Carbon paper for gas diffusion layer as well as preparation method and application of carbon paper

By using hydrogen peroxide etching and polydopamine modification technology in the preparation of carbon paper, combined with silane coupling agent to modify graphene oxide, the problem of poor bonding between carbon fiber and phenolic resin is solved, and high breathability and low resistance are prepared Carbon paper with high mechanical strength solves the problems of insufficient process risk and environmental protection in the prior art.

CN118932784AActive Publication Date: 2024-11-12SHANDONG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411007899.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In the prior art, the interface bond between carbon fiber and phenolic resin is poor, resulting in insufficient flatness, breathability, conductivity and mechanical strength of carbon paper, and the impregnation density enhancement process has hazardous and environmental protection problems.

Method used

By ultrasonic etching of the primary carbon fiber paper after wet papermaking, polydopamine was synthesized in situ, and graphene oxide modified with silane coupling agent was dispersed in phenolic resin to form an impregnation solution, and ultrasonic impregnation, drying and Carbonization at high temperatures can produce carbon paper with excellent interfaces.

Benefits of technology

It realizes high breathability, low resistivity and high mechanical strength of carbon paper, with resistivity below 15mΩ·cm and tensile strength above 10MPa. It has a simple process, environmental protection and high safety, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932784A_ABST
    Figure CN118932784A_ABST
Patent Text Reader

Abstract

The invention discloses carbon paper for a gas diffusion layer as well as a preparation method and application of the carbon paper, and belongs to the technical field of carbon paper preparation. The preparation method provided by the invention comprises the following steps: performing ultrasonic etching on primary carbon fiber paper subjected to wet papermaking through hydrogen peroxide, and then performing in-situ synthesis of polydopamine to obtain polydopamine modified primary carbon fiber paper; dispersing the silane coupling agent modified graphene oxide in ethanol, then adding phenolic resin, and performing ultrasonic dispersion to obtain a dipping solution; performing ultrasonic impregnation on the polydopamine modified primary carbon fiber paper in the impregnation solution, drying, and performing hot-pressing curing and high-temperature carbonization to obtain the carbon fiber paper. The preparation method disclosed by the invention is simple, the preparation process is environment-friendly and good in safety, and the prepared carbon paper material is excellent in interface and has high conductivity and high mechanical strength while keeping high air permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon paper preparation, and in particular to carbon paper for a gas diffusion layer and a preparation method and application thereof. Background Art

[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Proton exchange membrane fuel cells are a clean, efficient and sustainable energy storage device that can directly convert chemical energy into electrical energy. They are widely used in promoting large-scale energy storage such as hydrogen fuel cell vehicles. The gas diffusion layer is one of the most important components affecting the performance and stability of proton exchange membrane fuel cells. At present, there are many materials used for gas diffusion layers, mainly including carbon fiber paper (carbon paper), carbon cloth or non-woven fabrics, metal materials, etc. Compared with other substrate materials, carbon fiber paper has become an ideal material for gas diffusion layer substrates due to its advantages such as high conductivity, uniform porous structure, corrosion resistance, low cost, good mechanical properties and dimensional stability.

[0004] Carbon paper is a structural and functional integrated material composed of chopped carbon fibers and resin. Traditional carbon paper is mainly prepared from chopped carbon fibers as raw materials, and is produced through processes such as wet papermaking, impregnation densification, and high-temperature carbonization. The difficulties in preparing high-performance carbon paper mainly focus on the impregnation densification process. The core key technology of impregnation densification is the interface bonding between the primary carbon fiber paper (the paper obtained after wet papermaking) and the resin, which has a direct impact on the flatness, air permeability, electrical conductivity, and mechanical strength of the final carbon paper. At present, thermosetting phenolic resin is the main precursor for impregnation densification of carbon fiber paper because of its low cost, easy availability of raw materials, high carbon residue rate, and good heat resistance and chemical stability. However, since a layer of cured acrylic resin binder is attached to the surface of the carbon fiber in the primary carbon fiber paper, the carbon fiber surface has fewer active functional groups, is chemically inert, has poor wettability with the phenolic resin, and has uneven resin adhesion, resulting in problems such as uneven paper thickness and low interface bonding strength. At the same time, the resin carbon transformed into a single phenolic resin after carbonization is a hard carbon phase with poor crystallinity, which increases the difficulty of graphitization treatment and cannot effectively reduce the resistivity.

