Probiotic non-woven fabric manufacturing method

By using composite fiber mesh hot air bonding and probiotic emulsion coating technology, the problem of easy peeling of antibacterial coating is solved, thereby improving antibacterial properties and comfort, and maintaining vaginal health.

CN118932737APending Publication Date: 2024-11-12FOSHAN GOOD FEELING EISAI TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411258072.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing antibacterial nonwoven fabrics have low antibacterial coating adhesion strength, are easy to fall off, and are difficult to significantly improve vaginal health. Simply killing harmful bacteria is insufficient to maintain vaginal health.

Method used

The composite fiber mesh hot air bonding technology is used to form a microporous structure, and a probiotic emulsion is coated to form a firmly attached probiotic coating. The ethylene acrylic copolymer emulsion is combined to improve adhesion and softness.

Benefits of technology

It achieves improved antibacterial properties and comfort, with the probiotic coating adhering firmly to maintain vaginal flora balance, enhancing user comfort and antibacterial durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a probiotic non-woven fabric, and belongs to the technical field of non-woven fabrics, and the manufacturing method comprises the following steps: S1, mixing polyethylene, modified sodium bicarbonate and a dispersing agent, heating to melt, spinning, and carding into a two-layer composite fiber net; s2, the granular polyethylene particles and the granular high-melting-point resin are heated to be molten, and then spinning and mixing carding are conducted to form a bi-component fiber net; s3, laminating the composite fiber net, the bi-component fiber net and the composite fiber net, heating and bonding, and decomposing the modified sodium bicarbonate to obtain a composite non-woven fabric; s4, adding the inactivated probiotics into a protective agent to obtain a probiotic solution; s5, mixing the ethylene acrylic acid copolymer aqueous emulsion with the probiotic solution, and emulsifying to obtain a probiotic emulsion; s6, the surface of the composite non-woven fabric is coated with the probiotic emulsion, and the probiotic non-woven fabric is obtained; the probiotic non-woven fabric disclosed by the invention has good antibacterial property and can maintain bacterial colony balance of probiotics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of non-woven fabrics, and in particular to a method for preparing a probiotic non-woven fabric. Background Art

[0002] Non-woven fabrics are widely used in personal hygiene, public medical protection and other fields, such as baby diapers, sanitary napkins, medical masks, surgical gowns, surgical pads, etc. Non-woven fabrics are usually required to have good antibacterial properties in the process of application in the above fields to cope with the harm of bacteria growth to the human body during use. As people pay more and more attention to personal and public health, the antibacterial properties of non-woven fabrics are becoming more and more important. At present, antibacterial non-woven fabrics usually adopt the method of coating the surface with antibacterial agents to form antibacterial coatings to achieve good antibacterial properties. However, the fibers that make up the non-woven fabrics are usually smooth. After the antibacterial agent is coated on the surface of the non-woven fabric, it is difficult to adhere firmly and easily cause the antibacterial coating to fall off. When the antibacterial coating falls off, dust will be formed, which will affect the user's experience and affect the antibacterial properties and durability of the non-woven fabrics. In addition, women are paying more and more attention to the health of their vagina, and antibacterial non-woven fabrics are used to make sanitary napkins. When users use sanitary napkins, although the antibacterial coating can maintain vaginal health to a certain extent by killing harmful bacteria, the health of the vagina is affected by many factors. It is difficult to significantly improve the health of the vagina by simply killing harmful bacteria.

[0003] The Chinese patent with the announcement number CN108998895A discloses an antibacterial method for medical antibacterial nonwoven fabrics, which includes components A, B and C; wherein component A is composed of the following weight parts: 60-80 parts of modified polyamide and 40-60 parts of modified polyester; component B is viscose fiber; component C is composed of the following weight parts: 6-11 parts of nano-silver chitosan antibacterial agent, 5-15 parts of carboxyl styrene butadiene latex, and 80-100 parts of water; wherein the weight ratio of A, B and C is 1:3:5; the above patent uses modified polyamide , modified polyester spun filaments are mixed with viscose fibers and then soaked in a mixture of nano-silver chitosan antibacterial agent and carboxyl styrene butadiene latex, and then the antibacterial non-woven fabric is made through a self-adhesive spunlace process. Although the antibacterial non-woven fabric obtains antibacterial properties through a coating formed by nano-silver chitosan antibacterial agent and carboxyl styrene butadiene latex on the fiber surface, the strength of the coating attached to the non-woven fabric fiber surface is low and easily causes it to fall off, and the coating only has antibacterial properties. When the antibacterial non-woven fabric is used to make sanitary napkins, it is difficult for the sanitary napkins to significantly improve the health of the vagina through the antibacterial non-woven fabric, so there is still room for improvement. Summary of the invention

