High-strength degradable environment-friendly paper box material and preparation method thereof
The high-strength environmentally friendly carton material is formed through biological enzymatic bleaching and chemical treatment, which solves the problem that packaging cartons in the prior art are difficult to have waterproof, flame retardant and degradable at the same time, and achieves the multiple performance improvements of the material and environmental protection goals.
Patent Information
- Application Number
- CN202411020171.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
Existing packaging boxes are difficult to meet the requirements of high waterproof, flame retardant and degradable at the same time, especially in humid or rainy areas.
The waste pulp after bleaching by biological enzyme method, combined with lithium bromide and sodium alginate to form an aerogel, and then silicone gel is prepared using silicone prepolymer, modified melamine polyphosphate and fluoropolysiloxane. , and mixed with modified starch and cellulose fibers, and then extruded and dehydrated to form and hot press drying to prepare high-strength environmentally friendly carton material.
It realizes the high strength, waterproofness, flame retardancy and degradability of carton materials, reduces production costs, is suitable for a variety of packaging fields, and meets the dual needs of environmental protection and performance.
Smart Images

Figure BDA0004966984330000111
Abstract
Description
Technical Field
[0001] The present application relates to the field of packaging paper boxes, and in particular to a high-strength and degradable environmentally friendly paper box material and a preparation method thereof. Background Art
[0002] As an important part of logistics and commodity circulation, the performance of packaging cartons is crucial to the protection of products and the impact on the environment. With the improvement of environmental awareness, traditional plastic packaging materials are gradually being replaced by degradable and environmentally friendly paper packaging materials due to their non-degradability. At the same time, in humid or rainy areas, the waterproof performance of packaging cartons is also particularly important. However, packaging cartons in the prior art often find it difficult to simultaneously meet the requirements of high waterproofness, flame retardancy and degradability. Summary of the invention
[0003] The purpose of this application is to provide a high-strength and degradable environmentally friendly paper box material and a preparation method thereof in response to the deficiencies of current technology. The preparation method of the high-strength and degradable environmentally friendly paper box material of the present application has the advantages of simple production and low cost. At the same time, the high-strength and degradable environmentally friendly paper box material has excellent mechanical properties, waterproof properties, flame retardancy, wear resistance and tear resistance, and is degradable, and has broad application prospects.
[0004] In the first aspect, the present application provides a method for preparing a high-strength and degradable environmentally friendly paper box material, using the following technical solution: A method for preparing a high-strength and degradable environmentally friendly paper box material, comprising the following steps: S1, subjecting waste boxboard paper pulp to a bio-enzymatic bleaching treatment to obtain bleached waste paper pulp; S2, treating the bleached waste paper pulp with lithium bromide and sodium alginate in sequence to obtain waste paper aerogel; S3, preparing silicone gel using siloxane prepolymer, modified melamine polyphosphate and fluorine-containing polysiloxane; S4, mixing 15-20 parts of waste paper aerogel, 4-6 parts of silicone gel, 15-20 parts of modified starch, 8-10 parts of cellulose fiber and 50-55 parts of hardwood pulp with a mass concentration of 10% according to weight proportions to obtain a pulp mixture; S5. The pulp mixture is made into pulp molding wet blanks by using a paper sheet former, and then extruded, dehydrated and shaped, transferred to a flat mold, and hot-pressed and dried to obtain a high-strength and degradable environmentally friendly paper box material.
[0005] By adopting the above technical scheme, step S1: bioenzymatic bleaching treatment: use a composite enzyme solution (alkaline pectinase, xylanase, mannanase and ligninase) for bleaching, effectively remove residual ink and impurities in waste boxboard pulp, and enhance the bonding force between fibers. This not only improves the quality of the pulp, but also provides a better basis for subsequent chemical treatment. By improving the quality of the pulp, it is ensured that the final product has higher strength and durability. Step S2: lithium bromide and sodium alginate treatment This treatment transforms the waste paper pulp into an aerogel structure, increases the complexity of the cross-linked network of the material, and thus significantly improves its mechanical properties. The addition of sodium alginate not only improves the flame retardant and waterproof properties, but also produces good compatibility with the subsequently added siloxane prepolymer and modified melamine polyphosphate, creating conditions for the formation of a uniform composite material. Step S3: Preparation of silicone gel: by introducing fluorinated polysiloxane and modified melamine polyphosphate, the prepared silicone gel has excellent high temperature stability, hydrophobicity and flame retardant properties. These properties make silicone gel an ideal choice for improving the waterproofness and flame retardancy of paper box materials. At the same time, the introduction of lipoic acid enhances the cohesion and flexibility of the material through ring-opening polymerization. Step S4: Preparation of mixture: waste paper aerogel, silicone gel, modified starch, cellulose fiber and hardwood pulp are mixed in proportion to obtain a uniform pulp mixture. This mixing ensures a good distribution of various components, which is conducive to improving the uniformity and performance of the final material. The addition of modified starch and cellulose fiber not only improves the mechanical properties and wear resistance of the material, but also maintains the degradability of the material, which meets environmental protection requirements. Step S5: Molding and drying: The pulp is molded into a wet blank using a paper sheet former, and then extrusion dehydration shaping and hot pressing drying are performed to obtain a high-strength and degradable environmentally friendly paper box material. This process not only forms the final shape of the material, but also further removes moisture through hot pressing drying, ensuring the dimensional stability and durability of the material. In general, each step in this application is carefully designed to ensure the comprehensive performance of the environmentally friendly paper box material, including its mechanical properties, waterproofness, flame retardancy and degradability. Through the synergistic effect of these steps, a high-performance, low-cost, and environmentally friendly paper box material is obtained, which has broad application prospects.
