Method for preparing sizing carbon fiber by using polyether-containing polyurethane pre-sizing agent, application of sizing carbon fiber, sizing carbon fiber and application of sizing carbon fiber

By using pre-sizing agent containing polyether polyurethane and epoxy resin on carbon fiber and secondary sizing technology of resorcinol formaldehyde latex on carbon fiber, the problem of poor bonding between carbon fiber and rubber material is solved, and the adhesion is significantly improved and Wear resistance, suitable for high temperature and high strength working conditions.

CN118932726APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310536584.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The poor interface bond between carbon fiber and rubber material leads to insufficient adhesion and poor wear resistance. The prior art such as acidification treatment has safety and economic problems.

Method used

The carbon fiber is pre-sizing and pre-dryed with a pre-sizing agent containing polyether polyurethane and epoxy resin, followed by secondary sizing and secondary drying with resorcinol formaldehyde gel latex, and the wetting time is ≤25 seconds and viscosity is ≤45. Cipopol, to improve the adhesion and wear resistance of carbon fiber to rubber matrix.

Benefits of technology

It significantly enhances the adhesion between the sizing carbon fiber and the rubber matrix, with wear resistance of more than 4,000 times, and improves the temperature resistance to above 250℃. It has a simple process, safe and pollution-free process, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004226497930000111
    Figure BDA0004226497930000111
  • Figure BDA0004226497930000112
    Figure BDA0004226497930000112
  • Figure BDA0004226497930000121
    Figure BDA0004226497930000121
Patent Text Reader

Abstract

The invention relates to the field of carbon fiber sizing agents, and discloses a method for preparing sizing carbon fibers by using a polyether-containing polyurethane pre-sizing agent, application of the sizing carbon fibers, the sizing carbon fibers and application of the sizing carbon fibers. The method comprises the following steps: S1, carrying out pre-sizing and pre-drying on carbon fibers by adopting a pre-sizing agent containing polyether polyurethane and epoxy resin to obtain initial carbon fibers; s2, carrying out secondary sizing and secondary drying on the initial carbon fiber by adopting resorcinol formaldehyde latex to obtain sized carbon fiber; the infiltration time of the pre-sizing agent is less than or equal to 25 seconds, and the viscosity at 25 DEG C is less than or equal to 45 centipoises. The surface of the carbon fiber is coated with a pre-sizing agent containing polyether polyurethane and epoxy resin, pre-drying is conducted, primary bonding with the surface of the carbon fiber is achieved, and then secondary sizing and secondary drying are conducted through resorcinol formaldehyde latex. The existence of polyether polyurethane can obviously enhance the bonding force between the sizing carbon fiber and a rubber matrix, and meanwhile, improves the wear resistance of the sizing carbon fiber and improves the temperature resistance of the sizing carbon fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of carbon fiber sizing agents, and in particular to a method for preparing sized carbon fibers by utilizing a pre-sizing agent containing polyether polyurethane and its application, and the sized carbon fibers and their application. Background Art

[0002] Carbon fiber reinforced rubber composites can effectively combine the rigidity of carbon fiber and the flexibility of rubber. They have the advantages of high strength, high modulus, high elasticity, fatigue resistance and good dimensional stability. They expand the scope of use of rubber products and have broad potential application value in more demanding application fields such as tires, transmission belts, conveyor belts and high-pressure hoses. However, due to the difference in performance between the two materials, there is a problem of poor interface bonding between carbon fiber and rubber materials. In carbon fiber reinforced resin-based composites, surface coating sizing agents are usually used to improve interface bonding, but there is no special sizing agent suitable for carbon fiber reinforced rubber materials. At the same time, many of the actual application occasions of carbon fiber reinforced rubber composites are long-term high-intensity friction conditions, so higher requirements are also placed on the process properties such as wear resistance of carbon fiber and carbon fiber reinforced rubber composites.

[0003] CN107459682A provides a method for preparing a carbon fiber reinforced rubber composite material, in which the carbon fiber is acidified to increase the surface roughness of the fiber to improve the interface performance between the fiber and the rubber. However, this method is an intermittent method, requires the use of strong acid, is time-consuming, highly polluting, and has poor safety and economic efficiency.