[0005] The current impregnation process uses a mixture of conductive carbon filler or modified conductive carbon filler, thermosetting phenolic resin and organic solvent as a carbon paper impregnating agent, and then places the raw carbon fiber paper in the impregnating agent for impregnation treatment, and obtains carbon paper for gas diffusion layer after curing and carbonization. However, this method cannot improve the interface bonding between carbon fiber and phenolic resin, and the production process requires the use of concentrated nitric acid or concentrated hydrochloric acid, which is very dangerous, and the residual solution has an impact on the environment.

[0006] Therefore, how to provide a method for preparing carbon paper for gas diffusion layer that is safe and environmentally friendly, so as to simultaneously improve the interface bonding between carbon fiber and phenolic resin and increase the graphitization degree of the resin matrix. Summary of the invention

[0007] In view of this, the present invention provides a carbon paper for gas diffusion layer and a preparation method and application thereof, which solves the problems in the prior art that it is difficult to simultaneously improve the interface bonding between carbon fiber and phenolic resin and increase the graphitization degree of the resin matrix, and the preparation process is relatively dangerous and has poor environmental protection.

[0008] In a first aspect, the present invention provides a method for preparing carbon paper for a gas diffusion layer, comprising the following steps:

[0009] The nascent carbon fiber paper after wet papermaking is subjected to ultrasonic etching with hydrogen peroxide, and then polydopamine is synthesized in situ to obtain polydopamine-modified nascent carbon fiber paper;

[0010] The silane coupling agent-modified graphene oxide is dispersed in ethanol, and then a phenolic resin is added and ultrasonically dispersed to obtain an impregnation solution;

[0011] The polydopamine modified primary carbon fiber paper is ultrasonically impregnated in the impregnation solution, dried, hot pressed and solidified, and carbonized at high temperature to obtain the paper.

[0012] Preferably, the concentration of hydrogen peroxide is 5 to 30 wt %, the ultrasonic etching time is 2 to 10 min, and the ultrasonic frequency is 30 to 100 kHz.

[0013] Preferably, the step of synthesizing polydopamine in situ is: subjecting the as-received carbon fiber paper after ultrasonic etching to ultrasonic reaction in a dopamine aqueous solution with a pH of 8.5 to 9.5 for 0.5 to 2 hours, and then drying at 80 to 100° C.; the concentration of the dopamine aqueous solution is 1 to 5 g / L.

[0014] Preferably, the preparation method of the silane coupling agent modified graphene oxide is: heating the silane coupling agent in an aqueous solution to hydrolyze it, then adding the graphene oxide, soaking it at a constant temperature for 1 to 10 minutes, and centrifugally drying it to obtain the graphene oxide.

[0015] Furthermore, the silane coupling agent is selected from aniline methyl triethoxysilane, KH550, KH560 or KH590; the concentration of the silane coupling agent is 0.5-2wt%, the temperature of the heating hydrolysis is 30-50°C, and the time of the heating hydrolysis is 20-60min; the concentration of the graphene oxide is 0.1-1wt%; and the aqueous solution is water or ethanol aqueous solution.

[0016] Preferably, in the impregnation solution, the dispersion concentration of the silane coupling agent-modified graphene oxide in ethanol is 0.1-1 wt%, and the concentration of the phenolic resin is 5-15 wt%; and the ultrasonic dispersion time is 20-40 min.

[0017] Preferably, the dosage ratio of the polydopamine modified primary carbon fiber paper to the impregnation solution is (0.5-5) g:100 g; and the ultrasonic impregnation time is 8-20 min.

[0018] Preferably, in the steps of hot pressing curing and high-temperature carbonization after drying, the drying temperature is 60-90°C, the hot pressing curing temperature is 160-190°C, the hot pressing curing pressure is 2-5MPa, and the hot pressing curing time is 20-50min; the high-temperature carbonization temperature is 1400-1600°C, and the high-temperature carbonization time is 0.5-2h.