[0004] In view of the technical defects existing in the background technology, the present invention proposes a method for making a probiotic non-woven fabric, which solves the above technical problems and meets the actual needs. The specific technical solution is as follows: A method for making a probiotic non-woven fabric comprises the following steps: S1. After heating granular polyethylene until it is melted, adding modified sodium bicarbonate and a dispersant and stirring evenly to obtain a composite melt, the composite melt is ejected through a spinning nozzle, and then pulled, curled, dried, and cut to obtain a composite fiber; the decomposition temperature of the modified sodium bicarbonate is greater than the temperature at which the polyethylene particles are heated to melt; S2, heating the granular polyethylene particles and the granular high melting point resin to melt respectively, ejecting them through a spinning nozzle, and then pulling, curling, drying, and cutting to obtain polyethylene fibers and high melting point resin fibers respectively; S3, opening and combing the composite fibers to form a two-layer composite fiber web, mixing the polyethylene fiber and the high-melting-point resin fiber, opening and combing them to form a bicomponent fiber web, stacking the composite fiber web, the bicomponent fiber web, and the composite fiber web in sequence along the thickness direction to form a multi-layer fiber web, heating the multi-layer fiber web by hot air to make the internal fibers bond to each other, then increasing the hot air temperature until the modified sodium bicarbonate is decomposed, and cooling after the modified sodium bicarbonate is completely decomposed to obtain a composite non-woven fabric; S4, adding the inactivated probiotics into the protective agent and stirring evenly to obtain a probiotic solution; S5, dispersing the ethylene acrylic acid copolymer emulsion in deionized water to form an aqueous emulsion, heating the aqueous emulsion, mixing it with the probiotic solution and emulsifying it to obtain a probiotic emulsion; S6. Evenly apply the probiotic emulsion on the surface of the composite non-woven fabric, and then air-dry the composite non-woven fabric to obtain the probiotic non-woven fabric.

[0005] As a further technical solution of the present invention, the composite melt includes the following components in mass percentage: 97.5% to 99.88% polyethylene, 0.1% to 2% modified sodium bicarbonate, and 0.02% to 0.5% dispersant; the dispersant is selected from one or more of polyvinyl alcohol, alkanolamine, alkanolamide, and polyol fatty acid ester.

[0006] As a further technical solution of the present invention, in step S1, the polyethylene particles are heated to a melting temperature of 120-140°C, and the decomposition temperature of the modified sodium bicarbonate is 150-170°C.

[0007] As a further technical solution of the present invention, in step S3, the multilayer fiber web is first heated to melt the composite fibers and the polyethylene fibers by hot air at a temperature of 120-140°C so that the fibers inside the multilayer fiber web are bonded to each other, and then the temperature of the hot air is increased to 150-170°C to decompose the modified sodium bicarbonate to produce carbon dioxide, and the carbon dioxide escapes from the inside of the composite fibers to form a number of adsorption balloons with micropores in the composite fibers.

[0008] As a further technical solution of the present invention, the high melting point resin is selected from polypropylene resin and polyester resin; the mass ratio of polyethylene fiber to high melting point resin fiber in the bicomponent fiber web is 1:3~1:1.

[0009] As a further technical solution of the present invention, the denier of the composite fiber is 0.5~1D, the denier of the polyethylene fiber is 1~3D, and the denier of the high melting point resin fiber is 1~3D.

[0010] As a further technical solution of the present invention, the composite fiber web has a grammage of 10-15 gsm, and the bicomponent fiber web has a grammage of 15-30 gsm.

[0011] As a further technical solution of the present invention, the protective agent includes the following components in percentage by mass: 80% to 90% synthetic oil, 5% to 10% emulsifier, 3% to 6% thickener, 1% to 5% stabilizer, 0.1% to 0.5% antioxidant, and 0.1% to 0.2% preservative; the mass ratio of the inactivated probiotics to the protective agent in the probiotic solution is 1:3 to 1:1.

[0012] As a further technical solution of the present invention, the synthetic oil is selected from one or more of stearic acid, palmitic acid, and cetyl alcohol; the emulsifier is selected from one or more of monoglycerides, sucrose esters, and lecithin; the thickener is selected from one or two of sodium alginate and chitosan; the stabilizer is selected from one or more of xanthan gum, carrageenan, and sodium carboxymethyl cellulose; the antioxidant is selected from one or more of vitamin E, butylated hydroxyanisole, and butylated hydroxytoluene; the preservative is selected from one or more of methyl parahydroxybenzoate, n-propanol, and polylysine.

[0013] As a further technical solution of the present invention, the probiotic emulsion includes the following components in mass percentage: 10%~20% ethylene acrylic acid copolymer emulsion, 30%~50% deionized water, and 30%~60% probiotic solution; the coating amount of the probiotic emulsion on a single side of the composite non-woven fabric surface is 1~5gsm.

[0014] The beneficial effects of the present invention are: The present invention sequentially fixes a composite fiber web, a bicomponent fiber web and a composite fiber web by hot air bonding to obtain a composite non-woven fabric, so that the composite non-woven fabric has good fluffiness, softness, comfort and air permeability. During the bonding and fixing process of the composite non-woven fabric, modified sodium bicarbonate is simultaneously decomposed to form a plurality of micropores on the surface of the composite fiber. After the probiotic emulsion is coated on the surface of the composite non-woven fabric, a firmly attached probiotic coating is formed. The inactivated probiotics in the probiotic coating make the probiotic non-woven fabric have good antibacterial properties and can maintain the colony balance of the probiotics. At the same time, the surface of the probiotic coating is smooth and the composite fiber maintains good softness, so the comfort of the probiotic non-woven fabric can be improved. DETAILED DESCRIPTION

[0015] The implementation mode of the present invention is described below in conjunction with relevant embodiments. The implementation mode of the present invention is not limited to the following embodiments, and the present invention relates to relevant necessary components in the technical field, which should be regarded as the known technology in the technical field and can be known and mastered by the technical personnel in the technical field.