[0004] Therefore, how to overcome the above problems has become an important research topic in this field. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem that the sizing agent in the prior art has weak bonding force with the rubber matrix after sizing the carbon fiber, and the sizing carbon fiber has poor wear resistance, and to provide a method and application of preparing sizing carbon fiber using a pre-sizing agent containing polyether polyurethane, and sizing carbon fiber and application. The method is simple to operate, and a layer of pre-sizing agent containing polyether polyurethane and epoxy resin is coated on the surface of the carbon fiber and pre-dried to achieve preliminary bonding with the surface of the carbon fiber, and then resorcinol formaldehyde latex (hereinafter referred to as RFL emulsion) is used for secondary sizing and secondary drying. Due to the presence of polyether polyurethane, the bonding force between the sizing carbon fiber and the rubber matrix can be significantly enhanced, and the wear resistance of the sizing carbon fiber can be effectively improved, and its temperature resistance can be improved, and the applicability of subsequent processing of the sizing carbon fiber can be improved.

[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing sized carbon fiber using a polyether polyurethane pre-sizing agent, wherein the method comprises:

[0007] S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing polyether polyurethane and epoxy resin to obtain initial carbon fiber;

[0008] S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber;

[0009] The pre-sizing agent has a wetting time of ≤25 seconds and a viscosity of ≤45 centipoise at 25°C.

[0010] The second aspect of the present invention provides a sized carbon fiber prepared by the method for preparing sized carbon fiber using a polyether polyurethane pre-sizing agent as described in the first aspect of the present invention.

[0011] The third aspect of the present invention provides a method for preparing sized carbon fibers using a polyether polyurethane pre-sizing agent as described in the first aspect of the present invention, and application of the sized carbon fibers as described in the second aspect of the present invention in rubber materials.

[0012] Through the above technical scheme, the method and application of preparing sized carbon fiber containing polyether polyurethane pre-sizing agent, and the sized carbon fiber and application provided by the present invention achieve the following beneficial effects:

[0013] (1) The present invention uses epoxy resin and polyether polyurethane as the main components in the pre-sizing agent, and adopts an RFL emulsion sizing agent with good affinity to the rubber matrix in the secondary sizing process, which can significantly improve the bonding force between the prepared sized carbon fiber and the rubber matrix two-phase interface, which can reach more than 150N, and at the same time has good wear resistance, and the number of wear resistance can reach more than 4000 times.

[0014] (2) The present invention utilizes a pre-sizing agent and an RFL emulsion to perform pre-sizing and secondary sizing on carbon fibers, respectively, so that when the prepared sized carbon fibers are applied to rubber materials, the bonding strength between the carbon fibers and the rubber matrix is ​​significantly improved, while the temperature resistance of the sized carbon fibers is improved, and the carbon fibers can withstand high temperatures of more than 250°C.

[0015] (3) The present invention controls the wetting time of the pre-sizing agent to be ≤25 seconds, the viscosity at 25°C to be ≤45 centipoise, and specific pre-sizing and secondary sizing processes to ultimately prepare sized carbon fibers with high temperature resistance, excellent bonding strength with the rubber matrix, and good wear resistance.

[0016] (4) The method of the present invention is simple in process, highly stable, safe and pollution-free, and can be completed using an existing carbon fiber preparation production line, thus having broad industrial prospects. DETAILED DESCRIPTION

[0017] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0018] A first aspect of the present invention provides a method for preparing sized carbon fiber using a polyether polyurethane pre-sizing agent, wherein the method comprises:

[0019] S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing polyether polyurethane and epoxy resin to obtain initial carbon fiber;

[0020] S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber;

[0021] The pre-sizing agent has a wetting time of ≤25 seconds and a viscosity of ≤45 centipoise at 25°C.

