Method for preparing sizing carbon fiber by using aromatic polyamide-containing pre-sizing agent, application of sizing carbon fiber, sizing carbon fiber and application of sizing carbon fiber

By using a pre-sizing agent containing aramid and epoxy resin on carbon fiber and a secondary sizing treatment of resorcinol formaldehyde latex on carbon fiber, the problem of poor bonding between carbon fiber and rubber matrix is ​​solved, and the material is significantly improved Impact toughness and temperature resistance have achieved higher industrial application prospects.

CN118932728APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310536586.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The poor surface interface performance of carbon fiber and rubber matrix leads to poor load transfer, affecting the product's mechanical strength, toughness and fatigue resistance. The existing sizing treatment methods are complex and have poor results.

Method used

The carbon fiber is pre-sizing and pre-dryed with a pre-sizing agent containing aromatic polyamide and epoxy resin, followed by secondary sizing and secondary drying with resorcinol formaldehyde latex, controlled infiltration time ≤22 seconds and viscosity ≤ 65 centipoise to improve the adhesion and temperature resistance of carbon fiber to rubber matrix.

Benefits of technology

It significantly improves the impact toughness and temperature resistance of sizing carbon fiber and rubber composite materials, and the compression strength after impact reaches more than 400MPa, high temperature resistance reaches more than 250℃, and simplifies the sizing process, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004226498100000111
    Figure BDA0004226498100000111
  • Figure BDA0004226498100000112
    Figure BDA0004226498100000112
  • Figure BDA0004226498100000121
    Figure BDA0004226498100000121
Patent Text Reader

Abstract

The invention relates to the field of carbon fiber sizing agents, and discloses a method for preparing sizing carbon fibers by using an aromatic polyamide-containing pre-sizing agent, application of the sizing carbon fibers, the sizing carbon fibers and application of the sizing carbon fibers. The method comprises the following steps: S1, carrying out pre-sizing and pre-drying on carbon fibers by adopting a pre-sizing agent containing aromatic polyamide and epoxy resin to obtain initial carbon fibers; s2, carrying out secondary sizing and secondary drying on the initial carbon fiber by adopting resorcinol formaldehyde latex to obtain sized carbon fiber; the infiltration time of the pre-sizing agent is less than or equal to 22 seconds, and the viscosity at 25 DEG C is less than or equal to 65 centipoises. The aromatic polyamide contained in the pre-sizing agent can effectively relieve stress concentration of multiple interface phases after sizing carbon fibers are thermally cured, the impact toughness of a sizing carbon fiber-rubber composite material product is improved, meanwhile, excellent binding power is achieved between the sizing carbon fibers and a rubber matrix, and the sizing carbon fibers have good temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of carbon fiber sizing agents, and in particular to a method for preparing sized carbon fibers by utilizing a pre-sizing agent containing aromatic polyamide and its application, and the sized carbon fibers and their application. Background Art

[0002] Carbon fiber has excellent comprehensive properties and thermal properties such as high specific strength, high modulus, high thermal conductivity, chemical corrosion resistance, and radiation resistance. It is a new type of high-performance composite material reinforcement. Compared with carbon fiber reinforced resin-based composite materials, carbon fiber reinforced rubber-based composite materials are more excellent in toughness, elasticity, fatigue resistance, etc., and have the prospect of being widely used in transportation equipment, industrial parts, sporting goods, energy and chemical industries. However, the surface and interface properties of carbon fiber and rubber matrix are very different, and it is difficult to effectively combine them into a solid integrated material, resulting in poor load transfer and the inability to effectively play the reinforcing role of the fiber. The mechanical strength, toughness and other properties of the product are affected.

[0003] CN110527150A applies for a fiber-reinforced rubber V-belt and a preparation method thereof, wherein a reinforcement system such as N660 and N330 is mainly used to improve the lateral rigidity, but no method of improving the rigidity by sizing the fiber surface is mentioned.