[0016] A method for making a probiotic non-woven fabric comprises the following steps: S1. After heating granular polyethylene until it is melted, modified sodium bicarbonate and a dispersant are added and stirred to obtain a composite melt, and the composite melt is ejected through a spinning nozzle, and then pulled, curled, dried, and cut to obtain a composite fiber; the decomposition temperature of the modified sodium bicarbonate is greater than the temperature at which the polyethylene particles are heated to melt; S2, heating the granular polyethylene particles and the granular high melting point resin to melt respectively, ejecting them through a spinning nozzle, and then pulling, curling, drying, and cutting to obtain polyethylene fibers and high melting point resin fibers respectively; S3, opening and combing the composite fibers to form a two-layer composite fiber web, mixing the polyethylene fiber and the high-melting-point resin fiber, opening and combing them to form a bicomponent fiber web, stacking the composite fiber web, the bicomponent fiber web, and the composite fiber web in sequence along the thickness direction to form a multi-layer fiber web, heating the multi-layer fiber web by hot air to make the internal fibers bond to each other, then increasing the hot air temperature until the modified sodium bicarbonate is decomposed, and cooling after the modified sodium bicarbonate is completely decomposed to obtain a composite non-woven fabric; S4, adding the inactivated probiotics into the protective agent and stirring evenly to obtain a probiotic solution; S5, dispersing the ethylene acrylic acid copolymer emulsion in deionized water to form an aqueous emulsion, heating the aqueous emulsion, mixing it with the probiotic solution and emulsifying it to obtain a probiotic emulsion; S6. Evenly apply the probiotic emulsion on the surface of the composite non-woven fabric, and then air-dry the composite non-woven fabric to obtain the probiotic non-woven fabric.

[0017] The preparation method of the present invention is used to prepare a probiotic non-woven fabric, which belongs to a hot air non-woven fabric. The fibers inside the probiotic non-woven fabric include two components: polyethylene fibers and high-melting-point resin fibers. After the fibers are combed into a fiber web, the polyethylene fibers are heated by hot air to become a molten state, so that the fibers inside the fiber web are bonded to each other and then cooled to obtain a hot air non-woven fabric. The hot air non-woven fabric has the advantages of good fluffiness, comfort, air permeability, etc., and is often used for the surface layer of products such as diapers and sanitary napkins, which can improve the comfort of these products; the probiotic emulsion is coated on both sides of the hot air non-woven fabric obtained above , so that a probiotic coating is formed on the surface of the hot air non-woven fabric and a probiotic non-woven fabric is obtained. Although the inactivated probiotics in the probiotic coating have lost their activity, their cell walls and metabolites still contain antibacterial components, which can effectively inhibit the growth of harmful bacteria, so that the probiotic non-woven fabric has antibacterial function and can be used in occasions that require antibacterial protection. The inactivated probiotics are safer and will not cause secondary infection or develop resistance to antibiotics. When the probiotic non-woven fabric is used for the surface layer of the sanitary napkin, the inactivated probiotics are beneficial to maintaining the balance of the internal vaginal flora, thereby improving the health of the vagina.

[0018] In step S1 of the present invention, granular polyethylene is heated to melt to form a polyethylene melt, modified sodium bicarbonate is added to the polyethylene melt and uniformly dispersed under the action of a dispersant to obtain a composite melt, and the composite melt is ejected through a spinning nozzle to form a composite fiber, and the modified sodium bicarbonate is uniformly dispersed inside the composite fiber. In addition, since the decomposition temperature of the modified sodium bicarbonate is greater than the temperature at which the polyethylene particles are heated to melt, the modified sodium bicarbonate does not decompose in the composite melt; it should be noted that the modified sodium bicarbonate is preferably in powder form and has a particle size of less than 1 μm, which can avoid blocking the nozzle when the composite melt is ejected through the spinning nozzle, and the dispersant can improve the uniformity of the dispersion of the modified sodium bicarbonate powder, thereby ensuring the uniformity of the dispersion of the modified sodium bicarbonate in the composite melt.

