treatment, in μm.

[0042] On the other hand, an embodiment of the present invention provides a high-strength and high-modulus carbon fiber, wherein the high-strength and high-modulus carbon fiber is a polyacrylonitrile-based carbon fiber; wherein the bulk density of the high-strength and high-modulus carbon fiber is 1.92-1.97 g / cm 3 , tensile strength is 3.7-4.2GPa, tensile modulus is 580-700Gpa;

[0043] Preferably, the high-strength and high-modulus carbon fiber is prepared by the above-mentioned method for preparing high-strength and high-modulus carbon fiber; wherein the temperature zones for graphitization treatment include a first temperature zone, a second temperature zone, and a third temperature zone in sequence; wherein the temperature of the first temperature zone is 2450-2800°C, the temperature of the second temperature zone is 2550-3000°C, and the temperature of the third temperature zone is 2750-3150°C.

[0044] On the other hand, an embodiment of the present invention provides a high-strength and high-modulus carbon fiber, wherein the high-strength and high-modulus carbon fiber is a polyacrylonitrile-based carbon fiber; wherein the bulk density of the high-strength and high-modulus carbon fiber is 1.78-1.85 g / cm 3 , tensile strength is 5.0-5.9GPa, tensile modulus is 370-450Gpa;

[0045] Preferably, the high-strength and high-modulus carbon fiber is prepared by the above-mentioned method for preparing high-strength and high-modulus carbon fiber; wherein the temperature zones for graphitization treatment include a first temperature zone, a second temperature zone, and a third temperature zone in sequence; wherein the temperature of the first temperature zone is 1850-2050°C, the temperature of the second temperature zone is 1950-2200°C, and the temperature of the third temperature zone is 2050-2370°C.

[0046] In another aspect, an embodiment of the present invention provides a carbon fiber composite material, wherein the carbon fiber composite material is a resin-based carbon fiber unidirectional composite material; wherein the compressive strength of the carbon fiber composite material is 1500-1950 MPa;

[0047] Wherein, the carbon fiber composite material is prepared from the above-mentioned high modulus and high strength carbon fiber.

[0048] Compared with the prior art, the graphitization furnace, high-strength and high-modulus carbon fiber and preparation method thereof of the present invention have at least the following beneficial effects:

[0049] On the one hand, an embodiment of the present invention provides a graphitization furnace, wherein the graphitization furnace is an induction heating graphitization furnace; the inner cavity of the furnace chamber includes a plurality of temperature sections in sequence, the induction coil includes a plurality of induction coil sections, the number of induction coil sections is consistent with the number of temperature sections, and each induction coil section is arranged around the temperature section corresponding to it to heat the temperature section corresponding to it; wherein an electromagnetic shielding structure is arranged between any two adjacent induction coil sections to avoid mutual influence between the magnetic flux lines of any two adjacent temperature sections. The above design realizes the continuous multi-temperature zone design of the induction heating graphitization furnace (so that the temperatures between the continuous temperature zones do not interfere with each other, and continuous multi-temperature zones are realized), thereby meeting the needs of large-scale and continuous preparation of polyacrylonitrile-based high-strength and high-modulus carbon fibers.

[0050] Furthermore, the embodiment of the present invention provides a graphitization furnace, and the electromagnetic shielding structure is designed as follows: the electromagnetic shielding structure is formed by alternately stacking carbon fiber cloth and tungsten mesh in sequence, and preferably, the outer layers (first layer and last layer) of the electromagnetic shielding structure are both carbon fiber cloth. Through the above arrangement, the electromagnetic shielding structure has an excellent electromagnetic shielding effect, can well isolate the mutual influence of adjacent induction coils, and ensure the stable operation of the equipment.

[0051] Furthermore, in a graphitization furnace provided by an embodiment of the present invention, the furnace mouth (the inlet and outlet of the inner cavity of the furnace, and the cross section of the entire furnace) is set to a flat shape, which is adapted to the fiber filaments to be graphitized, so that the effective space is large, and energy saving is further achieved. The shape of the induction coil segment is set to a flat ring structure, which is more in line with the process requirements and can further reduce energy consumption. In addition, the furnace is designed as a splicing structure to solve the problem that a wide-mouthed ultra-temperature graphitization furnace cannot be made due to material problems.

[0052] Furthermore, in an embodiment of the present invention, a graphitization furnace is provided, wherein the furnace chamber is made of graphite, and the thickness K of the furnace chamber and the maximum design temperature T of the graphitization furnace satisfy the following relationship: when T < 2800°C, K = 30-45 mm; when 2800°C ≤ T ≤ 3200°C, K = 0.2593 × e 0.0019×T ; The unit of K is mm, and the unit of T is °C. Here, the above design purpose is to ensure the service life of the furnace and the structural strength of the furnace under the premise of considering the economic factors such as the furnace manufacturing cost; at the same time, the design of the furnace thickness can achieve a secondary temperature uniformity effect, ensuring that the graphitization furnace has a smaller cross-sectional temperature difference.

[0053] It should be noted that: the embodiment of the present invention provides a graphitization furnace, which optimizes the thickness of the graphite furnace (see the previous paragraph) so that different furnace thicknesses are used for different graphitization temperatures, thereby solving the problem of easy fracture of the wide-mouth furnace from an economic and practical point of view. At the same time, the embodiment of the present invention also solves the fracture problem of the wide-mouth graphitization furnace through the structural design of the graphitization furnace (such as a splicing design) and the coordinated design of the furnace thickness. Although the thicker the graphitization furnace, the less likely it is to break and the longer its life, the present invention fully considers issues such as economy, and coordinates the optimization design of the furnace structure and furnace thickness to ensure economy and practicality.

[0054] On the other hand, the present embodiment provides a high-strength and high-modulus carbon fiber and a preparation method thereof. The graphitization furnace provided in the above embodiment is used to reasonably match the process conditions of the graphitization treatment process, so that the tensile strength and tensile modulus of the fiber are further improved. The tensile strength is 3.7-4.2GPa and the tensile modulus is 580-700Gpa. The carbon fiber has good stability, realizing large-scale and continuous preparation.