[0019] In a second aspect, the present invention provides carbon paper for a gas diffusion layer prepared by the above preparation method.

[0020] In a third aspect, the present invention provides the use of the carbon paper for gas diffusion layer in a proton exchange membrane fuel cell.

[0021] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0022] (1) The present invention uses hydrogen peroxide solution to etch the nascent carbon fiber paper after wet papermaking, and then uses polydopamine to modify the etched carbon fiber paper to obtain a modified nascent carbon fiber paper rich in hydroxyl and amino groups and well impregnated with a phenolic resin, and then impregnates the phenolic resin solution containing silane coupling agent-modified graphene oxide, and after hot pressing and carbonization, obtains a carbon fiber paper with excellent interface, high air permeability and low resistivity. The preparation method is simple and easy to achieve low-cost continuous or batch production; and the preparation process is environmentally friendly and safe.

[0023] (2) The carbon paper material prepared by the present invention is a porous carbon / carbon composite material with excellent interface prepared by loading polydopamine and graphene oxide. The carbon paper material has excellent interface, high conductivity and high mechanical strength while maintaining high air permeability, with a resistivity lower than 15mΩ·cm and a tensile strength higher than 10MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0025] Figure 1 is a scanning electron microscope image of the carbon paper prepared in Example 1 of the present invention;

[0026] Figure 2 It is a high-resolution XPS image of the nascent carbon fiber paper before and after polydopamine modification prepared in Example 2 of the present invention, wherein CFP-PDA is the nascent carbon fiber paper after polydopamine modification, and CFP-H2O2 is the nascent carbon fiber paper before polydopamine modification;

[0027] Figure 3 is a scanning electron microscope image of the carbon paper prepared in Example 2 of the present invention;

[0028] Figure 4 is a scanning electron microscope image of the carbon paper prepared in Example 3 of the present invention;

[0029] Figure 5 is a scanning electron microscope image of the carbon paper prepared in Comparative Example 1 of the present invention;

[0030] Figure 6 3 is a scanning electron microscope image of the carbon paper prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0031] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0032] The present invention provides a method for preparing carbon paper for a gas diffusion layer, comprising the following steps:

[0033] The nascent carbon fiber paper after wet papermaking is subjected to ultrasonic etching with hydrogen peroxide, and then polydopamine is synthesized in situ to obtain polydopamine-modified nascent carbon fiber paper;

[0034] The silane coupling agent-modified graphene oxide is dispersed in ethanol, and then a phenolic resin is added and ultrasonically dispersed to obtain an impregnation solution;

[0035] The polydopamine modified primary carbon fiber paper is ultrasonically impregnated in the impregnation solution, dried, hot pressed and solidified, and carbonized at high temperature to obtain the paper.

[0036] The present invention first performs hydrogen peroxide etching activation on the nascent carbon fiber paper prepared by wet papermaking to remove the binder attached to the surface of the nascent carbon fiber paper, and then synthesizes polydopamine in situ on the etched surface of the nascent carbon fiber paper, introduces polar groups such as amino groups and hydroxyl groups, so as to have good wettability with the phenolic resin and improve the interface bonding strength. There are reports on the modification of carbon fiber using polydopamine in the prior art, but if the carbon fiber is first modified with polydopamine and then wet papermaking is performed, the binder will cover the surface of the carbon fiber, covering the polydopamine; at the same time, the functional groups of polydopamine react with the functional groups of the binder, consuming the polydopamine, so that the polydopamine cannot play a role in improving the interface during the resin impregnation process. The present invention adopts the above technical scheme to significantly improve the wettability between the nascent carbon fiber paper and the phenolic resin.

[0037] The impregnation solution of the present invention contains graphene oxide modified by a silane coupling agent. The surface of the graphene oxide modified by the silane coupling agent has more polar groups, which can improve the activity of the impregnation solution, thereby further increasing the wettability between the primary carbon fiber paper and the phenolic resin. At the same time, the introduction of the graphene oxide modified by the silane coupling agent can also improve the graphitization degree of the phenolic resin after carbonization, thereby improving the conductivity of the carbon paper.