[0019] In steps S2 and S3 of the present invention, polyethylene and high-melting-point resin are heated to melts respectively, and then ejected through spinning nozzles to form polyethylene fibers and high-melting-point resin fibers respectively. The polyethylene fibers and high-melting-point resin fibers are subsequently mixed, opened, and combed to form a bicomponent fiber web. The polyethylene fibers and high-melting-point resin fibers in the bicomponent fiber web are staggered, which is conducive to the mutual bonding of the molten polyethylene fibers and the high-melting-point resin fibers during subsequent hot air heating, so that the fibers inside the bicomponent fiber web are bonded and fixed to each other. In addition, a plurality of composite fibers are staggered inside the composite fiber web, and the main component of the composite fibers is polyethylene. During the subsequent hot air heating, the fibers inside the composite fiber web can be bonded and fixed to each other, and the composite fiber web is The fiber web and the two-component fiber web are bonded and fixed to each other through composite fibers and polyethylene fibers, thereby obtaining a composite non-woven fabric composed of the composite fiber web, the two-component fiber web, and the composite fiber web in sequence. The composite fiber web can ensure the softness and comfort of the surface of the composite non-woven fabric, and the high melting point resin fiber in the two-component fiber web can ensure the strength of the composite non-woven fabric; at the same time, in the process of hot air bonding and fixing the composite non-woven fabric, as the temperature of the hot air increases to the decomposition temperature of the modified sodium bicarbonate, the modified sodium bicarbonate decomposes to produce carbon dioxide. Since the composite fiber is heated to melt, the carbon dioxide can escape from the inside of the composite fiber to the outside, forming a number of micropores on the fiber surface, which is conducive to better adhesion of the probiotic emulsion to the surface of the composite non-woven fabric.

[0020] In steps S4 and S5 of the present invention, the inactivated probiotics are selected from inactivated lactobacillus and inactivated plant lactobacillus, or a mixture of the two. Other inactivated probiotics with similar functions commonly available on the market can also be used. The probiotic solution is formed by dispersing and dissolving the inactivated probiotics in the protective agent. The protective agent effectively prevents the inactivated probiotics from being affected by adverse factors such as light, oxygen, and temperature by wrapping or combining the inactivated probiotics, thereby maintaining the stability of its active ingredients. The protective agent can also delay the degradation process of the inactivated probiotics to a certain extent, prolong the durability of the efficacy of the inactivated probiotics, and improve the shelf life of the probiotic non-woven fabric; Ethylene Acrylic copolymer emulsion is a high molecular polymer made by copolymerization of ethylene and acrylic acid monomers and dispersed in water to form a liquid. The solid content of ethylene acrylic acid copolymer emulsion is 45%~50%. Ethylene acrylic acid copolymer has good adhesion and film-forming properties, and has good flexibility after drying and forming a film. The probiotic solution is mixed with the water emulsion and emulsified into a probiotic emulsion under the action of an emulsifier by ultrasonic emulsification or the like. The probiotic emulsion adheres to the surface of the composite non-woven fabric and dries to form a probiotic coating. The probiotic coating has the functions of antibacterial and maintaining the balance of vaginal flora because it contains inactivated probiotics.

[0021] In step S6 of the present invention, after the probiotic emulsion is coated on the surface of the composite non-woven fabric, the probiotic emulsion will adhere to the fiber surface of the composite non-woven fabric and form a probiotic coating. Since both sides of the composite non-woven fabric are composed of composite fibers, and the surface of the composite fiber has a number of micropores and is relatively rough, the probiotic coating can be more firmly attached to the fiber surface after curing, which can avoid the problem of easy shedding of the probiotic coating on the probiotic non-woven fabric. In addition, ethylene acrylic acid copolymer emulsion is added to the probiotic emulsion, which can make the surface of the probiotic coating smooth and keep the composite fiber soft, thereby improving the comfort of the probiotic non-woven fabric and having the advantages of good fluffiness, comfort, air permeability, etc. of hot air non-woven fabric. The probiotic non-woven fabric has the functions of antibacterial and maintaining the balance of vaginal colonies through the probiotic coating.

[0022] In summary, the present invention sequentially fixes the composite fiber web, the bicomponent fiber web, and the composite fiber web by hot air bonding to obtain a composite non-woven fabric, so that the composite non-woven fabric has good fluffiness, softness, comfort, and air permeability. During the bonding and fixing process of the composite non-woven fabric, the modified sodium bicarbonate is simultaneously decomposed to form a plurality of micropores on the surface of the composite fiber. After the probiotic emulsion is coated on the surface of the composite non-woven fabric, a firmly attached probiotic coating is formed. The inactivated probiotics in the probiotic coating make the probiotic non-woven fabric have good antibacterial properties and can maintain the colony balance of the probiotics. At the same time, the surface of the probiotic coating is smooth and the composite fiber maintains good softness, which can improve the comfort of the probiotic non-woven fabric.

[0023] As one of the preferred embodiments of the present invention, the composite melt includes the following components in mass percentage: 97.5% to 99.88% of polyethylene, 0.1% to 2% of modified sodium bicarbonate, and 0.02% to 0.5% of a dispersant; the dispersant is selected from one or more of polyvinyl alcohol, alkanolamine, alkanolamide, and polyol fatty acid ester; the polyethylene is heated to melt to form a polyethylene melt, and the modified sodium bicarbonate is added to the polyethylene melt and uniformly dispersed under the action of the dispersant to obtain a composite melt. The amount of modified sodium bicarbonate added to the composite melt is adaptively adjusted according to the number of micropores required to be formed in the composite fiber design. The more modified sodium bicarbonate is added, the more micropores are formed on the surface of the composite fiber after it is decomposed, which can improve the strength of the probiotic coating adhesion.