[0055] On the other hand, this embodiment provides a high-strength and high-modulus carbon fiber and a preparation method thereof, using the graphitization furnace of the above embodiment, finely matching the process conditions of the graphitization treatment process, achieving both high strength and high modulus of the fiber, and obtaining a new type of high-strength and high-modulus polyacrylonitrile-based carbon fiber, with a tensile strength of 5.0-5.9GPa and a tensile modulus of 370-450GPa, and can achieve large-scale and continuous preparation. The high-strength and high-modulus carbon fiber composite material prepared from the carbon fiber has a high compressive strength, meeting the needs of high-end fields such as aerospace.

[0056] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 is a structural schematic diagram of a graphitization furnace provided by an embodiment of the present invention;

[0058] Figure 2 is a cross-sectional schematic diagram of a graphitization furnace provided by an embodiment of the present invention;

[0059] Figure 3 is a structural schematic diagram of a furnace section provided by an embodiment of the present invention;

[0060] Figure 4 It is a structural schematic diagram of an electromagnetic shielding structure provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0061] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention application are described in detail below in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures, or characteristics in one or more embodiments may be combined in any suitable form.

[0062] Example 1

[0063] On the one hand, this embodiment provides a graphitization furnace, wherein, Figure 1 and Figure 2As shown, the graphitization furnace is an induction heating graphitization furnace; wherein the graphitization furnace includes a furnace 2 and an induction coil 3. wherein the inner cavity of the furnace 2 includes a plurality of temperature sections in sequence; the induction coil 3 is arranged around the outer circumference of the furnace 2, and is used to generate an induced current to the furnace 2 to heat the furnace 2. wherein the induction coil 3 includes a plurality of induction coil segments; wherein the number of the induction coil segments is consistent with the number of the temperature sections, and each induction coil segment is arranged around the temperature section corresponding thereto, to heat the temperature section corresponding thereto; wherein an electromagnetic shielding structure 4 is arranged between any two adjacent induction coil segments, to avoid mutual influence between the magnetic flux lines of any two adjacent temperature sections, so as to make the temperature of each temperature zone independent.

[0064] It should be noted here that: on the one hand, the graphitization furnace provided in this embodiment is an induction heating graphitization furnace, and there is no problem of "short life of graphite heating element" existing in the resistive graphitization furnace. Therefore, compared with the existing resistive graphitization furnace, the graphitization furnace of this embodiment has a long life, low energy consumption, and fast heating rate. On the other hand, the existing induction graphitization furnace that generates eddy current heating by induction has discontinuous temperature zones and cold zones between them. In this way, when the fiber is graphitized, after passing through a temperature zone, it first passes through the cold zone and then enters the next temperature zone. This is not conducive to the graphitization of the fiber and cannot meet the needs of large-scale and continuous preparation of polyacrylonitrile-based high-strength and high-modulus carbon fibers. However, this embodiment realizes the continuous multi-temperature zone design of the induction heating graphitization furnace through the above-mentioned setting, that is, there is no cold zone between the temperature zones, and the temperature is independent, thereby meeting the needs of large-scale and continuous preparation of polyacrylonitrile-based high-strength and high-modulus carbon fibers.

[0065] The inner cavity of the furnace 2 has a wire passage 21, so that the fiber to be graphitized enters the inner cavity of the furnace 2 from the inlet of the graphitization furnace, passes through multiple temperature sections in sequence, and then passes out from the outlet of the graphitization furnace.

[0066] Preferably, the electromagnetic shielding structure is made of a set material; wherein, in an inert atmosphere, the set material can withstand a temperature of ≥3000°C.

[0067] Preferably, the number of temperature zones in this embodiment is greater than 1 and less than or equal to 9.

[0068] Example 2

[0069] Preferably, this embodiment provides a graphitization furnace, compared with the previous embodiment 1, such as Figure 1 , Figure 2 and Figure 4 As shown, this embodiment is further designed as follows:

[0070] The electromagnetic shielding structure 4 is formed by stacking at least two layers of carbon fiber cloth. Figure 4As shown, the electromagnetic shielding structure 4 is formed by alternately stacking carbon fiber cloth 41 and tungsten mesh 42. Preferably, the outer layers (first layer and last layer) of the electromagnetic shielding structure 4 are both carbon fiber cloth. Here, through the above arrangement, not only a better shielding effect can be achieved, but also the ablation resistance of the electromagnetic shielding structure can be improved.

[0071] Through the above design, the electromagnetic shielding structure 4 has an excellent electromagnetic shielding effect, which can well isolate the mutual influence of adjacent induction coils and ensure the stable operation of the equipment.

[0072] Example 3

[0073] Preferably, this embodiment provides a graphitization furnace, compared with the above embodiment, Figure 1 , Figure 2 , Figure 3 As shown, this embodiment is further designed as follows:

[0074] The width W of the furnace opening of the furnace 2 is 0.1-4.0 m; when the width W of the furnace opening is ≤ 1 m, the furnace 2 is an integrated structure. When the width W of the furnace opening is greater than 1 m, the furnace 2 is an integrated structure or a spliced ​​structure.

[0075] Preferably, the furnace 2 is formed by sequentially splicing a plurality of furnace sections; the number of furnace sections is consistent with the number of temperature zones and corresponds one to one. An electromagnetic shielding structure 4 (electromagnetic shielding plate) is provided between any two adjacent furnace sections; the electromagnetic shielding structure 4 is provided with a through hole for the fiber to pass through.

[0076] Preferably, the design of the furnace section can be the following two solutions:

[0077] The first solution is that each furnace section is an integrated structure. Preferably, the cross section of the furnace section forms a flat ring structure.