[0022] In the present invention, the inventors found that in the prior art, RFL emulsion is used to improve the bonding force between sized carbon fiber and rubber matrix. However, it is found in actual application that due to the weak bonding ability between RFL emulsion and carbon fiber surface, the use of RFL emulsion alone cannot effectively improve the interface problem between carbon fiber and rubber matrix. The inventors found that because RFL emulsion itself is an aqueous emulsion, it does not spread well on the surface of inert carbon fiber, resulting in discontinuous and weak bonding points.

[0023] The inventors have found that a layer of pre-sizing agent containing polyether polyurethane and epoxy resin is first coated on the surface of the carbon fiber and pre-dried to achieve initial bonding with the surface of the carbon fiber. Furthermore, since the pre-sizing agent has good hydrophilicity, the RFL emulsion is used for secondary sizing and secondary drying, so that the RFL emulsion can be quickly spread and infiltrated on the surface of the carbon fiber coated with the pre-sizing agent, and the pre-sizing agent plays a role in coupling the RFL and carbon fiber phases. Due to the presence of polyether polyurethane in the pre-sizing agent, the wear resistance and temperature resistance of the sized carbon fiber can be effectively improved at the same time, and the applicability of subsequent processing of the sized carbon fiber can be improved. At the same time, when the sized carbon fiber prepared by the pre-sizing agent is used to reinforce rubber composite materials, the bonding force between the sized carbon fiber and the rubber matrix can be significantly enhanced.

[0024] Further research found that only when the infiltration time of the introduced pre-sizing agent is ≤25 seconds and the viscosity at 25°C is ≤45 centipoise, can the pre-sizing agent achieve secondary uniform infiltration of the RFL emulsion and provide a good coupling enhancement effect for the carbon fiber and the RFL emulsion. When the infiltration time is greater than 25 seconds, the hydrophilicity is insufficient, which will lead to insufficient binding ability of the pre-sizing agent with the carbon fiber and the RFL emulsion, and will not play a role in coupling enhancement. When the viscosity is greater than 45 centipoise at 25°C, the expansion of the pre-sizing agent on the surface of the carbon fiber is greatly hindered, and it cannot be evenly infiltrated and spread, thereby affecting the improvement of the bonding force and the uniformity of the process properties such as carbon fiber wear resistance.

[0025] In the present invention, the epoxy resin is a glycidyl ether epoxy resin containing two or more epoxy groups in the molecule, for example, it may be at least one of bisphenol A, bisphenol F, and bisphenol S.

[0026] In the present invention, the epoxy equivalent of the epoxy resin is 160-6000.

[0027] In the present invention, the epoxy equivalent of the epoxy resin satisfies the above range, so that the wetting time and viscosity of the prepared pre-sizing agent at 25° C. can meet the requirements.

[0028] In the present invention, the pre-sizing agent may further contain components such as antioxidants, lubricants, surfactants, etc. The surfactant is preferably a non-ionic surfactant.

[0029] According to a preferred embodiment of the present invention, the nonionic surfactant is selected from at least one of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyoxyethylene amine, polyoxyethylene amide, sorbitan ester and fluorocarbon surfactant.

[0030] In the present invention, there is no particular limitation on the types and contents of the antioxidant, lubricant and surfactant contained in the pre-sizing agent, and they can be adjusted according to the needs in the art.

[0031] According to a particularly preferred embodiment of the present invention, the pre-sizing agent contains 30-55 parts of epoxy resin, 20-35 parts of polyether polyurethane, 1-5 parts of antioxidant, 1-5 parts of lubricant and 10-40 parts of surfactant. When each component meets the above range, the pre-sizing agent has a better effect when applied to sizing carbon fiber.

[0032] In the present invention, the epoxy resin, antioxidant, lubricant and surfactant may be provided in the form of an epoxy resin aqueous emulsion.

[0033] In the present invention, the epoxy resin, antioxidant, lubricant and surfactant are configured into an epoxy resin aqueous emulsion for addition, and further combined with the RFL emulsion to enhance the synergistic effect between the components, significantly enhance the bonding force between the sized carbon fibers and the rubber matrix, and effectively improve the wear resistance and temperature resistance of the sized carbon fibers.

