Pair of heat-insulating protective members, method for manufacturing same, method for constructing same, furnace internal member, and heating furnace
By increasing the content and bulk density of the outer peripheral surface of the inorganic binder in the thermally insulating protection member, combined with the distribution of inorganic binder particles, the problems of low economics and insufficient physical strength of the existing thermally insulating materials are solved, and the high temperature environment is achieved. High rigidity and low risk of damage.
Patent Information
- Application Number
- CN202411255594.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-19
- Filing Date
- 2020-07-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing thermal insulation materials have low economic efficiency and insufficient physical strength, and are prone to damage due to scale corrosion or temperature changes in the furnace. Especially during regular repairs, the contact damage caused by contact is more serious.
The inorganic fiber molded body thermal protection member with hollow cylindrical shape increases the content and bulk density of the inorganic binder on the outer peripheral surface side, and combines the distribution of inorganic binder particles to improve the rigidity and bondability of the outer peripheral surface. The inner peripheral surface maintains buffering characteristics to reduce the risk of damage.
It is achieved to improve the rigidity of the outer peripheral surface without losing the buffering characteristics of the inner peripheral surface under high temperature environment, reduce the risk of damage of the insulation protection components, and improve physical strength and construction properties.
Smart Images

Figure CN118936075A_ABST
Abstract
Description
[0001] This application is a divisional application. The application number of the original application is 202080024905.6, the application date is July 9, 2020, and the name of the invention is "Thermal insulation protection component, its manufacturing method, construction method, furnace internal component and heating furnace". Technical Field
[0002] The present invention relates to a heat insulating protective member such as a chute pipe installed in a heating furnace, a construction method thereof, and a heating furnace. Background Art
[0003] As a protective member for a chute pipe in a heating furnace in the steel industry, an inorganic fiber aggregate or an inorganic fiber molded body having high thermal shock resistance is used (Patent Documents 1 to 3).
[0004] Patent Document 1 describes a technique for covering a slideway pipe with an annular heat insulating material made of ceramic fibers produced by punching.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: JP2004-43918A
[0008] Patent Document 2: WO2016 / 076258A1
[0009] Patent Document 3: WO2017 / 195606A1 Summary of the invention
[0010] Problems to be solved by the invention
[0011] However, the economic efficiency of punching is low, and the thermal insulation material of Patent Document 1 is not practical. In addition, the physical strength of the existing annular thermal insulation material composed of inorganic fibers is insufficient, and sometimes it becomes brittle due to scaling corrosion in the furnace or rapid temperature changes caused by heating and cooling. Therefore, when people frequently enter and exit the furnace due to regular repairs, it may be damaged due to contact. The purpose of the present invention is to provide a thermal insulation protection member composed of an inorganic fiber molded body with buffering properties and excellent construction properties and excellent physical strength, a manufacturing method and construction method of the thermal insulation protection member, a furnace internal member, and a heating furnace.
[0012] Means for solving problems
[0013] The present invention proposes a heat insulating protection member that is not easily damaged by contact, by focusing on improving the rigidity of the outer peripheral surface of a hollow cylindrical heat insulating protection member used in a high temperature environment such as in a furnace without impairing the cushioning properties of the inner peripheral surface.
[0014] The gist of the present invention is as follows.
[0015] [1] A thermal insulation protection component, which is a thermal insulation protection component composed of an inorganic fiber molded body having a hollow cylindrical shape or a divided shape of a hollow cylinder, characterized in that the inorganic fiber molded body has an inner peripheral surface (c) facing the hollow, and an outer peripheral surface (a) constituting the outer periphery, and in the inorganic fiber molded body, the closer to the outer peripheral surface (a), the higher the packing density.
[0016] [2] An insulating protective component as described in [1], wherein the middle point between the outer peripheral surface (a) and the inner peripheral surface (c) of the inorganic fiber molding is defined as the middle portion (b), and the packing density (Da) of the outer peripheral surface, the packing density (Db) of the middle portion, and the packing density (Dc) of the inner peripheral surface are in the relationship of Da>Db>Dc.
[0017] [3] The thermal insulation protection member described in [1] or [2], wherein the inorganic fiber molded body contains an inorganic binder, and the content of the inorganic binder increases toward the outer peripheral surface (a).
[0018] [4] An insulating protective component as described in any one of [1] to [3], characterized in that the above-mentioned inorganic fiber molded body is an inorganic fiber molded sintered body containing inorganic binder particles that bind the inorganic fibers together, and the closer to the above-mentioned peripheral surface (a), the more the above-mentioned inorganic binder particles are.