[0006] Preferably, in step S1, the method of bio-enzymatic bleaching treatment is: according to the mass fraction, 2-4 parts of the composite enzyme solution are added to 1000 parts of waste boxboard pulp with a mass concentration of 8% through a metering pump, so that it is evenly mixed with the waste boxboard pulp for enzymatic hydrolysis reaction, and the enzymatic hydrolysis reaction conditions are: temperature 50-55°C, pH 7.0-8.0, enzymatic hydrolysis time 50-60 minutes, and the bio-enzymatic bleaching process is repeated three times to obtain bleached waste paper pulp.
[0007] Preferably, the complex enzyme solution consists of alkaline pectinase, xylanase, mannanase and ligninase, the activity of the alkaline pectinase is 1000u / ml-1500u / ml, the activity of the xylanase is 1800u / ml-2200u / ml, the activity of the mannanase is 600u / ml-1000u / ml, and the activity of the ligninase is 100u / ml-150u / ml.
[0008] Preferably, in step S2, the preparation method of the waste paper aerogel is: dispersing 100 parts of bleached waste paper pulp with a mass concentration of 8% in 200 parts of lithium bromide solution with a mass concentration of 10%, stirring at 138°C, pouring into a mold, cooling to a gel state, soaking the gel with tap water and deionized water in turn until no precipitate is generated by silver nitrate solution detection, and then soaking it in 120 parts of a mixed solution consisting of a sodium alginate solution with a mass concentration of 10% and a tert-butanol solution with a mass concentration of 30%, stirring for 1 hour, and then freeze-drying at a temperature of -50°C for 2-3 hours to obtain the waste paper aerogel.
[0009] By adopting the above technical scheme, the bleached waste paper pulp is dispersed in the lithium bromide solution, and the pulp is fully dispersed by high-temperature stirring, which helps to improve the uniformity and performance of the final aerogel. After cooling to a gel state, the waste paper pulp forms an aerogel structure under the action of lithium bromide. This structure has a lower density and a higher specific surface area, which is beneficial to improving the mechanical properties and functionality of the material. The impurities in the aerogel are removed by soaking and washing with tap water and deionized water to ensure that the final product has better purity and performance. Soaking in a mixed solution of sodium alginate and tert-butyl alcohol and stirring the aerogel makes the cross-linked network more complex, thereby greatly improving its mechanical properties. At the same time, the introduction of sodium alginate effectively improves the flame retardant and waterproof properties of the material. Freeze drying at low temperature helps to maintain the porous structure of the aerogel, avoids the destruction of its structure due to shrinkage during the drying process, and ensures the light weight and high strength characteristics of the material. The surface properties and pore structure of the waste paper aerogel obtained by treating with lithium bromide and sodium alginate are optimized, making it compatible with the silicone gel added in the subsequent steps, which is conducive to the formation of a uniform composite material. The porous structure and excellent mechanical properties of the waste paper aerogel, combined with the waterproof and flame retardant properties of the silicone gel, and the reinforcing effect of other components such as modified starch and cellulose fibers, jointly improve the comprehensive properties of the final environmentally friendly paper box material, including mechanical properties, waterproofness, flame retardancy, wear resistance, tear resistance and degradability. No harmful chemicals are used in the entire preparation process, and the pollution to the environment is reduced by bio-enzymatic bleaching treatment. At the same time, the waste paper aerogel obtained can achieve the degradability of the paper box material without sacrificing performance, which meets environmental protection requirements.
[0010] Preferably, in step S3, the method for preparing the organic silicone gel comprises the following steps: S51, under a nitrogen atmosphere, 10 g of amino-terminated siloxane, 2.1 g of lipoic acid and 20 mL of tetrahydrofuran were mixed, and the mixture was kept at 61-65° C. for 4-5 h, and then the mixture was heated to 80-83° C. for 2-3 h to obtain a siloxane prepolymer; S52, 2 g of modified melamine polyphosphate, 10 g of siloxane prepolymer, 0.3 g of fluorine-containing polysiloxane and 12 mL of tetrahydrofuran were mixed, and ultrasonically dispersed for 60-70 min to obtain a silicone gel.
[0011] By adopting the above technical scheme, in step S3, the preparation method of the silicone gel includes two key steps, step S51: synthesis of siloxane prepolymer: in this step, amino-terminated siloxane, lipoic acid and tetrahydrofuran are mixed under a nitrogen atmosphere and subjected to a heat preservation reaction at a specific temperature. This process causes the amino-terminated siloxane to react with lipoic acid to form a siloxane prepolymer. Lipoic acid can initiate ring-opening polymerization under such conditions to form a hyperbranched structure, which gives the prepolymer good toughness and reactivity. The introduction of lipoic acid not only provides a biocompatible ring-opening polymerization pathway, but also enhances the cohesion and flexibility of the siloxane prepolymer through its multi-terminal carboxyl hyperbranched structure, laying the foundation for the subsequent reaction with modified melamine polyphosphate. Step S52: preparation of silicone gel: in this step, modified melamine polyphosphate, silicone prepolymer, fluorinated polysiloxane and tetrahydrofuran are mixed and dispersed by ultrasound to form a uniform silicone gel. As a flame retardant, the uniform dispersion of modified melamine polyphosphate in the mixture is crucial to improving the flame retardant properties of the final material. The addition of fluorinated polysiloxane improves the high temperature stability and hydrophobicity of the silicone gel, which is crucial to improving the waterproof performance of the paper box material. At the same time, the compatibility of modified melamine polyphosphate with siloxane prepolymer is improved, so that the flame retardant can be more evenly dispersed in the siloxane network, thereby improving the flame retardant performance. Overall, the two sub-steps in step S3 work together to prepare a silicone gel with excellent toughness, waterproofness and flame retardancy through a sophisticated chemical reaction and physical mixing process. This silicone gel not only improves the comprehensive performance of the paper box material, but also maintains its environmentally friendly and degradable characteristics, meeting the dual needs of high performance and environmental protection requirements in fields such as food packaging.