[0038] In the present invention, the concentration of hydrogen peroxide is 5-30wt%, more preferably 5-15wt%, and further preferably 8-12wt%; the ultrasonic etching time is 2-10min, more preferably 2-5min; the ultrasonic frequency is 30-100kHz, more preferably 40-80kHz. The resin adhesive attached to the surface of the primary carbon fiber paper is removed by the strong oxidation of hydrogen peroxide. The etching time should not be too long, otherwise the bonding part of the primary carbon fiber paper may be damaged, affecting the mechanical strength of the carbon fiber paper.

[0039] In the present invention, the step of in-situ synthesis of polydopamine is: ultrasonically reacting the nascent carbon fiber paper after ultrasonic etching in a dopamine aqueous solution with a pH of 8.5 to 9.5 for 0.5 to 2 hours, and then drying at 80 to 100°C; the concentration of the dopamine aqueous solution is 1 to 5 g / L. Dopamine can undergo self-polymerization under alkaline conditions, and the surface of the modified nascent carbon fiber paper has polar groups such as amino groups and hydroxyl groups. The present invention does not impose any special restrictions on the alkaline control means, and the alkaline control method commonly used by those skilled in the art can be adopted. The present invention does not impose any special restrictions on the drying time, as long as it is dried to constant weight.

[0040] In the present invention, the preparation method of the silane coupling agent modified graphene oxide is: heating the silane coupling agent in an aqueous solution to hydrolyze, then adding graphene oxide, and soaking at a constant temperature for 1 to 10 minutes, more preferably 2 to 5 minutes; centrifugal drying to obtain. After the silane coupling agent is heated and hydrolyzed, a silanol group is generated, which can form a hydrogen bond with the hydroxyl group on the surface of the graphene oxide, and Si-OC can be formed under heating conditions, so that the silane coupling agent is grafted onto the graphene oxide. The present invention does not impose any special restrictions on the centrifugal drying process, and the centrifugal drying means commonly used in the art can be used.

[0041] In the present invention, the silane coupling agent is selected from aniline methyl triethoxysilane, KH550, KH560 or KH590, and is more preferably aniline methyl triethoxysilane; the concentration of the silane coupling agent is 0.5-2wt%, and is more preferably 0.5-1wt%; the temperature of the heating hydrolysis is 30-50°C, and is more preferably 35-45°C; the time of the heating hydrolysis is 20-60min, and is more preferably 20-40min. The concentration of the graphene oxide is 0.1-1wt%. The aqueous solution is water or ethanol aqueous solution, and the specific solvent selection can be adjusted according to the solubility of the selected silane coupling agent, and the present invention does not impose any special restrictions on this.

[0042] In the impregnation solution of the present invention, the dispersion concentration of the silane coupling agent modified graphene oxide in ethanol is 0.1-1wt%, and the concentration of the phenolic resin is 5-15wt%; the ultrasonic dispersion time is 20-40min.

[0043] In the present invention, the usage ratio of the polydopamine modified primary carbon fiber paper to the impregnation solution is (0.5-5) g:100 g, more preferably (0.5-2) g:100 g; the ultrasonic impregnation time is 8-20 min, more preferably 8-15 min.

[0044] In the present invention, in the steps of hot pressing curing and high temperature carbonization after drying, the drying temperature is 60-90°C, the hot pressing curing temperature is 160-190°C, more preferably 160-180°C, the hot pressing curing pressure is 2-5MPa, and the hot pressing curing time is 20-50min, more preferably 20-40min; the high temperature carbonization temperature is 1400-1600°C, more preferably 1450-1550°C, and the high temperature carbonization time is 0.5-2h. The impregnation solution of the present invention contains silane coupling agent modified graphene oxide, which can make the phenolic resin have a higher degree of graphitization at a lower graphitization temperature. The higher the degree of graphitization, the smaller the contact resistance between the carbon fiber and the phenolic resin, and thus the higher the conductivity.