[0019] [5] The heat insulating protection member according to any one of [1] to [4], wherein the heat insulating protection member has a split shape of a hollow cylinder, and the split surfaces are oblique cut surfaces.
[0020] [6] The heat insulating protection member according to any one of [1] to [5], wherein a hole for inserting a pin is provided on an end surface of the heat insulating protection member.
[0021] [7] A furnace internal member having the heat insulating protective member according to any one of [1] to [6] mounted on its outer surface.
[0022] [8] The furnace internal component of [7], wherein the thermal insulation protection member is the thermal insulation protection member of [6], and pins are inserted into the holes of adjacent thermal insulation protection members that connect the end faces.
[0023] [9] The furnace internal member according to [7] or [8], comprising sheet-like inorganic fibers covering the thermal insulation protection member mounted on the furnace internal member.
[0024]
[10] A method for constructing a heat insulating protective member, comprising the step of assembling the heat insulating protective member of any one of [1] to [6] on the outer surface of a furnace internal member.
[0025]
[11] A method for constructing a thermal insulation protection member as described in
[10] , wherein the thermal insulation protection member is the thermal insulation protection member of [6], and pins are inserted into the holes of adjacent thermal insulation protection members that connect the end faces.
[0026]
[12] A method for constructing a heat insulating protective member as described in
[10] or
[11] , which comprises the step of filling a filler of inorganic fibers in the gap between the end surface of the heat insulating protective member and the furnace internal component after assembling the heat insulating protective member.
[0027]
[13] A method for constructing a thermal insulation protection member according to any one of
[10] to
[12] , comprising the step of covering the thermal insulation protection member with sheet-like inorganic fibers after assembling the thermal insulation protection member.
[0028]
[14] A heating furnace comprising the furnace internal component according to any one of [6] to [9].
[0029]
[15] A heating furnace as described in
[14] , wherein the above-mentioned furnace internal component is a slide column.
[0030]
[16] A method for manufacturing a thermal insulation protection component, which is a method for manufacturing a thermal insulation protection component according to any one of [1] to [6], comprising the following steps: a step of laminating an inorganic fiber blanket between an inner mold and an outer mold to form a hollow cylindrical molded body; a step of subsequently immersing the hollow cylindrical molded body in a liquid containing an inorganic binder; a step of pulling the hollow cylindrical molded body out of the liquid containing the inorganic binder and removing the liquid containing the inorganic binder by suction from the inner peripheral surface side to the outer peripheral surface side of the hollow cylindrical molded body; and a step of drying the hollow cylindrical molded body.
[0031]
[17] The method for producing a thermal insulation protective member as described in
[16] , which comprises the step of pressing and compressing the hollow cylindrical molded body of the stacked inorganic fiber blanket.
[0032]
[18] A method for manufacturing an insulating protective component as described in
[16] or
[17] , characterized in that the inner mold and the outer mold are arranged in a suction dehydration container, and the inner mold and the outer mold have a plurality of holes extending along a direction orthogonal to the axial core line of the inner mold.
[0033] Effects of the Invention
[0034] The heat insulating protective member of the present invention is impregnated with an inorganic binder, and contains more inorganic binder on the outer peripheral side than on the inner peripheral side, so that the packing density on the outer peripheral side is high. Thus, the inorganic binder can improve the rigidity of the outer peripheral surface without damaging the buffering properties of the inner peripheral surface while improving the integral bonding of the heat insulating protective member.
[0035] In addition, the heat insulating protective member of the present invention is an inorganic fiber molded fired body, and the inorganic binder particles as the fired product of the inorganic binder are more on the outer peripheral surface than on the inner peripheral surface, and the packing density on the outer peripheral surface side is high. Therefore, the inorganic binder particles can improve the rigidity of the outer peripheral surface without damaging the buffering properties of the inner peripheral surface while improving the integral bonding of the heat insulating protective member. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a perspective view showing a method of manufacturing a heat insulating protective member according to an embodiment.
[0037] Figure 2 It is a cross-sectional view showing a method of manufacturing a heat insulating protective member according to an embodiment.
[0038] Figure 3 It is a cross-sectional view showing a method of manufacturing a heat insulating protective member according to an embodiment.
[0039] Figure 4 It is a cross-sectional view showing a method of manufacturing a heat insulating protective member according to an embodiment.
[0040] Figure 5 It is a cross-sectional view showing a method of manufacturing a heat insulating protective member according to an embodiment.
[0041] Figure 6 It is a cross-sectional view showing a method of manufacturing a heat insulating protective member according to an embodiment.
[0042] Figure 7 It is a perspective view showing an example of a heat insulating protective member according to the embodiment.