[0012] Preferably, in step S3, the method for preparing the modified melamine polyphosphate comprises the following steps: S61. Prepare an aqueous suspension by mixing 30 parts of hydrotalcite and 30 parts of water in parts by mass; S62, dispersing 300 parts of melamine polyphosphate in a solution consisting of 8 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 80 parts of water according to weight percentage to obtain a mixed solution; S63, slowly drop the water suspension into the mixed solution, heat to 43°C, stir at 300 rpm, react for 30-40 minutes, filter, and vacuum dry at 80°C for 24 hours, grind and sieve to obtain modified melamine polyphosphate with a particle size of 1-2 μm.
[0013] By adopting the above technical scheme, step S61: preparing a hydrotalcite suspension: mixing hydrotalcite and water according to mass fractions to prepare a water suspension. As a layered double hydroxide, hydrotalcite can provide a large number of active sites and provide a basis for subsequent chemical reactions. The preparation of the hydrotalcite suspension provides a uniformly dispersed medium for the subsequent modification reaction, which is conducive to improving the efficiency of the reaction and the dispersibility of the modifier. Step S62: dispersing melamine polyphosphate and forming a mixed solution: dispersing melamine polyphosphate in a solution containing γ-aminopropyltrimethoxysilane, ethanol and water to obtain a mixed solution. This step fully disperses the melamine polyphosphate and introduces the coupling agent γ-aminopropyltrimethoxysilane to prepare for the modification reaction. The addition of the coupling agent improves the compatibility of melamine polyphosphate with the siloxane prepolymer, improves the dispersibility of the flame retardant in the siloxane prepolymer, and thus enhances the flame retardant properties of the final silicone gel. Step S63: modification reaction and post-treatment: slowly drop the hydrotalcite suspension into the mixed solution, react at a certain temperature and stirring rate, and then filter, dry, grind and sieve to obtain a modified melamine polyphosphate with a particle size of 1-2 μm. This process completes the modification of melamine polyphosphate, making it have better flame retardant properties and compatibility with other components. Modified melamine polyphosphate can release flame retardant gases, such as phosphoric acid, during the combustion process, forming a protective layer to slow down the combustion rate and prevent the spread of flames. At the same time, the modified particles are uniform in size, which is conducive to uniform dispersion in the carton material and improves the overall flame retardant properties of the material. In summary, the preparation method of modified melamine polyphosphate not only improves the performance of the flame retardant through precisely controlled chemical reactions and physical treatment processes, but also ensures its good compatibility with other components of the carton material, thereby significantly improving the flame retardant ability of the carton material without affecting the degradability of the material.
[0014] Preferably, in step S3, the preparation method of the fluorinated polysiloxane is as follows: 100 parts of terminal vinyl silicone oil and 0.5 parts of platinum catalyst are mixed according to mass parts, 17 parts of perfluoroalkyl acrylate are added dropwise after heating to 90°C, and the reaction is continued at 90°C for 3h, followed by washing, extraction, vacuum removal of solvent and small molecular substances, and finally 5 parts of pyridine are added. After reacting for 30 minutes, the fluorinated polysiloxane is obtained.
[0015] By adopting the above technical scheme, the end-vinyl silicone oil is mixed with a platinum catalyst, and a perfluoroalkyl acrylate is added dropwise after heating, and then reacted under specific conditions, followed by washing, extraction and vacuum removal of solvents and small molecules, and finally pyridine is added for reaction to obtain a fluorinated polysiloxane. This process utilizes organic synthesis reactions and introduces the element fluorine, so that the polysiloxane has high surface activity, high heat stability, high chemical stability and hydrophobic properties. The introduced fluorine element significantly improves the hydrophobic properties of the polysiloxane, which enables the final silicone gel to be used in paper box materials. The waterproof performance of the material can be effectively improved. At the same time, due to the introduction of fluorine, the fluorinated polysiloxane also provides higher heat stability and chemical stability, which is crucial to improving the durability and service life of the paper box material. In addition, due to its high surface activity, the fluorinated polysiloxane can also improve the compatibility with other components such as modified starch and hardwood pulp, further improving the overall performance of the paper box material. In summary, the preparation method of fluorinated polysiloxane not only provides excellent waterproof performance for environmentally friendly paper box materials, but also enhances the service life and durability of the materials through its high thermal stability and chemical stability. At the same time, its high surface activity also promotes good compatibility with other components in the material, ensuring the uniformity and consistency of the material performance.