[0024] As one of the preferred embodiments of the present invention, in step S1, the polyethylene particles are heated to a melting temperature of 120-140°C, and the decomposition temperature of the modified sodium bicarbonate is 150-170°C; the decomposition temperature of the modified sodium bicarbonate is greater than the temperature at which the polyethylene particles are heated to melt, and the modified sodium bicarbonate does not decompose in the composite melt. In the process of hot air bonding and fixing the composite non-woven fabric, the hot air temperature is increased to the decomposition temperature of the modified sodium bicarbonate to decompose it, thereby forming a number of micropores on the surface of the composite fiber, thereby improving the firmness of the probiotic emulsion attached to the surface of the composite fiber.

[0025] As one of the preferred embodiments of the present invention, in step S3, the multilayer fiber web is first heated to melt the composite fibers and the polyethylene fibers by hot air at a temperature of 120-140°C so that the fibers inside the multilayer fiber web are bonded to each other, and then the temperature of the hot air is increased to 150-170°C to decompose the modified sodium bicarbonate to produce carbon dioxide, and the carbon dioxide escapes from the inside of the composite fibers to form a number of adsorption balloons with micropores in the composite fibers.

[0026] Due to the small particle size of modified sodium bicarbonate, it is easy to agglomerate. Although the dispersion uniformity of modified sodium bicarbonate can be improved and agglomeration can be reduced under the action of dispersant, a small amount of modified sodium bicarbonate will still agglomerate. In the process of decomposing modified sodium bicarbonate by hot air, the agglomerated sodium bicarbonate produces a large amount of carbon dioxide to expand the surface of the composite fiber and form an adsorption balloon with micropores. The diameter of the adsorption balloon is larger than the diameter of the composite fiber, and more probiotic emulsion can be adsorbed through capillary fines and formed by drying. The probiotic balloon can slowly release the antibacterial function of inactivating probiotics and the function of regulating colony balance during the use of probiotic non-woven fabrics, thereby extending the effective time of the probiotic non-woven fabrics during use. Although the composite fiber forms an adsorption balloon with the above advantages, the dispersant is still a necessary component in the composite melt. It can improve the uniformity of forming micropores on the surface of the composite fiber and is an important factor in ensuring that the probiotic coating is firmly attached to the surface of the composite fiber.

[0027] Furthermore, the amount of modified sodium bicarbonate added to the composite melt can be increased to increase the number of adsorption balloons formed. After increasing the amount of modified sodium bicarbonate added, its distribution density in the composite fiber will increase, making it easier to expand the surface of the composite fiber and form adsorption balloons with micropores by concentratedly producing a larger amount of carbon dioxide. After the composite fiber forms more adsorption balloons, it can form more probiotic balloons by absorbing probiotic emulsion, which can further extend the effective time of the probiotic non-woven fabric during use and improve the stability of the efficacy of the probiotic non-woven fabric.

[0028] As one of the preferred embodiments of the present invention, the high melting point resin is selected from one of polypropylene resin and polyester resin; the mass ratio of polyethylene fiber to high melting point resin fiber in the two-component fiber web is 1:3~1:1; the mass ratio of polyethylene fiber to high melting point resin fiber in the two-component fiber web needs to be adaptively adjusted according to the use scenario of the probiotic non-woven fabric. The polyethylene fiber mainly plays the role of bonding and fixing in the two-component fiber web, while the polypropylene fiber and the polyester fiber have higher mechanical strength. Increasing the proportion of melting point resin fiber can improve the strength of the probiotic non-woven fabric and prevent the probiotic non-woven fabric from being easily torn during use.

[0029] As one of the preferred embodiments of the present invention, the denier of the composite fiber is 0.5~1D, the gram weight of the composite fiber web is 10~15gsm, the denier of the polyethylene fiber is 1~3D, the denier of the high-melting-point resin fiber is 1~3D, and the gram weight of the bicomponent fiber web is 15~30gsm; the composite fiber is arranged on the surface of the composite non-woven fabric, and the composite fiber with lower fiber denier can improve the softness and comfort of the surface of the composite non-woven fabric, while the polyethylene fiber and the high-melting-point resin fiber are arranged inside the composite non-woven fabric, and the strength of the composite non-woven fabric is improved by the polyethylene fiber and the high-melting-point resin fiber with higher fiber denier and the bicomponent fiber web with higher gram weight, so as to prevent the probiotic non-woven fabric from being easily torn during use.

[0030] As one of the preferred embodiments of the present invention, the protective agent includes the following components in percentage by mass: 80% to 90% synthetic oil, 5% to 10% emulsifier, 3% to 6% thickener, 1% to 5% stabilizer, 0.1% to 0.5% antioxidant, and 0.1% to 0.2% preservative; the mass ratio of inactivated probiotics to the protective agent in the probiotic solution is 1:3 to 1:1; the synthetic oil is selected from one or more of stearic acid, palmitic acid, and cetyl alcohol; the emulsifier is selected from one or more of monoglyceride, sucrose ester, and lecithin; the thickener is selected from one or two of sodium alginate and chitosan; the stabilizer is selected from one or more of xanthan gum, carrageenan, and sodium carboxymethyl cellulose; the antioxidant is selected from one or more of vitamin E, butylated hydroxyanisole, and dibutylhydroxytoluene; the preservative is selected from one or more of methyl paraben, n-propanol, and polylysine.