[0043] Figure 8 It is a perspective view showing an example of a heat insulating protective member according to the embodiment.
[0044] Fig. 9 It is a perspective view showing an example of the internal components of the furnace.
[0045] Fig.10 It is a perspective view showing a construction method of a heat insulating protective member according to an embodiment.
[0046] Fig.11 It is a perspective view showing a construction method of a heat insulating protective member according to an embodiment.
[0047] Fig.12 middle, Fig.12 a is a perspective view showing a method for constructing a heat insulating protective member according to an embodiment, Fig.12 b is Fig.12 a is a cross-sectional view taken along line XIb-XIb. DETAILED DESCRIPTION
[0048] The following reference Figures 1 to 12 b. The embodiment will be described. It should be noted that in the following description, the heat insulating protection member is mounted on the chute pipe, but it may also be mounted on other furnace internal members such as the chute beam.
[0049] It should be noted that, unless otherwise specified, the description “a to b” expressing a numerical range means “a or more and b or less” and also includes the meanings of “preferably greater than a” and “preferably less than b”.
[0050] In addition, even if the upper limit and the lower limit of the numerical range in the present specification are slightly outside the numerical range specified in the present invention, they are included in the equivalent range of the present invention as long as the same functions and effects as those in the numerical range are achieved.
[0051] like Fig. 9 As shown, the slide pipe 1 to which the heat insulation protection member is constructed is a tubular shape made of heat-resistant steel and is vertically installed from the hearth G of the heat treatment furnace. The slide beam 2 is provided in a manner supported by a plurality of slide pipes 1. A refractory coating layer 3 composed of a refractory castable is applied to the upper part of the slide pipe 1. In the present invention, the heat insulation protection member is constructed on the slide pipe on the lower side of the refractory coating layer 3 in the slide pipe 1.
[0052] A plurality of anchor bolts (not shown) are provided on the slide pipe 1 at intervals in the height direction.
[0053] The cross section of the slide pipe 1 is not a perfect circle, so it is preferred to form a base layer 5 (see Fig.12 b) Covering the outer peripheral surface of the chute pipe 1. This can improve the adhesion between the outer peripheral surface and the heat insulating protective member 10, and can exhibit a higher heat insulating effect. The base layer 5 is composed of inorganic fibers, castable refractory materials, and the like.
[0054] In the present invention, two or more heat insulating protective members 10 made of a needle punched blanket of inorganic fibers (alumina / silica based fibers in the present embodiment) are attached to the chute pipe 1 in multiple vertical stages.
[0055] like Figure 8 As shown, the heat insulating protection member 10 is in the shape of a hollow cylinder roughly split in half, and is butt-jointed and assembled in such a way that the slideway pipe 1 is clamped by a pair of heat insulating protection members 10 .
[0056] like Fig.10As shown, after a pair of heat insulating protection members 10 are mounted on the lowermost portion of the chute pipe 1, pins 12 made of refractory material (alumina in this embodiment) are inserted into holes 11 on the upper end surfaces of the heat insulating protection members 10 and made to stand upright.
[0057] Next, a pair of heat insulating protective members 10 as the second stage from the bottom is mounted on the slide pipe 1. At this time, the pin 12 protruding from the heat insulating protective member 10 on the lower stage side is inserted into the hole 11 on the lower end surface of the heat insulating protective member 10 of the second stage. In addition, the pin 12 is inserted into the hole 11 on the upper end surface of the heat insulating protective member 10 of the second stage and made to stand up.
[0058] After the second stage of the heat insulating protective member 10 is assembled, the third and subsequent stages of the heat insulating protective member 10 are assembled to the slideway pipe 1 in the same manner.
[0059] In order to prevent the gap formed by the butted surfaces of the heat insulating protection members 10 butted against each other so as to sandwich the slide tube 1 from continuing between the upper and lower adjacent heat insulating protection members 10 , it is preferred that the orientation of the heat insulating protection members 10 be different for each stage.
[0060] like Fig.11 As shown, the top segment ( Fig.11 After the thermal insulation protection component 10 (the third section in the figure) is assembled on the slide pipe 1, a filler 13 consisting of a needle-punched blanket of inorganic fibers (alumina / silica fibers in this embodiment) is pressed between the upper end surface of the uppermost thermal insulation protection component 10 and the refractory coating layer 3.
[0061] It should be noted that a paste-like heat-resistant adhesive composition may be attached to the butting surfaces of the heat-insulating protection members 10 and the inner peripheral surface of the heat-insulating protection members 10. The heat-resistant adhesive composition is preferably a composition obtained by kneading a pulverized inorganic fiber and refractory clay such as kaolinite with water.