[0016] Preferably, in step S4, the method for preparing the modified starch comprises the following steps: S81, placing 100 parts of corn starch in 700 parts of a solution consisting of 3 parts of sodium hydroxide, 150 parts of sodium chloride and 500 parts of deionized water for 4 hours, filtering and drying to obtain pretreated corn starch; S82. According to the weight ratio, 10 parts of hexamethyldisilazane, 20 parts of 3-aminopropyltrimethoxysilane and 100 parts of anhydrous ethanol are fully mixed to prepare a mixed modifier; S83. According to the mass proportions, 100 parts of pretreated corn starch and 100 parts of mixed modifier were fully mixed at room temperature for 40 minutes, and then ultrasonicated at room temperature for 2 hours, and then transferred into a vacuum mixer. The mixture was heated to 60°C and stirred under reflux conditions of -0.2 MPa for 4 hours. Finally, ethanol was removed under reduced pressure, and modified starch was obtained after drying.
[0017] By adopting the above technical scheme, step S81: pre-treating corn starch: treating corn starch in a solution consisting of sodium hydroxide, sodium chloride and deionized water, filtering and drying to obtain pre-treated corn starch. This process may help to open the structure of starch granules, making it easier for subsequent chemical modification. Pretreatment increases the active sites of starch, making it easier to react with the modifier, improving the modification efficiency and uniformity, and thus enhancing the performance of the modified starch finally obtained. Step S82: preparing a mixed modifier: mixing hexamethyldisilazane and 3-aminopropyltrimethoxysilane with anhydrous ethanol to prepare a mixed modifier. These modifiers contain functional groups that can react with starch hydroxyl groups, such as silazane and silaneoxy groups. Different components in the mixed modifier may have different reactivity and functions, so that the modified starch can obtain multiple functionalities in subsequent treatments, such as enhanced hydrophobicity and improved interfacial compatibility. Step S83: modification reaction and post-treatment: the pretreated corn starch is fully mixed with the mixed modifier, and ultrasonic and vacuum stirring reflux are carried out under specific conditions, and finally the ethanol is removed and dried to obtain modified starch. This process causes a chemical reaction between the starch and the modifier, and introduces new functional groups. Ultrasonic treatment helps to improve the uniformity and efficiency of the reaction, and vacuum stirring reflux ensures the complete reaction. The introduced siloxane group and aminopropyl group not only improve the hydrophobicity of the starch, but also may enhance its compatibility with other components in the pulp, especially the combination with silicone gel, thereby improving the overall performance of the carton material. In summary, the preparation method of the modified starch not only improves the performance of the starch itself through precisely controlled chemical reactions and physical treatment processes, but also ensures its good compatibility with other components in the carton material, thereby significantly improving the mechanical properties and durability of the carton material without affecting the degradability of the material.
[0018] Preferably, in step S5, the process conditions of the extrusion dehydration and shaping are: pressure of 0.5 MPa, so that the dryness reaches 49-50%; the process conditions of the hot press drying are: pressure of 0.7 MPa, temperature of 121-125°C, so that the dryness reaches 98-100%.
[0019] In the second aspect, the present application provides a high-strength and degradable environmentally friendly paper box material, which adopts the following technical solution: As a general technical concept, the present application also provides the above-mentioned high-strength and degradable environmentally friendly paper box material, which is prepared by the above-mentioned method for preparing the high-strength and degradable environmentally friendly paper box material.
[0020] In summary, the beneficial technical effects of this application are: 1. Environmental protection and sustainability: By using waste cardboard as raw material, this method provides a way to recycle waste, reducing environmental pollution and resource waste. At the same time, the prepared paper box material has good degradability, which meets the current high requirements for environmental protection and sustainability.
[0021] 2. Improve material performance: The addition of modified melamine polyphosphate significantly improves the flame retardancy of the paper box material, ensuring that the spread of fire can be effectively delayed in the event of a fire, thereby improving safety in use. The introduction of fluorinated silicone not only enhances the hydrophobicity of the material, but also improves the overall durability of the material due to its high thermal stability and chemical stability.
[0022] 3. Enhanced mechanical properties: The use of modified starch increases the internal bonding strength of the material, and together with cellulose fiber and hardwood pulp, greatly improves the mechanical properties of the carton, such as compression resistance and bending resistance. This ensures the stability and reliability of the carton during load-bearing and transportation.
[0023] 4. Improve processing performance: The use of bio-enzyme method to bleach pulp not only improves the processing efficiency, but also reduces the damage to the fiber due to its high selectivity and specificity, and maintains the integrity and strength of the fiber. At the same time, this method avoids the harmful by-products that may be produced in traditional chemical bleaching, which is more environmentally friendly.
[0024] 5. Cost-effectiveness: The entire preparation process is simple and low-cost. From the selection of raw materials to the optimization of the production process, economic benefits and environmental impacts are taken into consideration, making this method highly practical and market competitive.
[0025] 6. Broad application prospects: Since the obtained paper box material has a variety of excellent properties, such as waterproof, flame retardant, high strength, etc., it can be widely used in food packaging, electronic product packaging, logistics and transportation and other fields to meet the needs of packaging materials in different scenarios. DETAILED DESCRIPTION
[0026] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0027] In the following preparation examples and examples, 1 part means 1 kg.
[0028] Preparation Example 1 Preparation of modified melamine polyphosphate The preparation method of modified melamine polyphosphate comprises the following steps: S61. Prepare an aqueous suspension by mixing 30 parts of hydrotalcite and 30 parts of water in parts by mass; S62, dispersing 300 parts of melamine polyphosphate in a solution consisting of 8 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 80 parts of water according to weight percentage to obtain a mixed solution; S63, slowly drop the water suspension into the mixed solution, heat to 43°C, stir at 300 rpm, react for 35 minutes, filter, and vacuum dry at 80°C for 24 hours, grind and sieve to obtain modified melamine polyphosphate with a particle size of 1-2 μm.