[0031] The protective agent of the present invention is mainly used to prevent the inactivated probiotics from being affected by adverse factors such as light, oxygen, and temperature, and to maintain the stability and durability of the active ingredients in the inactivated probiotics. The protective agent usually needs to be properly heated during use, and the viscosity is reduced by heating to improve the fluidity and other properties, thereby improving the coating performance and emulsification performance of the protective agent. In the protective agent, the synthetic oil protects the probiotics by physically encapsulating them to prevent them from directly contacting the external environment, the emulsifier uses its emulsification effect and uses the probiotic solution as the oil phase and the ethylene acrylic acid copolymer emulsion as the water phase to emulsify to prepare the probiotic emulsion, the thickener increases the viscosity of the probiotic emulsion to achieve effective protection and controlled release of the probiotics, the stabilizer enhances the overall stability of the protective agent to prevent aggregation, precipitation or stratification, the antioxidant is used to prevent the synthetic oil from being oxidized to improve the stability of the protective agent, and the preservative can prevent the protective agent from being contaminated by microorganisms during storage and use.

[0032] As one of the preferred embodiments of the present invention, the probiotic emulsion includes the following components by mass percentage: 10% to 20% of ethylene acrylic acid copolymer emulsion, 30% to 50% of deionized water, and 30% to 60% of probiotic solution; the coating amount of the probiotic emulsion on a single side of the composite non-woven fabric surface is 1 to 5 gsm; in step S5, the ethylene acrylic acid copolymer emulsion is first dispersed, dissolved in deionized water and heated to form an aqueous emulsion, the aqueous emulsion is used as the aqueous phase of the emulsification system, and heating can improve the uniformity of the dispersion of the ethylene acrylic acid copolymer in the aqueous phase and improve the emulsification performance of the aqueous emulsion. Subsequently, the aqueous emulsion and the probiotic solution are emulsified to form a uniformly dispersed emulsion system, the ethylene acrylic acid copolymer provides good adhesion and film-forming properties for the probiotic emulsion, and the probiotic solution is antibacterial or maintains the balance of the colony by inactivating the active ingredients in the probiotics, so that the surface of the probiotic non-woven fabric has a firmly adhered probiotic coating and has the functions of antibacterial and maintaining the balance of the colony.

[0033] The present invention is further described below by way of examples and comparative examples.

[0034] Example 1

[0035] S1. After heating granular polyethylene until it is melted, modified sodium bicarbonate and polyvinyl alcohol are added and stirred to obtain a composite melt. After the composite melt is ejected through a spinning nozzle, it is pulled, curled, dried, and cut to obtain a composite fiber; the composite melt includes the following components by mass percentage: 99.88% polyethylene, 0.1% modified sodium bicarbonate, and 0.02% polyvinyl alcohol; S2, heating the granular polyethylene particles and the granular polypropylene to melt and ejecting them through a spinning nozzle, and then pulling, curling, drying and cutting to obtain polyethylene fibers and polypropylene fibers respectively; the mass ratio of the polyethylene fibers to the polypropylene fibers is 1:2; S3, opening and combing the composite fibers to form a two-layer composite fiber web with a gram weight of 10 gsm, mixing the polyethylene fiber and the polypropylene fiber, opening and combing them to form a bicomponent fiber web with a gram weight of 20 gsm, stacking the composite fiber web, the bicomponent fiber web, and the composite fiber web in sequence along the thickness direction to form a multi-layer fiber web, heating the multi-layer fiber web by hot air to make the internal fibers bond to each other, then increasing the hot air temperature until the modified sodium bicarbonate is decomposed, and cooling after the modified sodium bicarbonate is completely decomposed to obtain a composite non-woven fabric; S4, mixing the inactivated probiotics and the protective agent in a mass ratio of 1:2 and stirring to obtain a probiotic solution; the protective agent includes the following components in mass percentage: 84.55% of stearic acid, 7.5% of monoglyceride, 4.5% of chitosan, 3% of xanthan gum, 0.3% of vitamin E, and 0.15% of methyl paraben; S5, dispersing the ethylene acrylic acid copolymer emulsion in deionized water to form an aqueous emulsion, heating the aqueous emulsion, mixing it with the probiotic solution and emulsifying it to obtain a probiotic emulsion; the probiotic emulsion comprises the following components by mass percentage: 15% of the ethylene acrylic acid copolymer emulsion, 40% of deionized water, and 45% of the probiotic solution; S6. Evenly apply the probiotic emulsion on both sides of the composite non-woven fabric, the coating amount of the probiotic emulsion on one side of the composite non-woven fabric is 3 gsm, and then air-dry the composite non-woven fabric to obtain the probiotic non-woven fabric.