[0004] CN111484654A discloses a thermally conductive rubber material, in which carbon fibers are first treated with a silane coupling agent and then treated with CO2 plasma etching, and combined with pretreated hexagonal boron nitride powder and pretreated nanopowder to improve the thermal conductivity and mechanical properties of the rubber material. This technical solution can improve the interface bonding between the carbon fibers and the rubber material to a certain extent, but the treatment process is complicated, the industrialization degree of plasma etching is low, continuous production is not possible, the cost of the formula powder is high, and it is difficult to apply it on an online scale. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems that the sizing carbon fiber processing method in the prior art is complicated and the mechanical properties, temperature resistance and fatigue resistance of the obtained sizing carbon fiber are poor. A method and application of preparing sizing carbon fiber by using a pre-sizing agent containing aromatic polyamide, sizing carbon fiber and application are provided. The method is simple to operate. A layer of pre-sizing agent containing aromatic polyamide and epoxy resin is coated on the surface of the carbon fiber and pre-dried, and then resorcinol formaldehyde latex (hereinafter referred to as RFL emulsion) is used for secondary sizing and secondary drying. Due to the presence of aromatic polyamide in the pre-sizing agent, the wetting and spreading of the two-phase interface can be significantly improved, and the stress concentration after thermal curing of the sizing carbon fiber can be effectively alleviated. When used for rubber materials, the toughness of the sizing carbon fiber-rubber composite material can be improved, the occurrence of cracks can be alleviated, and the impact toughness of the sizing carbon fiber-rubber composite material product is further improved. At the same time, the sizing carbon fiber and the rubber matrix have excellent bonding force and good temperature resistance.

[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing sized carbon fiber using a pre-sizing agent containing aromatic polyamide, wherein the method comprises:

[0007] S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing aromatic polyamide and epoxy resin to obtain initial carbon fiber;

[0008] S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber;

[0009] The pre-sizing agent has a wetting time of ≤22 seconds and a viscosity of ≤65 centipoise at 25°C.

[0010] The second aspect of the present invention provides a sized carbon fiber prepared by the method described in the first aspect of the present invention.

[0011] The third aspect of the present invention provides an application of the method described in the first aspect of the present invention and the sized carbon fiber described in the second aspect of the present invention in a rubber material.

[0012] Through the above technical scheme, the method and application of preparing sized carbon fiber using aromatic polyamide pre-sizing agent, and the sized carbon fiber and application provided by the present invention achieve the following beneficial effects:

[0013] (1) The present invention uses epoxy resin and aromatic polyamide as the main components in the pre-sizing agent, and adopts an RFL emulsion sizing agent with good affinity to the rubber matrix in the secondary sizing process, which can significantly enhance the bonding force between the sized carbon fiber and the rubber matrix, improve the impact toughness of the prepared sized carbon fiber-rubber composite material, and the post-impact compressive strength can reach more than 400 MPa.

[0014] (2) The present invention utilizes a pre-sizing agent and an RFL emulsion to perform pre-sizing and secondary sizing on carbon fibers, respectively. When the obtained sized carbon fibers are applied to rubber materials, the bonding strength between the prepared sized carbon fibers and the rubber matrix can be significantly improved (can reach more than 150N), while the temperature resistance of the sized carbon fibers can be improved, reaching a high temperature resistance of more than 250°C.

[0015] (3) The present invention controls the wetting time of the pre-sizing agent to be ≤22 seconds, the viscosity at 25°C to be ≤65 centipoise, and uses specific pre-sizing and secondary sizing processes to ultimately prepare sized carbon fibers having high temperature resistance and excellent bonding strength with the rubber matrix, thereby improving the impact toughness of the sized carbon fiber-rubber composite material and breaking through the bottleneck limitations of the sized carbon fiber-rubber composite material in terms of high-temperature processing, interface bonding, and impact toughness.

[0016] (4) The method of the present invention is simple in process, highly stable, safe and pollution-free, and can be completed using an existing carbon fiber preparation production line, thus having broad industrial prospects. DETAILED DESCRIPTION

[0017] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0018] A first aspect of the present invention provides a method for preparing sized carbon fiber using a pre-sizing agent containing aromatic polyamide, the method comprising:

[0019] S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing aromatic polyamide and epoxy resin to obtain initial carbon fiber;

[0020] S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber;

[0021] The pre-sizing agent has a wetting time of ≤22 seconds and a viscosity of ≤65 centipoise at 25°C.