[0062] After the filling material 13 is filled as described above, Fig.12 As shown in Figs. 12a and 12b, the undried blanket 15 impregnated with an inorganic binder is wound around the outer peripheral surface of each heat insulating protective member 10, and the construction is completed. The undried blanket 15 impregnated with an inorganic binder is dried and fired by undergoing a temperature increase and heating process after the heating furnace starts to operate, and becomes a blanket containing an oxide-based refractory composition.
[0063] By winding the blanket 15 , it is possible to effectively prevent hot air from intruding into the heat insulating protection member attached to the chute pipe 1 .
[0064] Next refer to Figures 1 to 8 A method for manufacturing the heat insulating protective member 10 will be described.
[0065] like Figure 1, 2 As shown, an inner mold 20 having a bottomed hollow cylindrical shape and having a bottom surface 21 and a side peripheral portion 22 is prepared. A plurality of holes 23 penetrating from the inner peripheral surface to the outer peripheral surface are provided in the side peripheral portion 22. The bottom surface 21 is not provided with a hole.
[0066] After a release sheet (not shown) made of a glass fiber sheet or the like is wound around the outer circumferential surface of the inner mold 20, a needle-punched blanket 30 of inorganic fibers (alumina fibers in this embodiment) is stacked and filled between the inner mold and the outer mold. The size and shape of the needle-punched blanket are not particularly limited, and it is preferably processed according to the size of the thermal insulation protection component (the length from the inner circumferential surface side to the outer circumferential surface side, the length of the inner circumferential surface). For example, the needle-punched blanket of inorganic fibers is preferably processed to a length equal to the circumference of the inner mold 20 for use. In addition, the needle-punched blanket of inorganic fibers is preferably processed to a width equal to the length from the inner circumferential surface side to the outer circumferential surface side in the cross-sectional shape of the hollow cylinder of the target thermal insulation protection component.
[0067] In one embodiment, if Figure 2 As shown, a first outer mold 40 is disposed to surround the inner mold 20 , and the needle punched blanket 30 is pressed between the side peripheral portion 42 of the outer mold 40 and the side peripheral portion 22 of the inner mold 20 to fill the needle punched blanket 30 .
[0068] The outer mold 40 is a bottomed hollow cylindrical shape having a bottom portion 41 and a side peripheral portion 42. The inner mold 20 is coaxially arranged in the outer mold 40 so that the bottom portion 21 overlaps the bottom portion 41. A plurality of holes 43 are provided through the side peripheral portion 42. A flange 44 is provided at the upper end of the side peripheral portion 42.
[0069] The height of the outer mold 40 is preferably lower than that of the inner mold 20. In this embodiment, the height of the outer mold 40 is about half of that of the inner mold 20. After two or more needle punched blankets 30 are filled between the inner mold and the outer mold until they reach the vicinity of the upper end of the outer mold 40, a second outer mold 50 is arranged on the upper side of the outer mold 40. The second outer mold 50 is in the shape of a hollow cylinder and has the same diameter as the outer mold 40. A plurality of holes 53 are also provided in the outer mold 50. Flanges 54 and 55 are provided at the lower end and the upper end of the outer mold 50, respectively.
[0070] The flanges 44 and 54 of the outer molds 40 and 50 are overlapped and fastened with bolts to form an integrated body.
[0071] like Figure 3 As shown, the needle punched blanket 30 is also filled between the second outer mold 50 and the inner mold 20. Figure 3 After the needle punched blanket 30 is filled to the top, as shown in Figure 4As shown, the annular plate 61 of the press-in fixture 60 is pressed between the inner mold 20 and the second outer mold 50 to compress the needle punched blanket 30 wound between the inner mold 20 and the outer molds 40, 50, thereby forming a hollow cylindrical molded body 30A that integrates the needle punched blanket 30. It should be noted that the compression can also be performed by screwing in the bolt 62 described below.
[0072] The jig 60 includes an annular plate 61 and a cover plate 63. An opening 64 is provided in the center of the cover plate 63. The cover plate 63 is connected to the upper flange 55 of the second outer mold 50 by bolts (not shown), etc., and the annular plate 61 is pressed by bolts 62 to maintain the compressed state of the hollow cylindrical molded body 30A.
[0073] Afterwards, if Figure 5 As shown, the integrated body 80 of the inner mold 20, the hollow cylindrical molded body 30A, the outer molds 40, 50 and the clamp 60 is immersed in the liquid L containing the inorganic binder in the tank 81 so that the liquid containing the inorganic binder is fully impregnated in the hollow cylindrical molded body 30A.