[0034] In the present invention, the preparation method of the pre-sizing agent in step S1 can adopt the preparation method of the emulsion generally used in the art, such as phase inversion emulsification method, ultrasonic emulsification method and colloid mill emulsification method.

[0035] In the present invention, the viscosity of the pre-sizing agent refers to the viscosity when the pre-sizing agent is diluted with water to a concentration of 2 wt %.

[0036] In the present invention, the RFL emulsion is a mixed emulsion formed by the reaction of resorcinol, formaldehyde and rubber emulsion. The specific preparation process is: sodium hydroxide and resorcinol are added to the first reaction kettle, and then an appropriate amount of water is added, the temperature is controlled to 20-40°C, and then formaldehyde is slowly added, and a prepolymer is obtained after aging reaction for 2-4 hours; rubber latex is added to the second reaction kettle, the temperature is controlled to 20-40°C, and the synthesized prepolymer is slowly added dropwise, and the reaction is continued for 10-30 hours to finally prepare the RFL emulsion.

[0037] In the present invention, the rubber emulsion in the RFL emulsion can be acrylic rubber emulsion, acrylonitrile-butadiene rubber emulsion, isoprene rubber emulsion, polyurethane rubber emulsion, ethylene-propylene rubber emulsion, chloroprene rubber emulsion, silicone rubber emulsion, hydrogenated nitrile rubber emulsion, styrene-butadiene rubber emulsion, polysulfide rubber emulsion, natural rubber emulsion, butadiene rubber emulsion and butyl rubber emulsion, etc.

[0038] According to the present invention, the pre-sizing agent has a wetting time of ≤10 seconds and a viscosity of ≤35 centipoise at 25°C.

[0039] According to the present invention, in the pre-sizing agent, the mass ratio of the epoxy resin to the polyether polyurethane is 1:0.5-1.

[0040] In the present invention, the mass ratio of the epoxy resin and the polyether polyurethane satisfies the above range, so that the wetting time and the viscosity of the pre-sizing agent at 25°C can meet the requirements, further improve the hydrophilicity and two-phase coupling of the pre-sizing agent, improve the wear resistance and temperature resistance of the sized carbon fibers, and further enhance the bonding force between the sized carbon fibers and the rubber matrix.

[0041] Furthermore, in the pre-sizing agent, the mass ratio of the epoxy resin to the polyether polyurethane is 1:0.6-0.8.

[0042] According to the present invention, the number average molecular weight of the polyether polyurethane is 800-10000 g / mol, preferably 2000-6000 g / mol.

[0043] According to the present invention, the polyether polyurethane comprises a structural unit A provided by polyisocyanate and a structural unit B provided by polyether polyol.

[0044] Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:1.

[0045] Furthermore, the polyisocyanate is an aromatic polyisocyanate.

[0046] In the present invention, the polyisocyanate is selected from aromatic polyisocyanates, compared with aliphatic polyisocyanates, so that the prepared polyether polyurethane can further improve the bonding force between the sized carbon fiber and the rubber matrix when applied to the pre-sizing agent and used in combination with the RFL emulsion.

[0047] In the present invention, the aromatic polyisocyanate is selected from toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), polymethylene polyphenyl isocyanate (PAPI), etc., preferably at least one of toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI).

[0048] In the present invention, the polyether polyol is not particularly limited, and may be, for example, a random block polyether polyol prepared by using a polyhydroxy compound, a primary amino compound or an alcohol amine as an initiator and an epoxy compound such as propylene oxide or ethylene oxide as a polymerization monomer.

[0049] Furthermore, the polymerizable monomer is preferably ethylene oxide and / or propylene oxide.

[0050] In the present invention, the polyether polyol can be obtained commercially.

[0051] According to the present invention, the pre-drying temperature is 70-110°C.

[0052] In the present invention, the inventors have found that when the pre-drying temperature is too low, the drying time is too long and the dehydration efficiency is low; when the pre-drying temperature is too high, it is easy to cause too fast dehydration and the moisture content is difficult to control. The pre-dried carbon fiber can retain appropriate moisture to promote the rapid spreading and penetration of the subsequent RFL emulsion.