[0036] Example 2

[0037] The difference between this embodiment and the above-mentioned embodiment 1 is that in step S1, the composite melt includes the following components by mass percentage: 98.75% polyethylene, 1% modified sodium bicarbonate, and 0.25% polyvinyl alcohol; the remaining steps are the same.

[0038] Example 3

[0039] The difference between this embodiment and the above-mentioned embodiment 1 is that in step S1, the composite melt includes the following components by mass percentage: 97.5% polyethylene, 2% modified sodium bicarbonate, and 0.5% polyvinyl alcohol; the remaining steps are the same.

[0040] Comparative Example 1 S1, heating granular polyethylene particles and granular polypropylene to melt and ejecting them through a spinning nozzle, and then pulling, curling, drying and cutting to obtain polyethylene fibers and polypropylene fibers respectively; S2, opening and combing part of the polyethylene fibers to form a two-layer polyethylene fiber web with a gram weight of 10 gsm, mixing the remaining polyethylene fibers with polypropylene fibers, and then opening and combing them to form a bicomponent fiber web with a gram weight of 20 gsm, and stacking the polyethylene fiber web, the bicomponent fiber web, and the polyethylene fiber web in sequence along the thickness direction to form a multi-layer fiber web, heating the multi-layer fiber web by hot air so that the internal fibers are bonded to each other, and then cooling to obtain a composite non-woven fabric; S3, mixing the inactivated probiotics and the protective agent in a mass ratio of 1:2 and stirring to obtain a probiotic solution; the protective agent comprises the following components in mass percentage: 84.55% of stearic acid, 7.5% of monoglyceride, 4.5% of chitosan, 3% of xanthan gum, 0.3% of vitamin E, and 0.15% of methyl paraben; S4, dispersing the ethylene acrylic acid copolymer emulsion in deionized water to form an aqueous emulsion, heating the aqueous emulsion and mixing it with the probiotic solution and emulsifying it to obtain a probiotic emulsion; the probiotic emulsion comprises the following components by mass percentage: 15% of the ethylene acrylic acid copolymer emulsion, 40% of deionized water, and 45% of the probiotic solution; S5. Evenly apply the probiotic emulsion on both sides of the composite non-woven fabric, the coating amount of the probiotic emulsion on one side of the composite non-woven fabric is 3 gsm, and then air-dry the composite non-woven fabric to obtain the probiotic non-woven fabric.

[0041] Take some of the probiotic non-woven fabrics obtained in the above embodiments and comparative examples without any pretreatment and mark them as "before treatment", take some of the probiotic non-woven fabrics obtained in the above embodiments and comparative examples and vibrate them in a vibration testing machine for 10 minutes and mark them as "after treatment", and test some of the aforementioned non-woven fabrics for antibacterial performance, and the test results are shown in Table 1 below; some of the aforementioned non-woven fabrics were tested for strain culture of lactobacillus and bifidobacterium based on the plate count method, and the composite non-woven fabric obtained in step S2 of comparative example 1 was used as a blank control group, the non-woven fabric was placed in an MRA culture dish, and then the bacterial suspension with the same concentration was poured into the culture dish and cultured at a constant temperature of 37°C for 24 hours, and then part of the culture solution in the MRA culture dish was applied to a solid culture dish, and cultured anaerobically at 37°C for 48 hours, and the number of colonies was observed after the culture was completed. The results are shown in Table 2 below.

[0042]

[0043] Table 1

[0044] Table 2 It can be seen from the data in Table 1 that the probiotic non-woven fabrics have good antibacterial properties before vibration treatment. After vibration treatment, the antibacterial properties of the probiotic non-woven fabrics are reduced to varying degrees. This is because the probiotic coating on the surface of the probiotic non-woven fabrics falls off to varying degrees during the vibration test, which can simulate the shedding of the probiotic coating caused by friction and other factors during the use of the probiotic non-woven fabrics. Among them, the antibacterial property of the probiotic non-woven fabric obtained in Comparative Example 1 is the largest. In the probiotic non-woven fabrics obtained in Examples 1 to 3, the greater the amount of modified sodium bicarbonate added, the lower the reduction in antibacterial property. This is because after the amount of modified sodium bicarbonate added increases, more micropores and adsorption balloon structures are formed on the surface of the composite fiber, thereby making the probiotic coating more firmly attached.

[0045] It can be seen from the data in Table 2 that the probiotic coating has a significant promoting effect on the reproduction of the two probiotics, Lactobacillus and Bifidobacterium, used in the test, and the promoting effect is similar to the antibacterial property of the probiotic non-woven fabric. After vibration treatment, the promoting effect of the probiotic non-woven fabric on the reproduction of probiotics is reduced; thus, the probiotic non-woven fabric obtained in Examples 1 to 3 of the technical solution of the present invention can maintain stable antibacterial properties and the performance of promoting the reproduction of probiotics during use by firmly adhering the probiotic coating to the fiber surface.