[0074] Then, the integrated object 80 is pulled up from the liquid L containing the inorganic binder, as shown in FIG. Figure 6 As shown, it is arranged in a suction dehydration container 70. On the flange at the upper end of the container 70, the peripheral edge of the cover plate 63 is placed with a gasket 74 interposed therebetween.
[0075] The inside of the container 70 is sucked through the suction port 75 at the lower portion of the container 70. As a result, the liquid L containing the inorganic binder stored in the inner mold 20 is sucked out of the outer molds 40 and 50 through the hole 23 of the inner mold 20, the hollow cylindrical molded body 30A, and the holes 43 and 53 of the outer molds 40 and 50, and is discharged through the suction port 75. At this time, air flows into the inner mold 20 through the opening 64.
[0076] After suction is performed for a predetermined time, the opening 64 is connected to a hot air source (not shown) and suction is continued, whereby hot air passes through the hollow cylindrical molded body 30A to dry the hollow cylindrical molded body 30A.
[0077] After the hollow cylindrical molded body 30A is dried, the integrated body 80 of the inner mold 20, the hollow cylindrical molded body 30A, the outer molds 40, 50 and the clamp 60 is taken out of the container 70, the clamp 60 and the outer molds 40, 50 are removed, and then the inner mold 20 is demolded from the hollow cylindrical molded body 30A to obtain Figure 7 The hollow cylindrical molded body 30A is shown.
[0078] The upper and lower end surfaces of the hollow cylindrical molded body 30A are bored with holes 11. The method of boring is not particularly limited, but for example, a punch is preferably used from the viewpoint of dimensional accuracy.
[0079] Then, if Figure 8 As shown, the hollow cylindrical molded body 30A is cut in a direction parallel to the core line of the cylinder axis to produce a hollow cylindrical heat insulating protection member 10 divided in half. The cut surface 10c is oblique to the diameter direction of the hollow cylindrical molded body 30A.
[0080] The heat insulating protective member 10 manufactured in this way is usually shipped in the manufactured form and assembled in a furnace structure such as a chute pipe.
[0081] However, the thermal insulation protection member manufactured as described above may be further fired, naturally cooled, and then shipped as a thermal insulation protection member product.
[0082] When a pair of heat insulating protective members 10 are combined to form a hollow cylindrical shape, the axial length of the cylinder is preferably 100 to 600 mm, particularly 150 to 400 mm, and the thickness is preferably about 20 to 100 mm, particularly 30 to 80 mm.
[0083] According to the manufacturing method of the thermal insulation protection member 10, an inorganic binder such as Figure 5 , 6 As shown, the inorganic binder is impregnated in the entirety of the thermal insulation protection member 10. In this way, by impregnating the entirety of the thermal insulation protection member, the thermal insulation protection member can be made into an inorganic fiber molding that is not easily delaminated. Figure 6 As shown, since the liquid containing the inorganic binder is sucked from the inner mold 20 to the outer mold 40, 50 side, Figure 7 In the hollow cylindrical molded body 30A, the closer to the outer peripheral surface side, the greater the content of the inorganic binder. After the thermal insulation protection member 10 is fired, the inorganic binder forms inorganic binder particles and plays a role in bonding the fibers together. Therefore, the greater the content of the inorganic binder, the greater the amount of inorganic binder particles attached to the thermal insulation protection member 10 after firing, and the higher the rigidity, that is, the physical strength, of the outer peripheral surface of the thermal insulation protection member 10.
[0084] However, when the content of the inorganic binder is high, the weight of the thermal insulation protection member 10 increases. In this embodiment, since the content of the inorganic binder on the outer peripheral surface side of the thermal insulation protection member 10 is high, the strength and rigidity of the outer peripheral surface side of the thermal insulation protection member 10 are high. In addition, since the content of the inorganic binder on the inner peripheral surface side of the thermal insulation protection member 10 is low, the bulk density of the inner peripheral surface side of the thermal insulation protection member 10 is reduced.
[0085] [Material of the Heat Insulation Protection Member 10, etc.]
[0086] The needle punched blanket 30 used for manufacturing the thermal insulation protection member 10 is not particularly limited as long as it is made of inorganic fibers, but is preferably a needle punched blanket made of inorganic fibers as described below.
[0087] The needle punched blanket is preferably a blanket obtained by needle punching an inorganic fiber aggregate substantially free of fibers having a fiber diameter of 3 μm or less. By using such a needle punched blanket, the wind erosion resistance of the heat insulating protective member for a slide pipe of the present invention can be improved.