[0053] Furthermore, the pre-drying temperature is 80-100°C.

[0054] According to the present invention, the temperature of the secondary drying is 100-250°C, preferably 150-200°C.

[0055] According to the present invention, in the RFL emulsion, the molar ratio of resorcinol to formaldehyde is 1:1-20, preferably 1:5-15.

[0056] According to the present invention, based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%.

[0057] In the present invention, if the pre-sizing amount of the pre-sizing agent is too small, the coupling effect of improving the interface cannot be achieved; if the pre-sizing amount is too large, the fiber bundling and fiber opening ability will be affected.

[0058] Furthermore, based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.5-20wt%.

[0059] According to the present invention, based on the mass of the carbon fiber, the sizing amount of the RFL emulsion is 5-35wt%.

[0060] In the present invention, when the sizing amount of the RFL emulsion is less than 5wt%, the adhesion between the sized carbon fiber and the rubber matrix is ​​insufficient; when it exceeds 35wt%, the post-processing of the sized fiber will be difficult and the fatigue resistance will be reduced.

[0061] Furthermore, based on the mass of the carbon fiber, the sizing amount of the RFL emulsion is 10-20wt%.

[0062] The second aspect of the present invention provides a sized carbon fiber prepared by the method for preparing sized carbon fiber using a polyether polyurethane pre-sizing agent as described in the first aspect of the present invention.

[0063] The third aspect of the present invention provides a method for preparing sized carbon fibers using a polyether polyurethane pre-sizing agent as described in the first aspect of the present invention, and application of the sized carbon fibers as described in the second aspect of the present invention in rubber materials.

[0064] In the present invention, when the sized carbon fiber is used in a rubber material to prepare a reinforced rubber composite material, the content of the sized carbon fiber in the reinforced rubber composite material is 15-30wt%.

[0065] In the present invention, the reinforced rubber composite material may further contain zinc oxide, stearic acid, carbon black N330, accelerator DM, accelerator TMTD and sulfur.

[0066] In the present invention, there is no particular limitation on the rubber material, and it may be, for example, acrylic rubber, acrylonitrile-butadiene rubber, isoprene rubber, polyurethane rubber, ethylene-propylene rubber, chloroprene rubber, silicone rubber, hydrogenated nitrile rubber, styrene-butadiene rubber, polysulfide rubber, natural rubber, butadiene rubber, or butyl rubber, and is preferably of the same type as the rubber emulsion in the RFL emulsion described in the present invention.

[0067] The present invention will be described in detail below through examples. In the following examples, each parameter is obtained by the following method.

[0068] Wetting time: The pre-sizing agent was evenly coated on the glass slide, placed at room temperature for 12 hours, and then dried at 50°C to obtain a film sample. Using the OCA20 high-speed contact angle meter, 3 microliters of deionized water was dropped onto the surface of the glass slide, and the time required for the water drop to completely wet the surface was recorded. Complete wetting was measured when the contact angle was 0.

[0069] Viscosity: The pre-sizing agent was diluted to a concentration of 2 wt %, and the viscosity was tested using a rotational viscometer at a temperature of 25° C. and a torque range of 30-70%.

[0070] Adhesion: The sizing carbon fiber is buried in an unvulcanized natural rubber block (wherein the mass of the sizing carbon fiber is 20% of the mass of the natural rubber block), and vulcanized at 140°C, 40 minutes, and a stamping pressure of 3MPa. The vulcanization formula system includes 100 parts of natural rubber, 4 parts of zinc oxide, 1.5 parts of stearic acid, 15 parts of carbon black N330, 1.2 parts of accelerator DM, 0.2 parts of accelerator TMTD, and 3 parts of sulfur. On a universal strength tester, the sizing carbon fiber is pulled out at a speed of 200mm / min. The tension required to pull out a length of 1 cm is the adhesion between the fiber and the rubber.