[0029] Preparation Example 2 Preparation of fluorinated polysiloxane The preparation method of the fluorinated polysiloxane is as follows: 100 parts of vinyl-terminated silicone oil and 0.5 parts of platinum catalyst are mixed according to their weight parts, 17 parts of perfluoroalkyl acrylate are added dropwise after heating to 90° C., and the reaction is continued at 90° C. for 3 hours, followed by washing, extraction, vacuum removal of solvents and small molecular substances, and finally 5 parts of pyridine are added. After reacting for 30 minutes, the fluorinated polysiloxane is obtained.
[0030] Preparation Example 3 Preparation of modified starch The preparation method of modified starch comprises the following steps: S81, placing 100 parts of corn starch in 700 parts of a solution consisting of 3 parts of sodium hydroxide, 150 parts of sodium chloride and 500 parts of deionized water for 4 hours, filtering and drying to obtain pretreated corn starch; S82. According to the weight ratio, 10 parts of hexamethyldisilazane, 20 parts of 3-aminopropyltrimethoxysilane and 100 parts of anhydrous ethanol are fully mixed to prepare a mixed modifier; S83. According to the mass proportions, 100 parts of pretreated corn starch and 100 parts of mixed modifier were fully mixed at room temperature for 40 minutes, and then ultrasonicated at room temperature for 2 hours, and then transferred into a vacuum mixer. The mixture was heated to 60°C and stirred under reflux conditions of -0.2 MPa for 4 hours. Finally, ethanol was removed under reduced pressure, and modified starch was obtained after drying.
[0031] Example 1 A method for preparing a high-strength and degradable environmentally friendly paper box material, comprising the following steps: S1. According to the mass fraction, 2 parts of the composite enzyme solution are added into 1000 parts of waste boxboard pulp with a mass concentration of 8% by a metering pump, and the waste boxboard pulp is evenly mixed with the waste boxboard pulp for enzymatic hydrolysis reaction. The enzymatic hydrolysis reaction conditions are: temperature 50°C, pH 7.0, enzymatic hydrolysis time 50 minutes, and the bioenzymatic bleaching process is repeated three times to obtain bleached waste paper pulp. The composite enzyme solution is composed of alkaline pectinase, xylanase, mannanase and ligninase. The activity of the alkaline pectinase is 1000u / ml, the activity of the xylanase is 1800u / ml, the activity of the mannanase is 600u / ml, and the activity of the ligninase is 100u / ml, to obtain bleached waste paper pulp; S2, dispersing 100 parts of 8% bleached waste paper pulp in 200 parts of 10% lithium bromide solution, stirring at 138°C, pouring into a mold, cooling to a gel state, soaking the gel in tap water and deionized water in turn until no precipitation is generated by silver nitrate solution detection, and then soaking in 120 parts of a mixed solution consisting of 10% sodium alginate solution and 30% tert-butanol solution, stirring for 1 hour, and then freeze-drying at -50°C for 2 hours to obtain waste paper aerogel; S3, preparing an organic silicone gel using a siloxane prepolymer, a modified melamine polyphosphate and a fluorinated polysiloxane; the method for preparing the organic silicone gel comprises the following steps: S51, under a nitrogen atmosphere, 10 g of amino-terminated siloxane, 2.1 g of lipoic acid and 20 mL of tetrahydrofuran were mixed, the mixture was kept at 61° C. for 4 h, and the mixture was heated to 80° C. for 3 h to obtain a siloxane prepolymer; S52, 2 g of modified melamine polyphosphate, 10 g of siloxane prepolymer, 0.3 g of fluorinated polysiloxane and 12 mL of tetrahydrofuran were mixed, and ultrasonically dispersed for 60 min to obtain an organosilicon gel; S4, mixing 15 parts of waste paper aerogel, 4 parts of silicone gel, 15 parts of modified starch, 8 parts of cellulose fiber and 50 parts of hardwood pulp with a mass concentration of 10% according to the mass ratio to obtain a pulp mixture; S5. The pulp mixture is made into pulp molding wet blanks by using a paper sheet former, and then extruded and dehydrated to shape, wherein the process conditions of the extrusion and dehydration shaping are: a pressure of 0.5 MPa, so that the dryness reaches 49%; the pulp mixture is transferred to a flat mold and hot-pressed and dried, wherein the process conditions of the hot-pressing and drying are: a pressure of 0.7 MPa, a temperature of 121°C, so that the dryness reaches 98%, thereby obtaining a high-strength and degradable environmentally friendly paper box material.