[0088] <Inorganic Fiber>
[0089] There is no particular limitation on the inorganic fibers that constitute the needle-punched blanket, and examples include single fibers or composite fibers of silica, alumina / silica, zirconia containing these fibers, spinel, titanium dioxide, and calcium oxide. From the perspectives of heat resistance, fiber strength (toughness), and safety, alumina / silica fibers, especially polycrystalline alumina / silica fibers, are particularly preferred.
[0090] The alumina / silica composition ratio (mass ratio) of the alumina / silica fibers is preferably in the range of 65 to 98 / 35 to 2, which is called a mullite composition or a high alumina composition, more preferably 70 to 95 / 30 to 5, and particularly preferably 70 to 74 / 30 to 26.
[0091] In the present invention, it is preferred that 80% by mass or more, preferably 90% by mass or more, and particularly preferably the entire amount of the inorganic fiber is polycrystalline alumina / silicon dioxide-based fiber composed of the above-mentioned mullite. In addition, the molar ratio of Ca to Al in the inorganic fiber (Ca / Al) is preferably 0.03 or less, and particularly preferably the inorganic fiber does not contain Ca.
[0092] The inorganic fibers preferably do not substantially contain fibers having a fiber diameter of 3 μm or less. Here, “does not substantially contain fibers having a fiber diameter of 3 μm or less” means that fibers having a fiber diameter of 3 μm or less account for 0.1% by mass or less of the total fiber weight.
[0093] The average fiber diameter of the inorganic fibers is preferably 5 to 7 μm. If the average fiber diameter of the inorganic fibers is too thick, the resilience and toughness of the fiber aggregate will be lost; if it is too thin, the amount of dust suspended in the air will increase, and the probability of containing fibers with a fiber diameter of less than 3 μm will increase.
[0094] <Method for producing needle punched blanket>
[0095] An inorganic fiber aggregate having the above-mentioned suitable average fiber diameter and substantially containing no fibers with a fiber diameter of less than 3 μm can be obtained by controlling the viscosity of the spinning solution, controlling the air flow for the spinning nozzle, controlling the drying of the drawn yarn, and controlling the needle punching, etc. in the production of the inorganic fiber aggregate using the sol-gel method.
[0096] The needle punched blanket can be manufactured by the following steps as described in the conventionally known method, for example, Japanese Patent Gazette No. 2014-5173: a step of obtaining an aggregate of inorganic fiber precursors by a sol-gel method; a step of subjecting the obtained aggregate of inorganic fiber precursors to a needle punching treatment; and a step of calcining the aggregate of inorganic fiber precursors after the needle punching treatment to obtain an inorganic fiber aggregate.
[0097] <Needle density, bulk density and thickness of needle punched blanket>
[0098] The needle density of the needle punched blanket is preferably 2 to 200 needles / cm. 2 , especially 2 to 150 needles / cm 2 , especially 2 to 100 needles / cm 2 , especially 2 to 50 needles / cm 2 If the needle density is too low, the thickness uniformity of the needle punched blanket decreases and the heat shock resistance decreases. If it is too high, the fibers may be damaged and may be easily scattered after firing.
[0099] The bulk density of the needle punched blanket is preferably 50 to 200 kg / m 3 (0.05~0.2g / cm 3 ), more preferably 80 to 150 kg / m 3 (0.08~0.15g / cm 3 If the bulk density is too low, the inorganic fiber molded body becomes fragile; on the other hand, if the bulk density is too high, the mass of the inorganic fiber molded body increases, and the rebound force is lost, resulting in a molded body with low toughness.
[0100] The surface density of the needle punched blanket is preferably 500 to 4000 g / m 2 , particularly preferably 600 to 3800 g / m 2 , particularly preferably 1000 to 3500 g / m 2 If the surface density of the needle punched blanket is too small, the fiber content is small, and only an extremely thin molded body can be obtained, which reduces the usefulness of the inorganic fiber molded body for thermal insulation; if the surface density is too large, the fiber content is too large, making it difficult to control the thickness based on the needle punching process.
[0101] The thickness of the needle punched blanket 30 ( Figure 1The thickness in the vertical direction is preferably about 3 to 30 mm, particularly preferably about 5 to 15 mm, and the width is preferably about 20 to 100 mm, particularly preferably about 30 to 80 mm.
[0102] [Inorganic binder]
[0103] The inorganic binder impregnated in the needle punched blanket is not particularly limited as long as it is an inorganic binder such as an inorganic sol and a metal salt, or a mixture thereof that forms an oxide after firing. Specific examples are given below, but the present invention is not limited thereto.