[0078] The second solution is: each of the furnace sections includes: a top plate 22, a bottom plate 23, a first curved side plate 24, and a second curved side plate 25; wherein the bottom plate 23 and the top plate 22 are arranged opposite to each other. The first side of the first curved side plate 24 is docked with the first side of the top plate 22, and the second side of the first curved side plate is docked with the first side of the bottom plate 23. The first side of the second curved side plate 25 is docked with the second side of the top plate 22, and the second side of the second curved side plate 25 is docked with the second side of the bottom plate 23. wherein the first side and the second side are two sides arranged opposite to each other. preferably, through the top plate 22, the bottom plate 23, the first curved side plate 24 and the second curved side plate 25, the cross section of the furnace section forms a flat annular structure (for the term "flat annular structure" involved in the present invention, see Figure 2 The first arc-shaped side plate 24 is a U-shaped plate; the second arc-shaped side plate 25 is a U-shaped plate.

[0079] It should be noted here that the "docking" method mentioned above can be achieved by any of the methods of auxiliary splints, screws, and heat treatment after bonding. It is preferably achieved by direct connection with auxiliary splints and screws, so that the connection contact resistance is much smaller than the cross-sectional resistance.

[0080] Preferably, the auxiliary splint is designed as follows: the first side of the first arc-shaped side plate 24 is butted against the first side of the top plate 22 through the first connecting plate 26, and the second side of the first arc-shaped side plate 24 is butted against the first side of the bottom plate 23 through the second connecting plate 27. The first side of the second arc-shaped side plate 25 is butted against the second side of the top plate 22 through the third connecting plate 28, and the second side of the second arc-shaped side plate 25 is butted against the second side of the bottom plate 23 through the fourth connecting plate 29.

[0081] Preferably, the furnace opening of the furnace is in the shape of a flat annular opening.

[0082] Preferably, the induction coil segment is a rectangular water-cooled induction coil; preferably, the induction coil segment is wound around the outer periphery of the furnace, and the shape of the induction coil segment is a flat ring structure. The induction coil segment is used to cooperate with the controller to generate the required induction magnetic field.

[0083] In summary, setting the furnace mouth (the inlet and outlet of the inner cavity of the furnace, the cross section of the entire furnace) to be flat can increase the effective space and further achieve energy saving. Setting the shape of the induction coil segment to a flat ring structure is more in line with process requirements and can further reduce energy consumption.

[0084] Example 4

[0085] Preferably, this embodiment provides a graphitization furnace, compared with the above embodiment, Figure 1 , Figure 2 , Figure 3 As shown, this embodiment is further designed as follows:

[0086] The material of the furnace is graphite, preferably isostatically pressed high-purity graphite.

[0087] Preferably, the thickness K of the furnace and the design temperature T of the highest temperature zone of the graphitization furnace satisfy the following relationship:

[0088] When T<2800℃, K=30-45mm;

[0089] When 2800℃≤T≤3200℃, K=0.2593×e 0.0019×T ;

[0090] The unit of K is mm, and the unit of T is °C.

[0091] Here, the above design purpose is to ensure the service life of the furnace and the structural strength of the furnace while considering the economic factors such as the furnace manufacturing cost; at the same time, the design of the furnace thickness can achieve a secondary temperature equalization effect and ensure that the graphitization furnace has a smaller cross-sectional temperature difference.

[0092] Example 5

[0093] Preferably, this embodiment provides a graphitization furnace, compared with the above embodiment, Figure 1 , Figure 2 As shown, this embodiment is further designed as follows:

[0094] The space between the furnace 2 and the induction coil 3 is filled with heat insulating material 10; preferably, the heat insulating material 10 is high temperature resistant graphite carbon felt, and a staggered cross-section structure is adopted during filling, which not only isolates the heat of the furnace from diffusing outward, but also ensures that no induced current is generated inside to cause self-heating problems.

[0095] The induction coil 3 is mounted on an insulating frame 8 (specifically, the induction coil is wrapped with insulating material, which plays the role of insulation and frame); preferably, the insulating frame 8 is made of refractory clay. Soft magnetic materials are evenly distributed in the insulating frame to play a magnetic role.

[0096] The graphitization furnace comprises a furnace shell 1. A furnace chamber 2 and an induction coil 3 are both located in the furnace shell 1; and a heat-insulating material 7 is filled between the furnace shell 1 and the furnace chamber 2 and the induction coil.

[0097] The graphitization furnace also includes: a controller 5 and a temperature measuring device 6; wherein, the number of the controllers 5 and the temperature measuring devices 6 is consistent with the number of the temperature sections and corresponds one to one; preferably, the temperature measuring device 6 is used to measure the temperature of the corresponding temperature section; the controller 5 is connected to the corresponding temperature measuring device 6 and the induction coil section to control the temperature of the temperature sections respectively.

[0098] Preferably, the inlet and outlet of the graphitization furnace are both provided with a detachable plug 9 to prevent heat radiation. Specifically, the inlet and outlet of the furnace cavity are both provided with a plug 9, and the plug 9 is provided with a through hole for the fiber filament to pass through.

[0099] Along the wire feeding direction, an electromagnetic shielding structure 4 is also provided on the side of the first induction coil segment close to the inlet of the graphitization furnace; an electromagnetic shielding structure 4 is also provided on the side of the last induction coil segment close to the outlet of the graphitization furnace.

[0100] In summary, the graphitization furnace provided above has at least the following advantages:

[0101] (1) By adding electromagnetic shielding plates, multiple continuous temperature zone designs can be realized to meet the needs of large-scale and continuous preparation of polyacrylonitrile-based high-strength and high-modulus carbon fibers.

[0102] (2) There is no flat structure induction coil in the prior art. Compared with the conventional circular induction coil, the flat induction coil is more in line with the process requirements and can further reduce energy consumption.

[0103] (3) The spliced ​​structure of the furnace chamber in the embodiment of the present invention can solve the problem that a wide-mouthed super-temperature graphitization furnace cannot be manufactured due to material problems.

[0104] (4) The graphitization furnace has a long service life. As an ultra-high temperature graphitization furnace (≥2800°C) for long-term use, the multi-stage continuous heating medium frequency induction furnace has a long stable operation time. When the graphitization temperature is below 2800°C, the service life exceeds 2 years; when the graphitization temperature is 3200°C, the service life exceeds 1 month.