[0032] Example 2 A method for preparing a high-strength and degradable environmentally friendly paper box material, comprising the following steps: S1. According to the mass fraction, 4 parts of the composite enzyme solution are added into 1000 parts of waste boxboard pulp with a mass concentration of 8% by a metering pump, and the waste boxboard pulp is evenly mixed with the waste boxboard pulp for enzymatic hydrolysis reaction. The enzymatic hydrolysis reaction conditions are: temperature 55°C, pH 8.0, enzymatic hydrolysis time 60 minutes, and the bioenzymatic bleaching process is repeated three times to obtain bleached waste paper pulp. The composite enzyme solution is composed of alkaline pectinase, xylanase, mannanase and ligninase. The activity of the alkaline pectinase is 1500u / ml, the activity of the xylanase is 2200u / ml, the activity of the mannanase is 1000u / ml, and the activity of the ligninase is 150u / ml, to obtain bleached waste paper pulp; S2, dispersing 100 parts of 8% bleached waste paper pulp in 200 parts of 10% lithium bromide solution, stirring at 138°C, pouring into a mold, cooling to a gel state, soaking the gel in tap water and deionized water in turn until no precipitation is generated by silver nitrate solution detection, and then soaking in 120 parts of a mixed solution consisting of 10% sodium alginate solution and 30% tert-butanol solution, stirring for 1 hour, and then freeze-drying at -50°C for 3 hours to obtain waste paper aerogel; S3, preparing an organic silicone gel using a siloxane prepolymer, a modified melamine polyphosphate and a fluorinated polysiloxane; the method for preparing the organic silicone gel comprises the following steps: S51, under a nitrogen atmosphere, 10 g of amino-terminated siloxane, 2.1 g of lipoic acid and 20 mL of tetrahydrofuran were mixed, and the mixture was kept at 65° C. for 5 h, and then the mixture was heated to 83° C. for 3 h to obtain a siloxane prepolymer; S52, 2 g of modified melamine polyphosphate, 10 g of siloxane prepolymer, 0.3 g of fluorinated polysiloxane and 12 mL of tetrahydrofuran were mixed, and ultrasonically dispersed for 70 min to obtain an organosilicon gel; S4, mixing 20 parts of waste paper aerogel, 6 parts of silicone gel, 20 parts of modified starch, 10 parts of cellulose fiber and 55 parts of hardwood pulp with a mass concentration of 10% according to the mass ratio to obtain a pulp mixture; S5. The pulp mixture is made into pulp molding wet blanks by using a paper sheet former, and then extruded for dehydration and shaping. The process conditions of the extrusion dehydration and shaping are as follows: the pressure is 0.5 MPa, so that the dryness reaches 50%; the pulp is transferred to a flat mold and hot-pressed for drying. The process conditions of the hot-pressing and drying are as follows: the pressure is 0.7 MPa and the temperature is 125°C, so that the dryness reaches 100%, thereby obtaining a high-strength and degradable environmentally friendly paper box material.
[0033] Example 3 A method for preparing a high-strength and degradable environmentally friendly paper box material, comprising the following steps: S1. According to the mass fraction, 3 parts of the composite enzyme solution are added into 1000 parts of waste boxboard pulp with a mass concentration of 8% by a metering pump, and the waste boxboard pulp is evenly mixed with the waste boxboard pulp for enzymatic hydrolysis reaction. The enzymatic hydrolysis reaction conditions are: temperature 53°C, pH 7.5, enzymatic hydrolysis time 55 minutes, and the bioenzymatic bleaching process is repeated three times to obtain bleached waste paper pulp. The composite enzyme solution is composed of alkaline pectinase, xylanase, mannanase and ligninase. The activity of the alkaline pectinase is 1200u / ml, the activity of the xylanase is 2000u / ml, the activity of the mannanase is 800u / ml, and the activity of the ligninase is 120u / ml, to obtain bleached waste paper pulp; S2, dispersing 100 parts of 8% bleached waste paper pulp in 200 parts of 10% lithium bromide solution, stirring at 138°C, pouring into a mold, cooling to a gel state, soaking the gel in tap water and deionized water in turn until no precipitation is generated by silver nitrate solution detection, and then soaking in 120 parts of a mixed solution consisting of 10% sodium alginate solution and 30% tert-butanol solution, stirring for 1 hour, and then freeze-drying at -50°C for 2.5 hours to obtain waste paper aerogel; S3, preparing an organic silicone gel using a siloxane prepolymer, a modified melamine polyphosphate and a fluorinated polysiloxane; the method for preparing the organic silicone gel comprises the following steps: S51, under a nitrogen atmosphere, 10 g of amino-terminated siloxane, 2.1 g of lipoic acid and 20 mL of tetrahydrofuran were mixed, the mixture was kept at 63° C. for 4.5 h, and the mixture was heated to 82° C. for 2.4 h to obtain a siloxane prepolymer; S52, 2 g of modified melamine polyphosphate, 10 g of siloxane prepolymer, 0.3 g of fluorinated polysiloxane and 12 mL of tetrahydrofuran were mixed, and ultrasonically dispersed for 65 min to obtain an organosilicon gel; S4, mixing 18 parts of waste paper aerogel, 5 parts of silicone gel, 18 parts of modified starch, 9 parts of cellulose fiber and 53 parts of hardwood pulp with a mass concentration of 10% according to weight parts to obtain a pulp mixture; S5. The pulp mixture is made into pulp molding wet blanks by using a paper sheet former, and then extruded for dehydration and shaping. The process conditions of the extrusion dehydration and shaping are as follows: the pressure is 0.5 MPa, so that the dryness reaches 49.5%; the pulp is transferred to a flat mold and hot-pressed for drying. The process conditions of the hot-pressing and drying are as follows: the pressure is 0.7 MPa and the temperature is 123°C, so that the dryness reaches 99%, thereby obtaining a high-strength and degradable environmentally friendly paper box material.
[0034] Comparative Example 1 The same as Example 3, except that an equal amount of melamine polyphosphate is used instead of modified melamine polyphosphate.
[0035] Comparative Example 2 Same as Example 3, except that an equal amount of corn starch is used instead of modified starch.
[0036] Comparative Example 3 The same as Example 3, except that the amount of fluorinated polysiloxane added is 0 g.
[0037] Comparative Example 4 The same as Example 3, except that an equal amount of amino-terminated siloxane is used instead of the silicone gel.
[0038] The thickness of the high-strength and degradable environmentally friendly paper box material in each embodiment and comparative example is 0.8 mm.