[0104] As the inorganic sol, alumina sol, zirconia sol, titania sol or magnesia sol, calcium oxide sol, etc. can be cited. In addition, as the metal salt, organic acid salts of formic acid, acetic acid, citric acid, oxalic acid, benzoic acid, malic acid, etc., and inorganic acid salts of nitric acid, etc. of the above-mentioned metal species can be cited. Among them, alumina sol is preferred from the aspect that the thermal expansion coefficient value is close to that of the inorganic fiber aggregate. As the inorganic binder, two or more inorganic sols can be used.
[0105] The concentration of the liquid containing the inorganic binder is preferably 6 to 14 wt %, particularly preferably 8 to 11 wt % based on the solid content. In addition, the viscosity of the liquid containing the inorganic binder is preferably adjusted to 5 to 200 cp.
[0106] [Configuration of the Heat Insulating Protective Member 10]
[0107] The heat insulating protective member of the present invention is composed of an inorganic fiber molded body having an inner peripheral surface (c) constituting a hollow and an outer peripheral surface (a) constituting an outer periphery, and the bulk density increases toward the outer peripheral surface (a). Here, a method for measuring the bulk density is described.
[0108] That is, in the inorganic fiber molded body, in the cross section connecting the inner peripheral surface (c) and the outer peripheral surface (a), the 1 / 3 area on the inner peripheral surface (c) side is set as the inner peripheral area, the 1 / 3 area on the outer peripheral surface (a) side is set as the outer peripheral area, and the 1 / 3 area between the outer peripheral area and the inner peripheral area is set as the middle area. In addition, the middle point between the above-mentioned outer peripheral surface (a) and the above-mentioned inner peripheral surface (c) of the inorganic fiber molded body is set as the middle part (b). In the present invention, the measurement positions of the bulk density (C) and the inorganic binder adhesion amount (B) of each area are as follows. For example, the entire inorganic fiber molded body constituting the thermal insulation protection component, or an inorganic fiber molded body of any size cut in a manner that has a cross section in a direction perpendicular to the hollow axis in the thermal insulation protection component, is divided into three equal parts in the above-mentioned cross section as the outer peripheral area, the middle area, and the inner peripheral area. In addition, with respect to the packing density of the inner circumferential surface (Dc), the packing density of the inner circumferential area (for example, the range from the inner circumferential surface to 12 mm) is measured, with respect to the packing density of the outer circumferential surface (Da), the packing density of the outer circumferential area (for example, the range from the outer circumferential surface to 12 mm) is measured, and with respect to the packing density of the middle portion (Db), the packing density in the middle region is measured.
[0109] It should be noted that, in the present invention, "the closer to the outer peripheral surface (a) side, the higher the above-mentioned bulk density" means that the bulk density on the outer peripheral surface side is higher than the bulk density on the inner peripheral surface side, and the bulk density does not necessarily change continuously from the inside to the outside. Here, "inner peripheral surface side" refers to a portion that is relatively closer to the inner peripheral surface (c) than the outer peripheral surface (a), and "outer peripheral surface side" refers to a portion that is relatively closer to the outer peripheral surface (a) than the inner peripheral surface (c).
[0110] Therefore, for example, the value of the above-mentioned bulk density may increase sharply from the inner peripheral surface (c) to the middle part (b), and increase gently from the middle part (b) to the outer peripheral surface (a). Alternatively, it may be constant from the inner peripheral surface (c) to the middle part (b), and increase from the middle part to the outer peripheral surface (a). Alternatively, there may be a region with high bulk density in the form of dots in the middle part (b), and the bulk density value may decrease temporarily toward the outer peripheral surface (a) and then increase.
[0111] However, from the perspective of significantly improving the physical strength based on contact, the bulk density of the inorganic fiber molding constituting the thermal insulation protection member of the present invention is preferably in the relationship of Da>Db>Dc, and more preferably increases continuously from the inner peripheral surface (c) to the outer peripheral surface (a).
[0112] The bulk density (Dc) of the inner peripheral surface is lower than the bulk density (Da) of the outer peripheral surface, and is preferably about 50 to 99 mass %, more preferably 60 to 95 mass %, and particularly preferably about 70 to 90 mass %.
[0113] In addition, the bulk density (Db) of the middle portion is less than the bulk density (Da) of the outer peripheral surface and greater than the bulk density (Dc) of the inner peripheral surface. The bulk density (Db) of the middle portion is preferably 75 to 99% by mass, more preferably 80 to 98% by mass, and particularly preferably about 85 to 97% by mass relative to the bulk density (Da) of the outer peripheral surface. It should be noted that the bulk density (kg / m 3 ) can be found by dividing the weight by the volume.