[0071] Sizing amount: Weigh the mass of carbon fiber before and after sizing, and calculate the sizing amount according to the formula: Sizing amount % = (mass of carbon fiber after sizing - mass of carbon fiber before sizing) / mass of carbon fiber before sizing × 100%.

[0072] Abrasion times: The TM200H yarn abrasion tester is used to test the number of times the sized carbon fiber is rubbed until it breaks.

[0073] Temperature resistance: Take an appropriate amount of sizing carbon fiber and test the weight loss rate in the range of room temperature-300°C using a TGA thermogravimetric analyzer under a nitrogen atmosphere (weight loss rate % = loss weight / sizing agent weight × 100%). The temperature corresponding to 5wt% weight loss rate is used as the temperature resistance index.

[0074] Polyether polyurethane was purchased from Shanghai Institute of Organic Chemistry, Chinese Academy of Sciences, with the brands SiPu350, SiPu380, SiPu440, SiPu205, and SiPu280;

[0075] KTM-1 epoxy emulsion sizing agent, purchased from Sinopharm Reagent;

[0076] SS-1T epoxy emulsion sizing agent was purchased from Sinopharm Reagent.

[0077] Examples 1-6

[0078] A quantitative epoxy resin, a surfactant, a polyether polyurethane, an antioxidant, and a lubricant are put into a reaction kettle, and an appropriate amount of deionized water is added, and a uniformly distributed stable emulsion is prepared by high-speed stirring and phase inversion emulsification, which is a pre-sizing agent. The components and amounts of the pre-sizing agent are shown in Table 1, and the infiltration time of the obtained pre-sizing agent is shown in Table 2.

[0079] Among them, the brands of epoxy resin are: 6420, 6421, 6445, E21, E44, E51;

[0080] The surfactants are: fatty acid polyoxyethylene ester A110, polyethylene glycol PEG-1000, polyoxyethylene sorbitan fatty acid ester T-40, polypropylene glycol PPG-8000, fatty alcohol polyoxyethylene ether AEO-20, allyl polyethylene glycol APEG2400;

[0081] The lubricant is dimethyl phthalate DMP;

[0082] The grades of polyether polyurethane are: SiPu350 (number average molecular weight is 3770g / mol), SiPu380 (number average molecular weight is 4850g / mol), SiPu440 (number average molecular weight is 5780g / mol), SiPu205 (number average molecular weight is 2250g / mol), SiPu280 (number average molecular weight is 3120g / mol), and SiPu602 (number average molecular weight is 7420g / mol).

[0083] In the first reactor equipped with a stirrer and a temperature control device, 10g of sodium hydroxide and a certain amount of resorcinol were added, and then 90g of water was added, stirred and heated to 35°C, and a certain amount of formaldehyde was slowly added, wherein the total amount of resorcinol and formaldehyde was 30g. After reacting for 3 hours, the temperature was slowly lowered to obtain a resin prepolymer; in the second reactor, 97g of natural rubber latex was added, stirred and heated to 35°C, and the synthesized resin prepolymer was slowly added dropwise, and the reaction continued for 20 hours, and the temperature was slowly lowered to obtain an RFL emulsion. The molar ratio of resorcinol to formaldehyde in the RFL emulsion is shown in Table 2.

[0084] The unsized carbon fiber is pre-sized in the first sizing tank filled with a certain viscosity dilution of the above-mentioned pre-sizing agent (specific viscosity see Table 2), and then dried at a set drying temperature for 2 minutes; then secondary sizing is performed in the second sizing tank filled with a certain viscosity dilution of the above-mentioned RFL emulsion (specific viscosity see Table 2), and then dried at a set temperature for 3 minutes, and the sized carbon fiber for reinforcing rubber composite materials is prepared after winding and collecting. The pre-sizing amount and pre-drying temperature, the secondary sizing amount and the secondary drying temperature are shown in Table 2.

[0085] Comparative Example 1

[0086] The unsized carbon fiber was sized with commercially available KTM-1M epoxy emulsion sizing agent, with a sizing amount of 5 wt %, a drying temperature of 110° C., and winding to obtain sized carbon fiber.