[0039] Performance Testing The high-strength and degradable environmentally friendly paper box materials prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were sampled and subjected to the following tests. The test results are shown in Table 1.
[0040] Flame retardancy test: Cut the sample to be tested into 100×8×0.8mm 3 , put it into a glass combustion tube, pass a nitrogen and oxygen mixed flow, record the minimum oxygen concentration required for combustion, and take the average value of five tests for each group; Hydrophobicity test: 3 μL of deionized water was used as the solvent, and the contact angle was measured with a residence time of 3 s. The result was the average value of five different positions on the surface. The tensile strength and elongation at break were tested using ASTM-D638-14, with a sample width of 10 mm, a length of 100 mm, and a tensile rate of 300 mm / min; The burst resistance test was carried out according to GB / T454-2020, and the burst resistance index (KPa·m 2 / g); Microbial degradation test: 20g of high-strength and degradable environmentally friendly paper box material was buried in soil with a thickness of 10cm. The soil environment contained molds, yeasts, actinomycetes, bacteria and rich carbohydrates. The temperature was 20-45℃, PH>4, and the oxygen atmosphere was aerobic. After 2 consecutive months, the high-strength and degradable environmentally friendly paper box material was weighed and recorded as M. The degradation rate = (20g-M) / 20g*100%.
[0041] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The high-strength and degradable environmentally friendly paper box materials prepared in Examples 1 to 3 have excellent mechanical properties, waterproof properties, flame retardancy, wear and tear resistance, and are degradable. The preparation method of the high-strength and degradable environmentally friendly paper box material of the present application is simple to manufacture and low in cost, and has broad application prospects.
[0042] 2) The performance comparison analysis of the high-strength and degradable environmentally friendly paper box material obtained in combination with Example 3 and Comparative Example 1 shows that by modifying melamine polyphosphate, it has better flame retardant properties and compatibility with other components. The modified melamine polyphosphate can release flame-retardant gases, such as phosphoric acid, during the combustion process, forming a protective layer to slow down the combustion speed and prevent the spread of flames. At the same time, the modified particles are uniform in size, which is conducive to uniform dispersion in the paper box material, thereby significantly improving the flame retardant ability of the paper box material without affecting the degradability of the material.
[0043] 3) The performance comparison analysis of the preparation method of the high-strength and degradable environmentally friendly paper box material prepared in Example 3 and Comparative Example 2 shows that the modified starch, through the introduction of siloxane groups and aminopropyl groups, not only improves the hydrophobicity of the starch, but also may enhance its compatibility with other components in the pulp, especially with the organic silicone gel, thereby improving the overall performance of the paper box material. The preparation method of the modified starch not only improves the performance of the starch itself through the precisely controlled chemical reaction and physical treatment process, but also ensures its good compatibility with other components in the paper box material, thereby significantly improving the mechanical properties and durability of the paper box material without affecting the degradability of the material.
[0044] 4) The performance comparison analysis of the preparation method of the high-strength and degradable environmentally friendly paper box material obtained in combination with Example 3 and Comparative Example 3 shows that the introduced fluorine element significantly improves the hydrophobicity of the polysiloxane, which makes the application of the final silicone gel in the paper box material effectively improve the waterproof performance of the material. At the same time, due to the introduction of fluorine, the fluorine-containing polysiloxane also provides higher heat resistance and chemical stability, which is very important for improving the durability and service life of the paper box material. In addition, due to its high surface activity, the fluorine-containing polysiloxane can also improve the compatibility with other components such as modified starch and hardwood pulp, further improving the overall performance of the paper box material.
[0045] 5) The performance comparison analysis of the preparation method of the high-strength and degradable environmentally friendly paper box material obtained in combination with Example 3 and Comparative Example 4 shows that the prepared silicone gel has excellent toughness, waterproofness and flame retardancy. This silicone gel not only improves the comprehensive performance of the paper box material, but also maintains its environmental protection and degradable characteristics, which meets the dual requirements of high performance and environmental protection in the fields of food packaging.
[0046] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.
Claims
1. A method for preparing a high-strength and degradable environmentally friendly paper box material, characterized in that: The following steps are involved: S1, subjecting waste boxboard paper pulp to a bio-enzymatic bleaching treatment to obtain bleached waste paper pulp; S2, treating the bleached waste paper pulp with lithium bromide and sodium alginate in sequence to obtain waste paper aerogel; S3, preparing silicone gel using siloxane prepolymer, modified melamine polyphosphate and fluorine-containing polysiloxane; S4, mixing 15-20 parts of waste paper aerogel, 4-6 parts of silicone gel, 15-20 parts of modified starch, 8-10 parts of cellulose fiber and 50-55 parts of 10% hardwood pulp by mass to obtain a pulp mixture; S5. The pulp mixture is made into pulp molding wet blanks by using a paper sheet former, and then extruded, dehydrated and shaped, transferred to a flat mold, and hot-pressed and dried to obtain a high-strength and degradable environmentally friendly paper box material.
2. The method for preparing a high-strength and degradable environmentally friendly paper box material according to claim 1, characterized in that: In step S1, the method of the bio-enzymatic bleaching treatment is: according to the mass fraction, 2-4 parts of the composite enzyme solution are added to 1000 parts of waste boxboard pulp with a mass concentration of 8% through a metering pump, so that it is evenly mixed with the waste boxboard pulp for enzymatic hydrolysis reaction. The enzymatic hydrolysis reaction conditions are: temperature 50-55°C, pH 7.0-8.0, enzymatic hydrolysis time 50-60 minutes, and the bio-enzymatic bleaching process is repeated three times to obtain bleached waste paper pulp.