[0105] (5) The graphitization furnace of the embodiment of the present invention can also replace the resistance furnace in high-temperature application scenarios, such as low-temperature carbonization furnace, high-temperature carbonization furnace, ultra-high-temperature carbonization furnace, etc., and has a wide range of applications. It can be used for continuous preparation of fibers and other materials such as carbon fiber, graphite fiber, silicon carbide fiber, etc. by gradient heating under an inert atmosphere. Compared with the resistance furnace, the graphitization furnace of the embodiment of the present invention has the characteristics of high energy efficiency ratio, long life, low cost, etc., and can operate stably at ultra-high temperature (≥2800℃) for a long time.

[0106] Example 6

[0107] This embodiment provides a method for preparing high-strength and high-modulus carbon fiber, which mainly includes the following steps:

[0108] Graphitization treatment: Graphitization treatment is performed on the fibers after high-temperature carbonization treatment to obtain high-strength and high-modulus carbon fibers;

[0109] Preferably, the polyacrylonitrile precursor is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment in sequence to obtain the fiber after high-temperature carbonization treatment. The fiber after high-temperature carbonization treatment has a bulk density of 1.79-1.81 g / cm3, a tensile strength of 6.1-6.4 GPa, and a tensile modulus of 280-300 GPa.

[0110] Wherein, the graphitization furnace described in any one of the above items is used to graphitize the fibers after high-temperature carbonization treatment.

[0111] Preferably, in the step of graphitization treatment: the temperature of the highest temperature zone of the graphitization treatment is 2050-3200°C, preferably 2100-3100°C. The sealing gas in the graphitization furnace is selected from one or more of argon, nitrogen and helium. The carrier gas in the graphitization furnace is selected from one or more of argon, nitrogen and helium. The pressure in the graphitization furnace is 0-500Pa, preferably 30-100Pa.

[0112] The rotation speed of the roller before the graphitization furnace and the rotation speed of the roller after the graphitization furnace meet the following conditions: 1≤V2 / V1≤1.3, preferably 1.05≤V2 / V1≤1.2; wherein V1 represents the rotation speed of the roller before the graphitization furnace, and the unit is m / s; V2 represents the rotation speed of the roller after the graphitization furnace, and the unit is m / s. Through the above design, the fiber crystallites can be further oriented, defects can be reduced, and the occurrence of hairy and broken wires can be reduced.

[0113] The graphitization treatment time t satisfies the following conditions: t=L×(V1+V2) / (2×V1×V2); 4D≤t≤20D, preferably 5D≤t≤10D; wherein t represents the graphitization treatment time, in s; L represents the length of the furnace, in m; V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; D represents the diameter of the fiber after high-temperature carbonization treatment, in μm. Here, the above design can ensure the fiber crystallinity and grain size, and improve the fiber performance.

[0114] Preferably, after the graphitization step, a post-treatment step is further included: surface treatment, water washing, sizing and drying of the high-strength and high-modulus carbon fiber.

[0115] Example 7

[0116] This embodiment provides a high-strength and high-modulus carbon fiber; wherein the high-strength and high-modulus carbon fiber is a polyacrylonitrile-based carbon fiber; the bulk density of the high-strength and high-modulus carbon fiber is 1.92-1.97 g / cm 3 , tensile strength is 3.7-4.2GPa, and tensile modulus is 580-700Gpa.

[0117] The high-strength and high-modulus carbon fiber is prepared by the preparation method of the high-strength and high-modulus carbon fiber of Example 6. The temperature zones of the graphitization treatment include the first temperature zone, the second temperature zone, and the third temperature zone in sequence; the temperature of the first temperature zone is 2450-2800°C, the temperature of the second temperature zone is 2550-3000°C, and the temperature of the third temperature zone is 2750-3150°C.

[0118] Here, the continuous ultra-high temperature wide-mouth graphitization furnace provided in the above embodiment is used to reasonably match the process conditions of the graphitization treatment process, so that the tensile strength and tensile modulus of the fiber are further improved. The tensile strength of the fiber is 3.7-4.2GPa, and the tensile modulus is 580-700GPa. The fiber has good stability, and large-scale and continuous preparation is achieved.

[0119] Example 8

[0120] This embodiment provides a new type of high-strength and high-modulus carbon fiber, wherein the new type of high-strength and high-modulus carbon fiber is a polyacrylonitrile-based carbon fiber; the bulk density of the high-strength and high-modulus carbon fiber is 1.78-1.85 g / cm 3 , tensile strength is 5.0-5.9GPa, tensile modulus is 370-450Gpa;

[0121] Preferably, the novel high-strength and high-modulus carbon fiber is prepared by the preparation method of the high-strength and high-modulus carbon fiber described in Example 6. The temperature zones of the graphitization treatment include the first temperature zone, the second temperature zone, and the third temperature zone in sequence; wherein the temperature of the first temperature zone is 1850-2050°C, the temperature of the second temperature zone is 1950-2200°C, and the temperature of the third temperature zone is 2050-2370°C.

[0122] Preferably, the high-strength and high-modulus carbon fiber composite material (resin-based carbon fiber unidirectional composite material) prepared from the high-modulus carbon fiber has a compressive strength of 1500-1950 MPa.

[0123] Here, the graphitization furnace of the above embodiment is used to finely match the process conditions of the graphitization treatment process to achieve both high strength and high modulus of the fiber, and obtain a new type of high-strength and high-modulus carbon fiber with a fiber tensile strength of 5.0-5.9GPa and a tensile modulus of 370-450GPa, and can be prepared on a large scale and continuously. The new high-strength and high-modulus carbon fiber composite material has a high compressive strength and meets the needs of high-end fields such as aerospace.

[0124] The following is further described by specific examples:

[0125] Experimental Example 1

[0126] The graphitization furnace provided in the above embodiment is used to prepare high-strength and high-modulus carbon fibers. The process mainly includes the following steps:

[0127] The fibers after high-temperature carbonization treatment are graphitized and post-treated to obtain high-strength and high-modulus carbon fibers. The fibers after high-temperature carbonization treatment have a bulk density of 1.80 g / cm3, a tensile strength of 6.1 GPa, a tensile modulus of 290 GPa, and a single fiber diameter of 5.3 μm.