[0046] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for making a probiotic non-woven fabric, characterized in that: The following steps are involved: S1. After heating granular polyethylene until it is melted, adding modified sodium bicarbonate and a dispersant and stirring evenly to obtain a composite melt, the composite melt is ejected through a spinning nozzle, and then pulled, curled, dried, and cut to obtain a composite fiber; the decomposition temperature of the modified sodium bicarbonate is greater than the temperature at which the polyethylene particles are heated to melt; S2, heating the granular polyethylene and the granular high melting point resin respectively until they are melted and ejecting them through a spinning nozzle, and then pulling, curling, drying and cutting to obtain polyethylene fibers and high melting point resin fibers respectively; S3, opening and combing the composite fibers to form a two-layer composite fiber web, mixing the polyethylene fiber and the high-melting-point resin fiber, opening and combing them to form a bicomponent fiber web, stacking the composite fiber web, the bicomponent fiber web, and the composite fiber web in sequence along the thickness direction to form a multi-layer fiber web, heating the multi-layer fiber web by hot air to make the internal fibers bond to each other, then increasing the hot air temperature until the modified sodium bicarbonate is decomposed, and cooling after the modified sodium bicarbonate is completely decomposed to obtain a composite non-woven fabric; S4, adding the inactivated probiotics into the protective agent and stirring evenly to obtain a probiotic solution; S5, dispersing the ethylene acrylic acid copolymer emulsion in deionized water to form an aqueous emulsion, heating the aqueous emulsion, mixing it with the probiotic solution and emulsifying it to obtain a probiotic emulsion; S6. Evenly apply the probiotic emulsion on the surface of the composite non-woven fabric, and then air-dry the composite non-woven fabric to obtain the probiotic non-woven fabric.

2. The method for making a probiotic nonwoven fabric according to claim 1, characterized in that: The composite melt comprises the following components by mass percentage: 97.5% to 99.88% polyethylene, 0.1% to 2% modified sodium bicarbonate, and 0.02% to 0.5% dispersant; the dispersant is selected from one or more of polyvinyl alcohol, alkanolamine, alkanolamide, and polyol fatty acid ester.

3. The method for making the probiotic non-woven fabric according to claim 1, characterized in that: In step S1, the polyethylene particles are heated to a melting temperature of 120-140°C, and the decomposition temperature of the modified sodium bicarbonate is 150-170°C.

4. The method for making a probiotic nonwoven fabric according to claim 1, characterized in that: In step S3, the multilayer fiber web is first heated by hot air at a temperature of 120-140°C to melt the composite fibers and the polyethylene fibers so that the fibers inside the multilayer fiber web are bonded to each other, and then the temperature of the hot air is increased to 150-170°C to decompose the modified sodium bicarbonate to produce carbon dioxide. The carbon dioxide escapes from the inside of the composite fibers to form a number of adsorption balloons with micropores in the composite fibers.

5. The method for making a probiotic nonwoven fabric according to claim 1, characterized in that: The high melting point resin is selected from one of polypropylene resin and polyester resin; the mass ratio of polyethylene fiber to high melting point resin fiber in the bicomponent fiber web is 1:3~1:

1.

6. The method for making the probiotic nonwoven fabric according to claim 1, characterized in that: The denier of the composite fiber is 0.5-1D, the denier of the polyethylene fiber is 1-3D, and the denier of the high-melting-point resin fiber is 1-3D.

7. The method for making a probiotic nonwoven fabric according to claim 1, characterized in that: The composite fiber web has a grammage of 10 to 15 gsm, and the bicomponent fiber web has a grammage of 15 to 30 gsm.

8. The method for making a probiotic nonwoven fabric according to claim 1, characterized in that: The protective agent includes the following components in percentage by mass: 80% to 90% of synthetic oil, 5% to 10% of emulsifier, 3% to 6% of thickener, 1% to 5% of stabilizer, 0.1% to 0.5% of antioxidant, and 0.1% to 0.2% of preservative; the mass ratio of the inactivated probiotics to the protective agent in the probiotic solution is 1:3 to 1:

1.

9. The method for making the probiotic non-woven fabric according to claim 8, characterized in that: The synthetic oil is selected from one or more of stearic acid, palmitic acid, and cetyl alcohol; the emulsifier is selected from one or more of monoglycerides, sucrose esters, and lecithin; the thickener is selected from one or two of sodium alginate and chitosan; the stabilizer is selected from one or more of xanthan gum, carrageenan, and sodium carboxymethyl cellulose; the antioxidant is selected from one or more of vitamin E, butylated hydroxyanisole, and butylated hydroxytoluene; the preservative is selected from one or more of methyl paraben, n-propanol, and polylysine.

10. The method for making a probiotic nonwoven fabric according to claim 1, characterized in that: The probiotic emulsion comprises the following components by mass percentage: 10%-20% ethylene acrylic acid copolymer emulsion, 30%-50% deionized water, and 30%-60% probiotic solution; the coating amount of the probiotic emulsion on a single side of the composite non-woven fabric surface is 1-5gsm.

Citation Information

Cited By

  • Probiotic hygienic product and preparation method thereof

    CN119345439A

  • A probiotic hygiene product and preparation method thereof

    CN119345439B

  • Probiotic fiber non-woven fabric, preparation method thereof and probiotic hygienic product

    CN119571539A