[0045] The present invention also provides carbon paper for gas diffusion layer prepared by the above preparation method. The carbon paper for gas diffusion layer of the present invention has both low resistivity and high mechanical strength while maintaining high air permeability, with a resistivity lower than 15mΩ·cm and a tensile strength higher than 10MPa.

[0046] The present invention also provides an application of the carbon paper for gas diffusion layer in a proton exchange membrane fuel cell. Specifically, the carbon paper for gas diffusion layer is used as the gas diffusion layer of the proton exchange membrane fuel cell to transport gas and conduct electrons.

[0047] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0048] Example 1

[0049] This embodiment provides a method for preparing carbon paper.

[0050] Step 1: soak the wet-made raw carbon fiber paper in a 10 wt % hydrogen peroxide solution and perform ultrasonic etching for 5 minutes at an ultrasonic frequency of 40 kHz.

[0051] Step 2: The carbon fiber paper material treated in step 1 is ultrasonically immersed in a 2 g / L dopamine aqueous solution with a pH of 8.5 for 60 min, and then dried at 100° C. to obtain polydopamine-modified primary carbon fiber paper.

[0052] Step 3, prepare a 0.5wt% concentration of anilinemethyltriethoxysilane (AMT) ethanol aqueous solution (ethanol: water = 92:8, v / v); the solution is magnetically stirred at 40°C for 30min to ensure the hydrolysis of AMT, and then a single layer of graphene oxide (GO) is added, and the mixture is immersed at a constant temperature of 40°C for 2min, followed by centrifugal drying to obtain AMT-modified GO.

[0053] Step 4: Disperse the AMT-modified GO in step 3 in ethanol, control the concentration of AMT-modified GO to 0.1wt%, directly add 10wt% of phenolic resin powder (PF) after ultrasonication for 30min, and continue ultrasonic dispersion for 30min to obtain a uniformly dispersed GO-PF impregnation solution.

[0054] Step 5: impregnate 0.7 g of the polydopamine-modified virgin carbon fiber paper obtained in step 2 into 100 g of the GO-PF impregnation solution obtained in step 4, ultrasonicate for 10 min, and then dry at 80°C.

[0055] Step 6: The material dried in step 5 is hot-pressed and cured at 170° C. and 3 MPa for 30 min.

[0056] Step 7: Carbonize the material after hot pressing and curing in step 6 at 1500° C. for 1 hour.

[0057] Figure 1 The surface morphology of the carbon paper prepared in this example shows that the carbon fibers are closely overlapped, the structure is compact, and the pore structure is uniform.

[0058] Example 2

[0059] This embodiment provides a method for preparing carbon paper.

[0060] Step 1: soak the wet-made raw carbon fiber paper in a 10 wt% hydrogen peroxide solution and perform ultrasonic etching for 5 minutes at an ultrasonic frequency of 80 kHz.

[0061] Step 2, ultrasonically immersing the carbon fiber paper material treated in step 1 in a 2 g / L dopamine aqueous solution with a pH of 8.5 for 60 min, and then drying at 100° C. to obtain polydopamine-modified primary carbon fiber paper;

[0062] Step 3, prepare a 0.5wt% concentration of anilinemethyltriethoxysilane (AMT) ethanol aqueous solution (ethanol: water = 92:8, v / v); the solution is magnetically stirred at 40°C for 30min to ensure the hydrolysis of AMT, and then a monolayer of graphene oxide (GO) is added, and the mixture is immersed at a constant temperature of 40°C for 5min, followed by centrifugal drying to obtain AMT-modified GO.

[0063] Step 4: Disperse the AMT-modified GO in step 3 in ethanol, control the concentration of AMT-modified GO to 0.5wt%, directly add 10wt% of phenolic resin powder (PF) after ultrasonication for 30min, and continue ultrasonic dispersion for 30min to obtain a uniformly dispersed GO-PF impregnation solution.