[0128] Wherein, in the step of graphitization treatment: the temperature of graphitization treatment is 2500℃, 2610℃, 2810℃, and the sealing gas and carrier gas in the furnace are both argon gas; the pressure in the graphitization furnace is 40Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=1.08; the length of the furnace L=5.4m; the time of graphitization treatment t=31s. Wherein, the time t of the graphitization treatment satisfies the following conditions: t=L×(V1+V2) / (2×V1×V2); 5D≤t≤10D; wherein t represents the time of graphitization treatment, in s; L represents the length of the furnace, in m; V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; D is the diameter of the fiber after high-temperature carbonization treatment, in μm.

[0129] The performance indicators of the high-strength and high-modulus carbon fiber prepared in this embodiment are as follows: tensile strength is 4.10 GPa, tensile modulus is 590 GPa, elongation at break is 0.7%, and bulk density is 1.93 g / cm3.

[0130] Experimental Example 2

[0131] The graphitization furnace provided in the above embodiment is used to prepare high-strength and high-modulus carbon fibers. The process mainly includes the following steps:

[0132] The fiber after high-temperature carbonization treatment is graphitized and post-treated to obtain high-strength and high-modulus carbon fiber. The bulk density of the fiber after high-temperature carbonization treatment is 1.80g / cm3, the tensile strength is 6.2GPa, the tensile modulus is 290Gpa, and the single fiber diameter is 5.3μm. In the step of graphitization treatment: the temperature of graphitization treatment is 2600℃, 2720℃, and 2930℃, and argon is used as the sealing gas and carrier gas in the furnace; the pressure in the graphitization furnace is 40Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=1.15; the furnace length L=5.4m; the graphitization treatment time t=30s. Among them, the time t of the graphitization treatment satisfies the following conditions: t=L×(V1+V2) / (2×V1×V2); 5D≤t≤10D; wherein, t represents the time of graphitization treatment, and the unit is s; L represents the length of the furnace, and the unit is m; V1 represents the rotation speed of the roller before the graphitization furnace, and the unit is m / s; V2 represents the rotation speed of the roller after the graphitization furnace, and the unit is m / s; D is the diameter of the fiber after high-temperature carbonization treatment, and the unit is μm.

[0133] The performance indicators of the high-strength and high-modulus carbon fiber prepared in this embodiment are as follows: tensile strength is 3.90 GPa, tensile modulus is 646 GPa, elongation at break is 0.6%, and bulk density is 1.95 g / cm3.

[0134] Experimental Example 3

[0135] The graphitization furnace provided in the above embodiment is used to prepare high-strength and high-modulus carbon fibers. The process mainly includes the following steps:

[0136] The fibers after high-temperature carbonization treatment are graphitized and post-treated to obtain high-strength and high-modulus carbon fibers. The fibers after high-temperature carbonization treatment have a bulk density of 1.80 g / cm3, a tensile strength of 6.3 GPa, a tensile modulus of 290 GPa, and a single fiber diameter of 5.3 μm.

[0137] Wherein, in the step of graphitization treatment: the temperature of graphitization treatment is 2750℃, 2940℃, 3100℃, argon gas is selected as sealing gas and carrier gas in the furnace; the pressure in the graphitization furnace is 40Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=1.2; the length of the furnace L=5.4m; the graphitization treatment time t=30s. Wherein, the graphitization treatment time t satisfies the following conditions: t=L×(V1+V2) / (2×V1×V2); 5D≤t≤10D; where t represents the time of graphitization treatment, in s; L represents the length of the furnace, in m; V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; D is the diameter of the fiber after high-temperature carbonization treatment, in μm.

[0138] The performance indicators of the high-strength and high-modulus carbon fiber prepared in this embodiment are as follows: tensile strength is 3.80 GPa, tensile modulus is 690 GPa, elongation at break is 0.5%, and bulk density is 1.97 g / cm3.

[0139] Experimental Example 4

[0140] The graphitization furnace provided in the above embodiment is used to prepare a new type of high-strength and high-modulus carbon fiber. The main steps are as follows:

[0141] The fibers after high-temperature carbonization treatment are graphitized and post-treated to obtain high-strength and high-modulus carbon fibers. The fibers after high-temperature carbonization treatment have a bulk density of 1.80 g / cm3, a tensile strength of 6.2 GPa, a tensile modulus of 295 GPa, and a single fiber diameter of 5.6 μm.

[0142] Wherein, in the step of graphitization treatment: the temperature of graphitization treatment is 1900℃, 1990℃, 2100℃, argon gas is selected as sealing gas and carrier gas in the furnace; the pressure in the graphitization furnace is 40Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=1.05; the length of the furnace L=5.4m; the graphitization treatment time t=32s. Wherein, the graphitization treatment time t satisfies the following conditions: t=L×(V1+V2) / (2×V1×V2); 5D≤t≤10D; where t represents the time of graphitization treatment, in s; L represents the length of the furnace, in m; V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; D is the diameter of the fiber after high-temperature carbonization treatment, in μm.

[0143] The performance indicators of the high-strength and high-modulus carbon fiber prepared in this embodiment are as follows: tensile strength is 5.80 GPa, tensile modulus is 380 GPa, elongation at break is 1.5%, and bulk density is 1.79 g / cm3.

[0144] Experimental Example 5

[0145] The graphitization furnace provided in the above embodiment is used to prepare a new type of high-strength and high-modulus carbon fiber. The main steps are as follows:

[0146] The fibers after high-temperature carbonization treatment are graphitized and post-treated to obtain high-strength and high-modulus carbon fibers. The fibers after high-temperature carbonization treatment have a bulk density of 1.80 g / cm3, a tensile strength of 6.2 GPa, a tensile modulus of 295 GPa, and a single fiber diameter of 5.6 μm.