[0022] The inventors discovered that the RFL emulsion sizing agent commonly used in the prior art is an aqueous emulsion, which is easy to poorly infiltrate and spread on the surface of the carbon fiber, resulting in discontinuous and loose bonding points, resulting in weak bonding ability with the carbon fiber surface. The use of RFL emulsion alone cannot effectively improve the bonding strength between the carbon fiber and the rubber matrix after sizing, nor can it effectively improve the impact toughness, temperature resistance and bonding strength of the sized carbon fiber-rubber composite material with the rubber matrix.

[0023] In the present invention, the inventors have found that by pre-coating a layer of pre-sizing agent containing aromatic polyamide and epoxy resin on the surface of carbon fiber, and then performing secondary sizing on it with RFL emulsion, the RFL emulsion can be quickly spread and infiltrated on the surface of carbon fiber coated with the pre-sizing agent. At the same time, the introduction of aromatic polyamide in the pre-sizing agent can significantly improve the infiltration and spreading of the two-phase interface. When the sized carbon fiber is applied to the rubber material, the stress concentration of the multi-interface phase after the thermal curing of the sized carbon fiber can be effectively alleviated, and the impact toughness of the sized carbon fiber-rubber composite material can be improved. At the same time, the sized carbon fiber and the rubber matrix have excellent bonding force and good temperature resistance.

[0024] In the present invention, further research results show that only when the pre-sizing agent has an infiltration time of ≤22 seconds and a viscosity of ≤65 centipoise at 25°C, can the secondary uniform infiltration of the RFL emulsion be achieved, and can a good coupling enhancement effect be achieved in the carbon fiber and the RFL emulsion. When the infiltration time is greater than 22 seconds, the hydrophilicity is insufficient, and the binding ability of the pre-sizing agent with the carbon fiber and the RFL emulsion is insufficient, and the coupling enhancement effect cannot be achieved. When the viscosity at 25°C is greater than 65 centipoise, the expansion of the pre-sizing agent on the surface of the carbon fiber is greatly hindered, and it cannot be evenly infiltrated and spread, which makes it easy to form regional defects at the intermediate phase interface, and produce stress concentration after later curing, thereby reducing the mechanical properties, impact toughness, fatigue resistance and other comprehensive properties of the sized carbon fiber-rubber composite material.

[0025] In the present invention, the epoxy resin is a glycidyl ether epoxy resin containing two or more epoxy groups in the molecule, for example, it may be at least one of bisphenol A, bisphenol F, and bisphenol S.

[0026] In the present invention, the epoxy equivalent of the epoxy resin is 160-6000.

[0027] In the present invention, the epoxy equivalent of the epoxy resin satisfies the above range, so that the wetting time and viscosity of the prepared pre-sizing agent at 25° C. can meet the requirements.

[0028] In the present invention, the pre-sizing agent may further contain components such as antioxidants, lubricants, surfactants, etc. The surfactant is preferably a non-ionic surfactant.

[0029] According to a preferred embodiment of the present invention, the nonionic surfactant is selected from at least one of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyoxyethylene amine, polyoxyethylene amide, sorbitan ester and fluorocarbon surfactant.

[0030] In the present invention, there is no particular limitation on the types and contents of the antioxidant, lubricant and surfactant contained in the pre-sizing agent, and they can be adjusted according to the needs in the art.

[0031] According to a particularly preferred embodiment of the present invention, the pre-sizing agent contains 40-60 parts of epoxy resin, 5-30 parts of aromatic polyamide, 1-5 parts of antioxidant, 1-5 parts of lubricant and 15-45 parts of surfactant. When each component meets the above range, when the pre-sizing agent is applied to sized carbon fiber, the prepared sized carbon fiber-rubber composite material has more excellent comprehensive properties.

[0032] In the present invention, the epoxy resin, antioxidant, lubricant and surfactant may be provided in the form of an epoxy resin aqueous emulsion.