[0087] Comparative Example 2

[0088] The RFL emulsion in Example 2 was used to size the carbon fiber, with a sizing amount of 10 wt % and a drying temperature of 160° C. The sizing carbon fiber was prepared by winding and collecting.

[0089] Comparative Example 3

[0090] The unsized carbon fibers were pre-sized using a commercially available SS-1T epoxy emulsion sizing agent with a sizing amount of 5 wt% and a pre-drying temperature of 90°C to obtain initial carbon fibers. The initial carbon fibers were then secondary-sized and secondary-dried using the RFL emulsion in Example 2 with a sizing amount of 10 wt% and a secondary drying temperature of 180°C, and the sized carbon fibers were prepared by winding and collecting.

[0091] Table 1

[0092]

[0093] Table 2

[0094]

[0095] Test Case

[0096] The sized carbon fibers prepared in the examples and comparative examples were tested for wear resistance, high temperature resistance and adhesion. The results are shown in Table 3.

[0097] Table 3

[0098]

[0099] From the results in Table 3, it can be seen that in Comparative Example 1, only the traditional epoxy resin emulsion is used, and in Comparative Example 2, only the RFL emulsion is used. The bonding force between the prepared carbon fiber and the rubber matrix is ​​low, and the wear resistance is low. The commercially available SS-1T epoxy emulsion used in Comparative Example 3 has a too long soaking time and too high viscosity, and the improvement effect is not obvious.

[0100] In Examples 1-6, a pre-sizing agent with epoxy resin and polyether polyurethane resin emulsion as the main body, a wetting time ≤ 25 seconds and a viscosity ≤ 45 centipoise at 25°C is introduced in the pre-sizing process, and an RFL emulsion sizing agent with good affinity to the rubber matrix is ​​used in the secondary sizing process. The prepared sized carbon fibers have high temperature resistance (not less than 250°C), significantly increased bonding strength with the rubber matrix (not less than 150N), and improved wear resistance (not less than 4000 times).

[0101] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing sized carbon fiber using a polyether polyurethane pre-sizing agent, characterized in that: The method comprises: S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing polyether polyurethane and epoxy resin to obtain initial carbon fiber; S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber; The pre-sizing agent has a wetting time of ≤25 seconds and a viscosity of ≤45 centipoise at 25°C.

2. The method according to claim 1, wherein: The pre-sizing agent has a wetting time of ≤10 seconds and a viscosity of ≤35 centipoise at 25°C.

3. The method according to claim 1 or 2, wherein: In the pre-sizing agent, the mass ratio of the epoxy resin to the polyether polyurethane is 1:0.5-1, preferably 1:0.6-0.

8.

4. The method according to claim 3, wherein: The number average molecular weight of the polyether polyurethane is 800-10000 g / mol, preferably 2000-6000 g / mol.

5. The method according to any one of claims 1 to 4, wherein: The polyether polyurethane comprises a structural unit A provided by a polyisocyanate and a structural unit B provided by a polyether polyol; Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:1; Preferably, the polyisocyanate is an aromatic polyisocyanate.

6. The method according to any one of claims 1 to 5, wherein: The pre-drying temperature is 70-110°C, preferably 80-100°C; Preferably, the secondary drying temperature is 100-250°C, preferably 150-200°C.

7. The method according to any one of claims 1 to 6, wherein: In the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:1-20, preferably 1:5-15.

8. The method according to any one of claims 1 to 7, wherein: Based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%; Preferably, based on the mass of the carbon fiber, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%, preferably 10-20wt%.

9. Sized carbon fiber prepared by the method for preparing sized carbon fiber using a polyether polyurethane pre-sizing agent as described in any one of claims 1 to 8.

10. The method for preparing sized carbon fiber by using a polyether polyurethane pre-sizing agent as described in any one of claims 1 to 8, and the use of the sized carbon fiber as described in claim 9 in rubber materials.

Citation Information

Patent Citations

  • Preparation method for carbon fiber enhanced rubber composite material

    CN107459682A