[0064] Step 5: impregnate 0.7 g of the polydopamine-modified virgin carbon fiber paper obtained in step 2 into 100 g of the GO-PF impregnation solution obtained in step 4, ultrasonicate for 10 min, and then dry at 80°C.

[0065] Step 6: The material dried in step 5 is hot-pressed and cured at 170° C. and 3 MPa for 30 min.

[0066] Step 7: Carbonize the material after hot pressing and curing in step 6 at 1500° C. for 1 hour.

[0067] Figure 2 This is a high-resolution XPS image (X-ray photoelectron spectroscopy) of the nascent carbon fiber paper before and after polydopamine modification in this example. It can be seen that the successful modification of polydopamine increases the N and O contents of the nascent carbon paper, thereby enhancing the activity of the nascent carbon fiber paper. Figure 3This is a surface morphology of the carbon paper prepared in this example. It can be seen from the figure that the amount of resin impregnated on the surface of the carbon fiber increases, and the phenolic resin is fully carbonized and tightly bonded to the carbon fiber without any cracks.

[0068] Example 3

[0069] This embodiment provides a method for preparing carbon paper.

[0070] Step 1: soak the wet-made raw carbon fiber paper in a 10 wt% hydrogen peroxide solution and perform ultrasonic etching for 2 minutes at an ultrasonic frequency of 60 kHz.

[0071] Step 2: The carbon fiber paper material treated in step 1 is ultrasonically immersed in a 2 g / L dopamine aqueous solution with a pH of 8.5 for 60 min, and then dried at 100° C. to obtain polydopamine-modified primary carbon fiber paper.

[0072] Step 3, prepare a 0.75wt% concentration of anilinemethyltriethoxysilane (AMT) ethanol aqueous solution (ethanol: water = 92:8, v / v); the solution is magnetically stirred at 40°C for 30min to ensure the hydrolysis of AMT, and then multilayer GO is added and soaked at a constant temperature of 40°C for 2min, followed by centrifugal drying to obtain AMT-modified GO.

[0073] Step 4: Disperse the AMT-modified GO in step 3 in ethanol, control the concentration of AMT-modified GO to 0.75wt%, directly add 5wt% of phenolic resin powder (PF) after ultrasonication for 30min, and continue ultrasonic dispersion for 30min to obtain a uniformly dispersed GO-PF impregnation solution.

[0074] Step 5: impregnate 0.7 g of the polydopamine-modified nascent carbon fiber paper obtained in step 2 into 100 g of the impregnation solution obtained in step 4, ultrasonicate for 10 min, and then dry at 80°C.

[0075] Step 6: The material dried in step 5 is hot-pressed and cured at 170° C. and 3 MPa for 30 min.

[0076] Step 7: Carbonize the material after hot pressing and curing in step 6 at 1500° C. for 1 hour.

[0077] Figure 4 This is the surface morphology of the carbon paper prepared in this embodiment. It can be seen that the resin bonding area at the carbon fiber overlap is reduced, the resin is more attached to the fiber surface, and the carbon paper structure is uniform and flat, so the tensile strength is better and the air permeability is better.

[0078] Comparative Example 1

[0079] The difference between this comparative example and Example 1 is that the impregnation solution of this comparative example does not contain AMT-modified GO. The specific steps are as follows:

[0080] Step 1: soak the wet-made raw carbon fiber paper in a 10 wt % hydrogen peroxide solution and perform ultrasonic etching for 5 minutes at an ultrasonic frequency of 40 kHz.

[0081] Step 2: The carbon fiber paper material treated in step 1 is ultrasonically immersed in a 2 g / L dopamine aqueous solution with a pH of 8.5 for 60 min, and then dried at 100° C. to obtain polydopamine-modified primary carbon fiber paper.

[0082] Step 3: Immerse the polydopamine-modified primary carbon fiber paper prepared in step 2 in a 10 wt % phenolic resin ethanol solution, ultrasonicate for 10 min, and then dry at 80°C.

[0083] Step 4: The material dried in step 3 is hot-pressed and cured at 170° C. and 3 MPa for 30 min.

[0084] Step 5: Carbonize the material after hot pressing and curing in step 4 at 1500° C. for 1 hour.