[0033] In the present invention, the epoxy resin, antioxidant, lubricant and surfactant are configured into an epoxy resin aqueous emulsion for addition, and further combined with the RFL emulsion to improve the synergistic effect between the components, significantly improve the bonding force between the sized carbon fiber and the rubber matrix, and the sized carbon fiber has good temperature resistance. At the same time, when the sized carbon fiber is applied to a rubber material, the sized carbon fiber-rubber composite material obtained has good impact toughness.

[0034] In the present invention, the preparation method of the pre-sizing agent in step S1 can adopt the preparation method of the emulsion generally used in the art, such as phase inversion emulsification method, ultrasonic emulsification method and colloid mill emulsification method.

[0035] In the present invention, the RFL emulsion is a mixed emulsion formed by the reaction of resorcinol, formaldehyde and rubber emulsion. The specific preparation process is: sodium hydroxide and resorcinol are added to the first reaction kettle, and then an appropriate amount of water is added, the temperature is controlled to 20-40°C, and then formaldehyde is slowly added, and a prepolymer is obtained after aging reaction for 2-4 hours; rubber latex is added to the second reaction kettle, the temperature is controlled to 20-40°C, and the synthesized prepolymer is slowly added dropwise, and the reaction is continued for 10-30 hours to finally prepare the RFL emulsion.

[0036] In the present invention, the rubber emulsion in the RFL emulsion can be acrylic rubber emulsion, acrylonitrile-butadiene rubber emulsion, isoprene rubber emulsion, polyurethane rubber emulsion, ethylene-propylene rubber emulsion, chloroprene rubber emulsion, silicone rubber emulsion, hydrogenated nitrile rubber emulsion, styrene-butadiene rubber emulsion, polysulfide rubber emulsion, natural rubber emulsion, butadiene rubber emulsion and butyl rubber emulsion, etc.

[0037] According to the present invention, the pre-sizing agent has a wetting time of ≤10 seconds and a viscosity of ≤30 centipoise at 25°C.

[0038] According to the present invention, the average particle size of the aromatic polyamide is ≤0.7 micrometer.

[0039] In the present invention, the average particle size of the aromatic polyamide meets the above range, which can ensure that the pre-sizing agent is infiltrated and spread on the surface of the carbon fiber, thereby improving its effect on the coupling of the carbon fiber and the RFL emulsion.

[0040] Furthermore, the average particle size of the aromatic polyamide is ≤0.5 micrometer.

[0041] According to the present invention, in the pre-sizing agent, the mass ratio of the epoxy resin to the aromatic polyamide is 1:0.1-0.5.

[0042] In the present invention, the mass ratio of the epoxy resin and the aromatic polyamide satisfies the above range, so that the wetting time and the viscosity of the pre-sizing agent at 25°C can meet the requirements, further improve the hydrophilicity and coupling of the pre-sizing agent, improve the temperature resistance of the sized carbon fiber, and further enhance the bonding force between the sized carbon fiber and the rubber matrix.

[0043] Furthermore, in the pre-sizing agent, the mass ratio of the epoxy resin to the aromatic polyamide is 1:0.2-0.3.

[0044] According to the present invention, the number average molecular weight of the aromatic polyamide is 5000-35000 g / mol, preferably 10000-20000 g / mol.

[0045] According to the present invention, the aromatic polyamide includes a structural unit A provided by a diamine and a structural unit B provided by an aromatic dibasic acid.

[0046] In the present invention, compared with aliphatic polyamide, when the aromatic polyamide is added to the pre-sizing agent and used in combination with the RFL emulsion, the bonding force between the sized carbon fiber and the rubber matrix can be further improved.

[0047] In the present invention, the diamine can be commercially available, for example, it can be at least one of ethylenediamine, m-phenylenediamine, p-phenylenediamine, hexamethylenediamine, and decanediamine.

[0048] In the present invention, the aromatic dibasic acid can be commercially available, for example, phthalic acid, isophthalic acid, and terephthalic acid.

[0049] In the present invention, “the aromatic polyamide includes a structural unit A provided by a diamine and a structural unit B provided by an aromatic dibasic acid” means that the aromatic polyamide is prepared by condensation polymerization of a diamine and an aromatic dibasic acid.