[0147] Wherein, in the step of graphitization treatment: the temperature of graphitization treatment is 2000℃, 2160℃, 2320℃, argon gas is selected as sealing gas and carrier gas in the furnace; the pressure in the graphitization furnace is 40Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=1.08; the length of the furnace L=5.1m; the time of graphitization treatment t=31s. Wherein, the time t of the graphitization treatment satisfies the following conditions: t=L×(V1+V2) / (2×V1×V2); 5D≤t≤10D; wherein t represents the time of graphitization treatment, in s; L represents the length of the furnace, in m; V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; D is the diameter of the fiber after high-temperature carbonization treatment, in μm.

[0148] The performance indicators of the high-strength and high-modulus carbon fiber prepared in this embodiment are as follows: tensile strength is 5.10 GPa, tensile modulus is 440 GPa, elongation at break is 1.2%, and bulk density is 1.84 g / cm3.

[0149] Here, it should be noted that with the increase of graphitization temperature, the modulus of carbon fiber increases and the strength decreases.

[0150] The carbon fibers prepared in Experimental Examples 4-5 can be prepared in a conventional graphitization furnace because of their low graphitization temperature. However, large-scale preparation is not possible due to the small mouth width of the existing graphitization furnace.

[0151] For the carbon fibers prepared in Experimental Examples 1-3, since the temperature of the existing conventional graphitization furnace cannot reach the required process temperature, the carbon fibers cannot be prepared using a conventional graphitization furnace, let alone large-scale preparation.

[0152] Comparative Example 1

[0153] Comparative Example 1 uses a conventional resistive graphitization furnace to prepare high-strength and high-modulus carbon fibers. The main steps are as follows:

[0154] The fibers after high-temperature carbonization treatment are graphitized and post-treated to obtain high-strength and high-modulus carbon fibers. The fibers after high-temperature carbonization treatment have a bulk density of 1.80 g / cm3, a tensile strength of 6.1 GPa, a tensile modulus of 290 GPa, and a single fiber diameter of 5.3 μm.

[0155] Among them, in the step of graphitization treatment: the temperature of graphitization treatment is 2500°C, 2610°C, and 2810°C, and argon is used as the sealing gas and the carrier gas in the furnace; the pressure in the graphitization furnace is 40Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=1.08; the furnace length L=5.4m; the time t of graphitization treatment is 31s.

[0156] The performance indicators of the high-strength and high-modulus carbon fiber prepared in Comparative Example 1 are as follows: tensile strength is 4.00 GPa, tensile modulus is 580 GPa, elongation at break is 0.7%, and bulk density is 1.93 g / cm3.

[0157] In addition, the loss of graphite heating elements increases sharply, and the life of the heating elements is greatly reduced to 6 days, which makes it impossible to achieve large-scale and continuous production, and the fiber production cost increases significantly.

[0158] Comparative Example 2

[0159] Comparative Example 2 uses a conventional induction heating graphitization furnace to prepare high-strength and high-modulus carbon fibers. The difference between this induction heating graphitization furnace and the embodiment of the present invention is that no electromagnetic shielding structure is set between any two adjacent induction coil segments. In order to avoid the mutual influence of the magnetic flux lines between any two adjacent temperature sections, the distance between the two adjacent temperature sections is increased to 500 mm. It mainly includes the following steps:

[0160] The fibers after high-temperature carbonization treatment are graphitized and post-treated to obtain high-strength and high-modulus carbon fibers. The fibers after high-temperature carbonization treatment have a bulk density of 1.80 g / cm3, a tensile strength of 6.1 GPa, a tensile modulus of 290 GPa, and a single fiber diameter of 5.3 μm.

[0161] Among them, in the step of graphitization treatment: the temperature of graphitization treatment is 2500°C, 2610°C, and 2810°C, and argon is used as the sealing gas and the carrier gas in the furnace; the pressure in the graphitization furnace is 40Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=1.08; the furnace length L=5.4m; the time t of graphitization treatment is 31s.

[0162] The performance indicators of the high-strength and high-modulus carbon fiber prepared in Comparative Example 2 are as follows: tensile strength is 4.10 GPa, tensile modulus is 550 GPa, elongation at break is 0.7%, and bulk density is 1.92 g / cm3.

[0163] In Comparative Example 2, the distance between two adjacent temperature sections (the distance between two adjacent furnaces) is relatively large, so that there is a cold zone between the two adjacent temperature sections, and thus the tensile modulus of the prepared carbon fiber is significantly reduced.

[0164] Comparative Example 3

[0165] Comparative Example 3 uses the graphitization furnace provided in the above embodiment to prepare high-strength and high-modulus carbon fibers. The main difference between Comparative Example 3 and Experimental Example 1 is that the process parameters are different. The main steps are as follows:

[0166] The fibers after high-temperature carbonization treatment are graphitized and post-treated to obtain high-strength and high-modulus carbon fibers. The fibers after high-temperature carbonization treatment have a bulk density of 1.80 g / cm3, a tensile strength of 6.1 GPa, a tensile modulus of 290 GPa, and a single fiber diameter of 5.3 μm.

[0167] Among them, in the step of graphitization treatment: the temperature of graphitization treatment is 2400°C, 2520°C, and 2710°C, and argon is used as the sealing gas and the carrier gas in the furnace; the pressure in the graphitization furnace is 10Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=0.99; the furnace length L=5.4m; the time t of graphitization treatment is 33s.

[0168] The performance indicators of the high-strength and high-modulus carbon fiber prepared in Comparative Example 3 are as follows: tensile strength is 4.10 GPa, tensile modulus is 548 GPa, elongation at break is 0.7%, and bulk density is 1.91 g / cm3.

[0169] It should be noted here that: Comparative Experimental Example 1 and Comparative Example 3 both use the graphitization furnace provided by the embodiment of the present invention, and prepare high-strength and high-modulus carbon fibers under the same fiber performance after high-temperature carbonization treatment. The reason why there are differences in the performance of the high-strength and high-modulus carbon fibers prepared in Experimental Example 1 and Comparative Example 3 is mainly due to the different preparation processes. The synergistic effect of factors such as the low graphitization treatment temperature of Comparative Example 3, the small ratio of the rotation speed V2 of the roller after the graphitization furnace to the rotation speed V1 of the roller before the graphitization furnace, and the small pressure in the graphitization furnace, results in the tensile modulus of Comparative Example 3 being lower than that of Experimental Example 1.