[0085] The overall performance test data results of the final product carbon paper are shown in Table 1.

[0086] Figure 5 The surface morphology of the carbon paper prepared for this comparative example shows that the phenolic resin is unevenly impregnated and there is a phenomenon of resin agglomeration. Although the unilateral modification of carbon fiber by polydopamine improves the polarity of carbon fiber, the phenolic resin still has the problem of poor activity. Therefore, during impregnation, agglomeration occurs at the overlap of carbon fiber paper. The presence of graphene oxide can enhance the activity of phenolic resin, improve the interfacial strength of carbon paper, and reduce the resistivity of carbon paper after carbonization. This comparative example only adds polydopamine and does not use graphene oxide, so the tensile strength is lower than that of the embodiment and the resistivity is higher.

[0087] Comparative Example 2

[0088] The difference between this comparative example and Example 1 is that this comparative example does not use polydopamine for modification. The specific steps are as follows:

[0089] Step 1: Soak the raw carbon fiber paper in a 10 wt% hydrogen peroxide solution and perform ultrasonic etching for 5 minutes at an ultrasonic frequency of 40 kHz.

[0090] Step 2, prepare a 0.5wt% concentration of anilinemethyltriethoxysilane (AMT) ethanol aqueous solution (ethanol: water = 92:8, v / v); the solution is magnetically stirred at 40°C for 30min to ensure the hydrolysis of AMT, and then a single layer of graphene oxide (GO) is added, and the mixture is immersed at a constant temperature of 40°C for 2min, followed by centrifugal drying to obtain AMT-modified GO.

[0091] Step 3: Disperse the AMT-modified GO in step 2 in ethanol, control the concentration of AMT-modified GO to 0.1wt%, directly add 10wt% of phenolic resin powder (PF) after ultrasonication for 30min, and continue ultrasonic dispersion for 30min to obtain a uniformly dispersed GO-PF impregnation solution.

[0092] Step 4: 0.7 g of the material treated in step 1 was immersed in 100 g of the GO-PF impregnation solution obtained in step 4, ultrasonicated for 10 min, and then dried at 80°C.

[0093] Step 5: The material dried in step 4 is hot-pressed and cured at 170° C. and 3 MPa for 30 min.

[0094] Step 6: Carbonize the material after hot pressing and curing in step 5 at 1500° C. for 1 hour.

[0095] Figure 6 This is the surface morphology of the carbon paper prepared in this comparative example; it can be seen from the figure that resin carbon aggregation and cracking exist on the surface of the carbon paper. Because of the addition of graphene in this comparative example, the viscosity of the impregnated resin is further increased, but the fiber surface is not modified, the resin wettability is poor, more resin adheres to the fiber overlap, and after compression molding, a larger resin film is formed at the overlap. After high-temperature carbonization, the resin carbon film cracks. The resin carbon cannot fully play a role in connection and fixation, so the mechanical properties are not good. At the same time, because the graphene oxide is converted into graphene with good conductivity after carbonization, the resistivity of the carbon paper is slightly lower, but due to the poor interface, the resistivity is still higher than that of Example 1.

[0096] Test example

[0097] The carbon papers prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were tested for performance. The air permeability was tested using an air permeability meter, the pressure was increased to 50 Pa, and the system automatically detected the air flow through the carbon paper. The tensile properties were measured using a universal tensile testing machine, and the length and width of the tensile specimen were 70 mm*10 mm. The resistivity was measured using a four-probe resistivity meter.

[0098] The test results are shown in Table 1.

[0099] Table 1 Carbon paper performance test data results

[0100]

[0101]

[0102] As can be seen from Table 1, in Comparative Example 1, the phenolic resin was not modified, and the degree of graphitization of the phenolic resin after carbonization was not high, so the resistivity was much lower than that of the carbon paper after adding GO, indicating that graphene oxide has a good effect on improving the conductivity of carbon paper. In Comparative Example 2, the virgin carbon fiber paper was simply etched with hydrogen peroxide, and then impregnated with the phenolic resin impregnation solution doped with modified graphene oxide, and the carbon paper was prepared. The tensile strength was much lower than that of the carbon paper prepared in Example 1. It can be seen that the surface polydopamine has a good effect on repairing the etching effect brought by hydrogen peroxide, improving the interface, and improving the mechanical strength.