[0050] According to the present invention, the molar ratio of the structural unit A to the structural unit B is 1-2:1.

[0051] In the present invention, the aromatic polyamide can be obtained commercially.

[0052] According to the present invention, the pre-drying temperature is 70-110°C.

[0053] In the present invention, the inventors have found that when the pre-drying temperature is too low, the drying time is too long and the dehydration efficiency is low; when the pre-drying temperature is too high, it is easy to cause too fast dehydration and the moisture content is difficult to control. When the pre-drying temperature meets the above range, the carbon fiber after pre-drying can retain appropriate moisture to promote the rapid spreading and penetration of the subsequent RFL emulsion.

[0054] Furthermore, the pre-drying temperature is 80-100°C.

[0055] According to the present invention, the temperature of the secondary drying is 100-250°C, preferably 150-200°C.

[0056] According to the present invention, in the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:1-20, preferably 1:5-15.

[0057] According to the present invention, based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%.

[0058] In the present invention, if the pre-sizing amount of the pre-sizing agent is too small, the coupling effect of improving the interface cannot be achieved; if the pre-sizing amount is too large, the fiber bundling and fiber opening ability will be affected.

[0059] Furthermore, based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.5-20wt%.

[0060] According to the present invention, based on the mass of the carbon fiber, the sizing amount of the RFL emulsion is 5-35wt%.

[0061] In the present invention, when the sizing amount of the RFL emulsion is less than 5wt%, the adhesion between the sized carbon fiber and the rubber matrix is ​​insufficient; when it exceeds 35wt%, the post-processing of the sized fiber will be difficult and the fatigue resistance will be reduced.

[0062] Furthermore, based on the mass of the carbon fiber, the sizing amount of the RFL emulsion is 10-20wt%.

[0063] The second aspect of the present invention provides a sized carbon fiber prepared by the method described in the first aspect of the present invention.

[0064] The third aspect of the present invention provides an application of the method described in the first aspect of the present invention and the sized carbon fiber described in the second aspect of the present invention in a rubber material.

[0065] In the present invention, when the sized carbon fiber is used in a rubber material to prepare a reinforced rubber composite material, the content of the sized carbon fiber in the reinforced rubber composite material is 15-30wt%.

[0066] In the present invention, the reinforced rubber composite material may further contain zinc oxide, stearic acid, carbon black N330, accelerator DM, accelerator TMTD and sulfur.

[0067] In the present invention, there is no particular limitation on the rubber material, and it may be, for example, acrylic rubber, acrylonitrile-butadiene rubber, isoprene rubber, polyurethane rubber, ethylene-propylene rubber, chloroprene rubber, silicone rubber, hydrogenated nitrile rubber, styrene-butadiene rubber, polysulfide rubber, natural rubber, butadiene rubber, or butyl rubber, and is preferably of the same type as the rubber emulsion in the RFL emulsion described in the present invention.

[0068] The present invention will be described in detail below through examples. In the following examples, each parameter is obtained by the following method.

[0069] Wetting time: The pre-sizing agent was evenly coated on the glass slide, placed at room temperature for 12 hours, and then dried at 50°C to obtain a film sample. Using the OCA20 high-speed contact angle meter, 3 microliters of deionized water was dropped onto the surface of the glass slide, and the time required for the water drop to completely wet the surface was recorded. Complete wetting was measured when the contact angle was 0.

[0070] Viscosity: The pre-sizing agent was diluted to a concentration of 2 wt %, and the viscosity was tested using a rotational viscometer at a temperature of 25° C. and a torque range of 30-70%.

[0071] Adhesion: The sizing carbon fiber is buried in an unvulcanized natural rubber block (wherein the mass of the sizing carbon fiber is 20% of the mass of the natural rubber block), and vulcanized at 140°C, 40 minutes, and a stamping pressure of 3MPa. The vulcanization formula system includes 100 parts of natural rubber, 4 parts of zinc oxide, 1.5 parts of stearic acid, 15 parts of carbon black N330, 1.2 parts of accelerator DM, 0.2 parts of accelerator TMTD, and 3 parts of sulfur. On a universal strength tester, the sizing carbon fiber is pulled out at a speed of 200mm / min. The tension required to pull out a length of 1 cm is the adhesion between the fiber and the rubber.