[0170] Comparative Example 4

[0171] Comparative Example 4 uses the graphitization furnace provided in the above embodiment to prepare a new type of high-strength and high-modulus carbon fiber. The main difference between Comparative Example 4 and Experimental Example 4 is that the process parameters are different. It mainly includes the following steps:

[0172] The fibers after high-temperature carbonization treatment are graphitized and post-treated to obtain high-strength and high-modulus carbon fibers. The fibers after high-temperature carbonization treatment have a bulk density of 1.80 g / cm3, a tensile strength of 6.2 GPa, a tensile modulus of 295 GPa, and a single fiber diameter of 5.6 μm.

[0173] Among them, in the step of graphitization treatment: the temperature of graphitization treatment is 1800°C, 1890°C, and 2000°C, and argon is used as the sealing gas and the carrier gas in the furnace; the pressure in the graphitization furnace is 10Pa; the relationship between the rotation speed V1 of the roller before the graphitization furnace and the rotation speed V2 of the roller after the graphitization furnace is: V2 / V1=0.99; the furnace length L=5.4m; the graphitization treatment time t=33s.

[0174] The performance indicators of the high-strength and high-modulus carbon fiber prepared in Comparative Example 4 are as follows: tensile strength is 5.70 GPa, tensile modulus is 351 GPa, elongation at break is 1.6%, and bulk density is 1.77 g / cm3.

[0175] It should be noted here that: both the comparative experimental example 4 and the comparative example 4 use the graphitization furnace provided by the embodiment of the present invention, and prepare a new type of strong high modulus carbon fiber under the condition that the fiber performance after high-temperature carbonization treatment is the same. The reason why the performance of the new high-strength and high modulus carbon fiber prepared by the experimental example 4 and the comparative example 4 is different is mainly due to the different preparation processes. The synergistic effect of factors such as the low graphitization treatment temperature of the comparative example 4, the small ratio of the rotation speed V2 of the roller after the graphitization furnace to the rotation speed V1 of the roller before the graphitization furnace, and the small pressure in the graphitization furnace, causes the tensile modulus of the comparative example 4 to be lower than that of the experimental example 4.

[0176] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A graphitization furnace, characterized in that: The graphitization furnace is an induction heating graphitization furnace; wherein the graphitization furnace comprises: A furnace, wherein the inner cavity of the furnace comprises a plurality of temperature sections arranged in sequence; an induction coil, the induction coil being arranged around the outer circumference of the furnace and being used for generating an induced current in the furnace to heat the furnace; The induction coil includes a plurality of induction coil segments; wherein the number of the induction coil segments is consistent with the number of the temperature zones, and each of the induction coil segments is arranged around the corresponding temperature zone to heat the corresponding temperature zone; Wherein, an electromagnetic shielding structure is arranged between any two adjacent induction coil segments to avoid mutual influence between the magnetic flux lines of any two adjacent temperature zones.

2. The graphitization furnace according to claim 1, characterized in that: The inner cavity of the furnace is provided with a wire passage, so that the fibers to be graphitized can pass through a plurality of temperature sections in sequence and continuously.

3. The graphitization furnace according to claim 1 or 2, characterized in that: The material of the electromagnetic shielding structure is selected from a set material; wherein, in an inert atmosphere, the set material can withstand a temperature of ≥3000°C; and / or The electromagnetic shielding structure is formed by stacking at least two layers of carbon fiber cloth; or the electromagnetic shielding structure is formed by stacking carbon fiber cloth and tungsten mesh alternately in sequence. Further preferably, the outer layers of the electromagnetic shielding structure are all carbon fiber cloth.

4. The graphitization furnace according to any one of claims 1 to 3, characterized in that: The electromagnetic shielding structure is an electromagnetic shielding plate.

5. The graphitization furnace according to any one of claims 1 to 4, characterized in that: The width W of the furnace mouth of the furnace is 0.1-4.0m; When the width W of the furnace mouth is ≤1m, the furnace is an integrated structure; When the width W of the furnace opening is greater than 1 m, the furnace chamber is an integrated structure or a spliced ​​structure.

6. The graphitization furnace according to any one of claims 1 to 5, characterized in that: The furnace is formed by sequentially splicing a plurality of furnace sections; wherein the number of the furnace sections is consistent with the number of the temperature zones and corresponds one to one; Preferably, an electromagnetic shielding structure is provided between any two adjacent furnace sections; and a through hole for allowing the fiber to pass through is provided on the electromagnetic shielding structure.

7. The graphitization furnace according to claim 6, characterized in that: Each of the furnace sections is an integrated structure. Preferably, the cross section of the furnace section forms a flat annular structure.

8. The graphitization furnace according to claim 6, characterized in that: Each of the furnace sections comprises: roof; A bottom plate, wherein the bottom plate and the top plate are arranged opposite to each other; a first arc-shaped side plate, wherein a first side of the first arc-shaped side plate is butted against a first side of the top plate, and a second side of the first arc-shaped side plate is butted against a first side of the bottom plate; a second curved side plate, wherein a first side of the second curved side plate is butted against a second side of the top plate, and a second side of the second curved side plate is butted against a second side of the bottom plate; Wherein, the first side and the second side are two sides arranged opposite to each other; Preferably, the cross section of the furnace section forms a flat annular structure through the top plate, the bottom plate, the first arc-shaped side plate and the second arc-shaped side plate; Preferably, the first arc-shaped side plate is a U-shaped plate; Preferably, the second arc-shaped side plate is a U-shaped plate; Preferably, the first side of the first curved side panel is connected to the first side of the top panel via a first connecting plate, and the second side of the first curved side panel is connected to the first side of the bottom panel via a second connecting plate; the first side of the second curved side panel is connected to the second side of the top panel via a third connecting plate, and the second side of the second curved side panel is connected to the second side of the bottom panel via a fourth connecting plate.