[0103] It can be seen from the test results of Examples 1 to 3 that the carbon fiber paper material prepared by the present invention has a well-connected interface and a uniform pore structure. The prepared carbon paper has the advantages of high mechanical strength, high conductivity and high air permeability, and can be used as a gas diffusion layer of a proton exchange membrane fuel cell to transport gas and conduct electrons.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing carbon paper for a gas diffusion layer, characterized in that: The steps include: The nascent carbon fiber paper after wet papermaking is subjected to ultrasonic etching with hydrogen peroxide, and then polydopamine is synthesized in situ to obtain polydopamine-modified nascent carbon fiber paper; The silane coupling agent-modified graphene oxide is dispersed in ethanol, and then a phenolic resin is added and ultrasonically dispersed to obtain an impregnation solution; The polydopamine modified primary carbon fiber paper is ultrasonically impregnated in the impregnation solution, dried, hot pressed and solidified, and carbonized at high temperature to obtain the paper.

2. The preparation method according to claim 1, characterized in that The concentration of the hydrogen peroxide is 5-30wt%, the ultrasonic etching time is 2-10min, and the ultrasonic frequency is 30-100kHz.

3. The preparation method according to claim 1, characterized in that: The steps of synthesizing polydopamine in situ are as follows: subjecting the nascent carbon fiber paper after ultrasonic etching to ultrasonic reaction in a dopamine aqueous solution with a pH value of 8.5 to 9.5 for 0.5 to 2 hours, and then drying at 80 to 100° C.; the concentration of the dopamine aqueous solution is 1 to 5 g / L.

4. The preparation method according to claim 1, characterized in that: The preparation method of the silane coupling agent modified graphene oxide is as follows: heating the silane coupling agent in an aqueous solution to hydrolyze it, then adding the graphene oxide, soaking it at a constant temperature for 1 to 10 minutes, and centrifugally drying it to obtain the graphene oxide.

5. The preparation method according to claim 4, characterized in that: The silane coupling agent is selected from aniline methyl triethoxysilane, KH550, KH560 or KH590; the concentration of the silane coupling agent in water is 0.5-2wt%, the temperature of the heating hydrolysis is 30-50°C, and the time of the heating hydrolysis is 20-60min; the concentration of the graphene oxide is 0.1-1wt%; and the aqueous solution is water or ethanol aqueous solution.

6. The preparation method according to claim 1, characterized in that: In the impregnation solution, the dispersion concentration of the silane coupling agent modified graphene oxide in ethanol is 0.1-1wt%, and the concentration of the phenolic resin is 5-15wt%; the ultrasonic dispersion time is 20-40 minutes.

7. The preparation method according to claim 1, characterized in that: The dosage ratio of the polydopamine modified primary carbon fiber paper to the impregnation solution is (0.5-5) g:100 g; and the ultrasonic impregnation time is 8-20 min.

8. The preparation method according to claim 1, characterized in that: In the steps of hot pressing curing and high-temperature carbonization after drying, the drying temperature is 60-90°C, the hot pressing curing temperature is 160-190°C, the hot pressing curing pressure is 2-5MPa, and the hot pressing curing time is 20-50min; the high-temperature carbonization temperature is 1400-1600°C, and the high-temperature carbonization time is 0.5-2h.

9. Carbon paper for gas diffusion layer prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the carbon paper for gas diffusion layer according to claim 9 in a proton exchange membrane fuel cell.

Citation Information

Patent Citations

  • Functionalized polydopamine derived carbon layer coated carbon substrate preparation method and application

    CN106340399A

  • Preparation method and application of carbon paper impregnated resin for gas diffusion layer of fuel cell

    CN111900416A

  • Impregnating resin material for densification modification of carbon fiber paper, high-performance carbon fiber paper and preparation method of high-performance carbon fiber paper