[0072] Sizing amount: Weigh the mass of carbon fiber before and after sizing, and calculate the sizing amount according to the formula: Sizing amount % = (mass of carbon fiber after sizing - mass of carbon fiber before sizing) / mass of carbon fiber before sizing × 100%.

[0073] Temperature resistance: Take an appropriate amount of sizing carbon fiber and test the weight loss rate in the range of room temperature-300°C using a TGA thermogravimetric analyzer under a nitrogen atmosphere (weight loss rate % = loss weight / sizing agent weight × 100%). The temperature corresponding to 5wt% weight loss rate is used as the temperature resistance index.

[0074] Compression strength after impact: Referring to SACMA SRM 2R-94 standard, a 6.7 J / mm drop hammer impact is applied to the center of the sized carbon fiber-rubber composite sample to calculate the compression strength after impact.

[0075] Aromatic polyamide, purchased from Shanghai Institute of Organic Chemistry, Chinese Academy of Sciences, brand RI925, RI930;

[0076] KTM-4 epoxy emulsion, purchased from Sinopharm Reagent;

[0077] SS-3A epoxy emulsion was purchased from Sinopharm Reagent.

[0078] Examples 1-6

[0079] A quantitative epoxy resin, a surfactant, an aromatic polyamide, an antioxidant, and a lubricant are put into a reaction kettle, and an appropriate amount of deionized water is added, and a uniformly distributed stable emulsion is prepared by high-speed stirring and phase inversion emulsification, which is a pre-sizing agent. The components and amounts of the pre-sizing agent are shown in Table 1, and the infiltration time of the obtained pre-sizing agent is shown in Table 2.

[0080] Among them, the brands of epoxy resin are: E44, E20, E51, 6445, 6276, 6263;

[0081] The surfactants are: alkylphenol polyoxyethylene ether APEO-9, polyethylene glycol PEG-2000, fatty amine polyoxyethylene ether AC-1215, polyoxyethylene sorbitan fatty acid ester T-60, sorbitan fatty acid ester S-80, fatty acid polyoxyethylene ester A115;

[0082] The lubricant is diisononyl phthalate DINP;

[0083] The grades of aromatic polyamide are: RI925 (number average molecular weight is 15000) and RI930 (number average molecular weight is 20000).

[0084] In the first reactor equipped with a stirrer and a temperature control device, 10g of sodium hydroxide and a certain amount of resorcinol were added, and then 90g of water was added, stirred and heated to 35°C, and a certain amount of formaldehyde was slowly added, wherein the total amount of resorcinol and formaldehyde was 30g. After reacting for 3 hours, the temperature was slowly lowered to obtain a resin prepolymer; in the second reactor, 97g of natural rubber latex was added, stirred and heated to 35°C, and the synthesized resin prepolymer was slowly added dropwise, and the reaction continued for 20 hours, and the temperature was slowly lowered to obtain an RFL emulsion. The molar ratio of resorcinol to formaldehyde in the RFL emulsion is shown in Table 2.

[0085] The unsized carbon fiber is pre-sized in the first sizing tank filled with a certain viscosity dilution of the above-mentioned pre-sizing agent (specific viscosity see Table 2), and then dried at a set drying temperature for 2 minutes; then secondary sizing is performed in the second sizing tank filled with a certain viscosity dilution of the above-mentioned RFL emulsion (specific viscosity see Table 2), and then dried at a set temperature for 3 minutes, and the sized carbon fiber for reinforcing rubber composite materials is prepared after winding and collecting. The pre-sizing amount and pre-drying temperature, the secondary sizing amount and the secondary drying temperature are shown in Table 2.

[0086] Comparative Example 1

[0087] The unsized carbon fiber was sized with a commercially available KTM-4 epoxy emulsion sizing agent, with a sizing amount of 5 wt %, a drying temperature of 110° C., and winding to obtain the sized carbon fiber.