9. The graphitization furnace according to any one of claims 1 to 8, characterized in that: The furnace opening of the furnace is in the shape of a flat annular opening; and / or The induction coil segment is wound around the outer periphery of the furnace; preferably, the induction coil segment is a flat ring structure; and / or The furnace is made of graphite, preferably isostatic graphite.

10. The graphitization furnace according to any one of claims 1 to 9, characterized in that: The thickness K of the furnace and the design temperature T of the highest temperature zone of the graphitization furnace satisfy the following relationship: When T<2800℃, K=30-45mm; When 2800℃≤T≤3200℃, K=0.2593×e 0.0019×T ; The unit of K is mm, and the unit of T is °C.

11. The graphitization furnace according to any one of claims 1 to 10, characterized in that: The furnace and the induction coil are filled with a heat insulating material; preferably, the heat insulating material is high temperature resistant graphite carbon felt; and / or The induction coil is mounted on an insulating frame; preferably, the insulating frame is made of refractory clay; preferably, soft magnetic material is evenly distributed in the insulating frame to play a magnetic role; and / or The graphitization furnace comprises a furnace shell; the furnace chamber and the induction coil are both located in the furnace shell; and the gap between the furnace shell and the furnace chamber and the induction coil is filled with a thermal insulation material; and / or The graphitization furnace further comprises: a controller and a temperature measuring device; wherein the number of the controllers and the temperature measuring devices is consistent with the number of the temperature sections and corresponds one to one; preferably, the temperature measuring device is used to measure the temperature of the corresponding temperature section; the controller is connected to the corresponding temperature measuring device and the induction coil section; and / or The inlet and outlet of the graphitization furnace are both provided with removable plugs to prevent heat radiation; and / or The number of the temperature zones is greater than 1 and less than or equal to 9; and / or Along the wire feeding direction, an electromagnetic shielding structure is also provided on the side of the first induction coil segment close to the inlet of the graphitization furnace; an electromagnetic shielding structure is also provided on the side of the last induction coil segment close to the outlet of the graphitization furnace.

12. A method for preparing high-strength and high-modulus carbon fiber, characterized in that: It includes the following steps: Graphitization treatment: Graphitization treatment is performed on the fibers after high-temperature carbonization treatment to obtain high-strength and high-modulus carbon fibers; Wherein, the graphitization furnace described in any one of claims 1 to 11 is used to graphitize the fiber after high-temperature carbonization treatment; The polyacrylonitrile precursor is subjected to a pre-oxidation treatment, a low-temperature carbonization treatment, and a high-temperature carbonization treatment in sequence to obtain the fiber subjected to the high-temperature carbonization treatment; Preferably, the fiber after high-temperature carbonization has a bulk density of 1.79-1.81 g / cm3, a tensile strength of 6.1-6.4 GPa, and a tensile modulus of 280-300 GPa.

13. The method for preparing high-strength and high-modulus carbon fiber according to claim 12, characterized in that: In the step of graphitization: The temperature of the highest temperature zone of the graphitization treatment is 2050-3200° C., preferably 2100-3100° C.; and / or The sealing gas in the graphitization furnace is selected from one or more of argon, nitrogen and helium; and / or The carrier gas in the graphitization furnace is one or more of argon, nitrogen and helium; and / or The pressure inside the graphitization furnace is 0-500 Pa, preferably 30-100 Pa; and / or The rotation speed of the roller before the graphitization furnace and the rotation speed of the roller after the graphitization furnace meet the following conditions: 1≤V2 / V1≤1.3, preferably 1.05≤V2 / V1≤1.2; wherein V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; and / or The time t of graphitization treatment satisfies the following conditions: t=L×(V1+V2) / (2×V1×V2); 4D≤t≤20D, preferably 5D≤t≤10D; wherein t represents the time of graphitization treatment, in s; L represents the length of the furnace, in m; V1 represents the rotation speed of the roller before the graphitization furnace, in m / s; V2 represents the rotation speed of the roller after the graphitization furnace, in m / s; D is the diameter of the fiber after high-temperature carbonization treatment, in μm.

14. A high-strength and high-modulus carbon fiber, characterized in that: The high-strength and high-modulus carbon fiber is a polyacrylonitrile-based carbon fiber; wherein the bulk density of the high-strength and high-modulus carbon fiber is 1.92-1.97 g / cm 3 , tensile strength is 3.7-4.2GPa, tensile modulus is 580-700Gpa; Preferably, the high-strength and high-modulus carbon fiber is prepared by the preparation method of the high-strength and high-modulus carbon fiber according to claim 12 or 13; wherein the temperature zones for graphitization treatment include a first temperature zone, a second temperature zone, and a third temperature zone in sequence; wherein the temperature of the first temperature zone is 2450-2800°C, the temperature of the second temperature zone is 2550-3000°C, and the temperature of the third temperature zone is 2750-3150°C.

15. A high-strength and high-modulus carbon fiber, characterized in that: The high-strength and high-modulus carbon fiber is a polyacrylonitrile-based carbon fiber; wherein the bulk density of the high-strength and high-modulus carbon fiber is 1.78-1.85 g / cm 3 , tensile strength is 5.0-5.9GPa, tensile modulus is 370-450Gpa; Preferably, the high-strength and high-modulus carbon fiber is prepared by the preparation method of the high-strength and high-modulus carbon fiber according to claim 12 or 13; wherein the temperature zones for graphitization treatment include a first temperature zone, a second temperature zone, and a third temperature zone in sequence; wherein the temperature of the first temperature zone is 1850-2050°C, the temperature of the second temperature zone is 1950-2200°C, and the temperature of the third temperature zone is 2050-2370°C.

16. A carbon fiber composite material, characterized in that: The carbon fiber composite material is a resin-based carbon fiber unidirectional composite material; wherein the compressive strength of the carbon fiber composite material is 1500-1950 MPa; Wherein, the carbon fiber composite material is prepared from the high modulus and high strength carbon fiber described in claim 15.

Citation Information

Cited By

  • Medium-frequency induction type carbon fiber self-heating graphitization furnace

    CN122329005A