3. The method for preparing a high-strength and degradable environmentally friendly paper box material according to claim 2, characterized in that: The complex enzyme solution consists of alkaline pectinase, xylanase, mannanase and ligninase, the activity of the alkaline pectinase is 1000u / ml-1500u / ml, the activity of the xylanase is 1800u / ml-2200u / ml, the activity of the mannanase is 600u / ml-1000u / ml, and the activity of the ligninase is 100u / ml-150u / ml.
4. The method for preparing a high-strength and degradable environmentally friendly paper box material according to claim 1, characterized in that: In step S2, the preparation method of the waste paper aerogel is as follows: 100 parts of bleached waste paper pulp with a mass concentration of 8% are dispersed in 200 parts of lithium bromide solution with a mass concentration of 10%, stirred at 138°C, poured into a mold, cooled to a gel state, and the gel is soaked in tap water and deionized water in turn until no precipitation is generated by silver nitrate solution detection, and then soaked in 120 parts of a mixed solution consisting of a sodium alginate solution with a mass concentration of 10% and a tert-butanol solution with a mass concentration of 30%, stirred for 1 hour, and then freeze-dried at a temperature of -50°C for 2-3 hours to obtain the waste paper aerogel.
5. The method for preparing a high-strength and degradable environmentally friendly paper box material according to claim 1, characterized in that: In step S3, the method for preparing the organic silicone gel comprises the following steps: S51, under a nitrogen atmosphere, 10 g of amino-terminated siloxane, 2.1 g of lipoic acid and 20 mL of tetrahydrofuran were mixed, and the mixture was kept at 61-65° C. for 4-5 h, and then the mixture was heated to 80-83° C. for 2-3 h to obtain a siloxane prepolymer; S52, 2 g of modified melamine polyphosphate, 10 g of siloxane prepolymer, 0.3 g of fluorine-containing polysiloxane and 12 mL of tetrahydrofuran were mixed, and ultrasonically dispersed for 60-70 min to obtain a silicone gel.
6. The method for preparing a high-strength and degradable environmentally friendly paper box material according to claim 1, characterized in that: In step S3, the preparation method of the modified melamine polyphosphate comprises the following steps: S61. Prepare an aqueous suspension by mixing 30 parts of hydrotalcite and 30 parts of water in parts by mass; S62, dispersing 300 parts of melamine polyphosphate in a solution consisting of 8 parts of γ-aminopropyltrimethoxysilane, 300 parts of ethanol and 80 parts of water according to parts by mass to obtain a mixed solution; S63, slowly drop the water suspension into the mixed solution, heat to 43°C, stir at 300 rpm, react for 30-40 minutes, filter, and vacuum dry at 80°C for 24 hours, grind and sieve to obtain modified melamine polyphosphate with a particle size of 1-2 μm.
7. The method for preparing a high-strength and degradable environmentally friendly paper box material according to claim 5, characterized in that: In step S3, the preparation method of the fluorinated polysiloxane is as follows: 100 parts of terminal vinyl silicone oil and 0.5 parts of platinum catalyst are mixed according to mass parts, 17 parts of perfluoroalkyl acrylate are added dropwise after heating to 90°C, and the reaction is continued at 90°C for 3 hours, and then the solvent and small molecular substances are removed by washing, extraction, and vacuum, and finally 5 parts of pyridine are added. After reacting for 30 minutes, the fluorinated polysiloxane is obtained.
8. The method for preparing a high-strength and degradable environmentally friendly paper box material according to claim 1, characterized in that: In step S4, the method for preparing the modified starch comprises the following steps: S81, placing 100 parts of corn starch in 700 parts of a solution consisting of 3 parts of sodium hydroxide, 150 parts of sodium chloride and 500 parts of deionized water for 4 hours, filtering and drying to obtain pretreated corn starch; S82. According to the weight ratio, 10 parts of hexamethyldisilazane, 20 parts of 3-aminopropyltrimethoxysilane and 100 parts of anhydrous ethanol are fully mixed to prepare a mixed modifier; S83. According to the mass proportions, 100 parts of pretreated corn starch and 100 parts of mixed modifier were fully mixed at room temperature for 40 minutes, and then ultrasonicated at room temperature for 2 hours, and then transferred into a vacuum mixer. The mixture was heated to 60°C and stirred under reflux conditions of -0.2 MPa for 4 hours. Finally, ethanol was removed under reduced pressure, and modified starch was obtained after drying.
9. The method for preparing a high-strength and degradable environmentally friendly paper box material according to claim 1, characterized in that: In step S5, the process conditions of the extrusion dehydration and shaping are: pressure of 0.5 MPa, so that the dryness reaches 49-50%; the process conditions of the hot press drying are: pressure of 0.7 MPa, temperature of 121-125°C, so that the dryness reaches 98-100%.
10. A high-strength and degradable environmentally friendly paper box material, characterized in that: It is prepared according to the method for preparing a high-strength and degradable environmentally friendly paper box material according to any one of claims 1-9.
Citation Information
Patent Citations
Compound, resin composition, and resin molded article
CN102633645A
Preparation method of cationic starch with high substituted degree
CN104497152A
Preparation method of color-developing antibacterial sucrose packaging paper
CN107604752A
Preparation method of modified corn starch adhesive
CN108659751A
High-whiteness coated ivory board and preparation method thereof
CN113668281A