[0088] Comparative Example 2

[0089] The RFL emulsion in Example 1 was used to impregnate and size the unsized carbon fiber, with a sizing amount of 10 wt % and a drying temperature of 160° C. to prepare the sized carbon fiber by winding and collecting.

[0090] Comparative Example 3

[0091] The unsized carbon fiber was pre-sized using a commercially available SS-3A epoxy emulsion sizing agent with a sizing amount of 5wt% and a drying temperature of 90°C. The carbon fiber was then secondary-sized using the RFL emulsion in Example 1 with a sizing amount of 10wt% and a drying temperature of 180°C, and the sized carbon fiber was prepared by winding and collecting.

[0092] Table 1

[0093]

[0094] Table 2

[0095]

[0096] Test Case

[0097] The sized carbon fibers prepared in the examples and comparative examples were tested for high temperature resistance and adhesion between the sized carbon fibers and the rubber matrix. The post-impact compressive strength of the sized carbon fiber-rubber composite material was tested with reference to the SACMA SRM 2R-94 standard. The results are shown in Table 3.

[0098] Table 3

[0099]

[0100] It can be seen from the results in the table that comparative example 1 only uses traditional epoxy resin emulsion, and comparative example 2 only uses RFL emulsion. The bonding force between the prepared carbon fiber and the rubber matrix is ​​low, and the compression strength after impact is poor. The complete impregnation time of the pre-sizing epoxy emulsion used in comparative example 3 is too long, the viscosity is too large, and the improvement effect is not obvious. Examples 1-6 introduce a pre-sizing agent with epoxy resin and aromatic polyamide as the main body, an impregnation time of less than 22 seconds, and a viscosity of less than 65 centipoise at 25°C in the pre-sizing process, and use an RFL emulsion sizing agent with good affinity to the rubber matrix in the secondary sizing process. The prepared sized carbon fiber has high temperature resistance, excellent interface adhesion and stability with the rubber matrix, and has a high compression strength after impact, which can meet the application requirements of sizing carbon fiber-rubber composite materials at a higher level.

[0101] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing sized carbon fiber using a pre-sizing agent containing aromatic polyamide, characterized in that: The method comprises: S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing aromatic polyamide and epoxy resin to obtain initial carbon fiber; S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber; The pre-sizing agent has a wetting time of ≤22 seconds and a viscosity of ≤65 centipoise at 25°C.

2. The method according to claim 1, wherein: The pre-sizing agent has a wetting time of ≤10 seconds and a viscosity of ≤30 centipoise at 25°C; Preferably, the average particle size of the aromatic polyamide is ≤0.7 micron, preferably ≤0.5 micron.

3. The method according to claim 1 or 2, wherein: In the pre-sizing agent, the mass ratio of the epoxy resin to the aromatic polyamide is 1:0.1-0.5, preferably 1:0.2-0.

3.

4. The method according to any one of claims 1 to 3, wherein: The number average molecular weight of the aromatic polyamide is 5000-35000 g / mol, preferably 10000-20000 g / mol.

5. The method according to any one of claims 1 to 4, wherein: The aromatic polyamide comprises a structural unit A provided by a diamine and a structural unit B provided by an aromatic dibasic acid; Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:

1.

6. The method according to any one of claims 1 to 5, wherein: The pre-drying temperature is 70-110°C, preferably 80-100°C; Preferably, the secondary drying temperature is 100-250°C, preferably 150-200°C.

7. The method according to any one of claims 1 to 6, wherein: In the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:1-20, preferably 1:5-15.

8. The method according to any one of claims 1 to 7, wherein: Based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%; Preferably, based on the mass of the carbon fiber, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%, preferably 10-20wt%.

9. Sized carbon fiber prepared by the method according to any one of claims 1 to 8.

10. Use of the method according to any one of claims 1 to 8 and the sized carbon fiber according to claim 9 in rubber materials.

Citation Information

Cited By

  • Carbon fiber reinforced composite material for aerospace low-temperature storage tank and preparation method of carbon fiber reinforced composite material