[0114] In the heat-insulating protective member of the present invention, the amount of inorganic binder attached (the amount of attachment in terms of solid content) increases as the distance to the outer peripheral surface (a) increases. That is, the amount of binder attached to the outer peripheral surface (Ba), the amount of binder attached to the middle portion (Bb), and the amount of binder attached to the inner peripheral surface (Bc) are preferably in the relationship of Ba>Bb>Bc.
[0115] The amount of inorganic binder attached to the inner surface (Bc) is less than the amount of binder attached to the outer surface (Ba), preferably 0.1 to 50% by mass, more preferably 0.5 to 30% by mass, and particularly preferably about 1.0 to 20% by mass. In addition, the amount of binder attached to the middle portion (Bb) is less than the amount of binder attached to the outer surface (Ba) and greater than the amount of binder attached to the inner surface (Bc). The amount of binder attached to the middle portion (Bb) is preferably 10 to 95% by mass, more preferably 20 to 90% by mass, and particularly preferably about 30 to 80% by mass relative to the amount of binder attached to the outer surface (Ba).
[0116] The amount of adhesive (Ba) in the outer peripheral region of the heat insulating protective member 10 of the present invention is preferably 2 to 70 parts by mass, more preferably 2 to 50 parts by mass, based on 100 parts by mass of the inorganic fibers in terms of oxide (eg, Al 2 O 3 ).
[0117] The amount of adhesive (Bc) in the inner peripheral region of the heat insulating protective member 10 of the present invention is preferably 0.5 to 40 parts by mass, more preferably 0.5 to 40 parts by mass, based on 100 parts by mass of the inorganic fibers in terms of oxide (eg, Al2O3).
[0118] The amount of binder adhesion (Bb) in the middle region of the heat insulating protective member 10 of the present invention is preferably 2 to 55 parts by mass, more preferably 2 to 35 parts by mass, based on 100 parts by mass of the inorganic fibers, in terms of oxide (eg, Al 2 O 3 ).
[0119] The amount of the inorganic binder attached to the entire thermal insulation member (calculated as oxide) is preferably 5 to 40 parts by mass, particularly preferably 8 to 30 parts by mass, based on 100 parts by mass of the inorganic fibers in the entire thermal insulation member.
[0120] In one embodiment, the thermal insulation protection component of the present invention is an inorganic fiber molded body (a molded body formed by impregnating a liquid containing an inorganic binder, drying, and attaching) containing inorganic binder particles that bind inorganic fibers together. In the inorganic fiber molded body, the closer to the peripheral surface (c) side, the greater the amount of the inorganic binder particles attached. The inorganic binder particles are not particularly limited, but are preferably particles with an average particle size of 20 to 35 nm. It can be considered that when more inorganic binder particles are contained in the inorganic fiber molded body, the adhesion between the inorganic fibers constituting the inorganic fiber molded body can be improved, and the gaps between the inorganic fibers can be filled, thereby increasing the rigidity of the peripheral surface side.
[0121] In one embodiment, the heat insulating protective member of the present invention is an inorganic fiber molded fired body formed by firing the above-mentioned inorganic fiber molded body. In this mode, the inorganic binder particles, which are the fired product of the inorganic binder, are also more present on the outer peripheral side of the inorganic fiber molded fired body than on the inner peripheral side, and the packing density on the outer peripheral side is high. Therefore, the inorganic binder particles improve the integral bonding of the heat insulating protective member while also improving the rigidity of the outer peripheral side. The inorganic binder particles can be observed, for example, using various microscopes.
[0122] In one embodiment, the heat insulating protective member of the present invention is preferably composed of an inorganic fiber molded body or an inorganic fiber molded and fired body, and the packing density increases toward the lower part in the vertical direction.
[0123] In one embodiment, the heat insulating protective member of the present invention is preferably a single-layer structure in any cross section connecting the inner peripheral surface (c) and the outer peripheral surface (a). Specifically, for example, an inorganic fiber blanket wound once in a direction parallel to the axis of the hollow, an inorganic fiber blanket stacked in a direction perpendicular to the axis of the hollow, etc. can be cited.
[0124] The heat insulating protective member of the present invention is preferably composed of an inorganic fiber blanket layered in the axial direction of the hollow portion.
[0125] [Furnace internals]
[0126] The furnace internal component of the present invention is a furnace internal component having the above-mentioned heat insulation protection component installed on the outer surface. The furnace internal component is not particularly limited, and preferably has a curved surface, especially a cylindrical surface. For example, it is a slide column (a component formed by installing the heat insulation protection component of the present invention on a slide pipe), a slide beam, etc. Among them, in the present invention, the slide column is preferably used for the contribution of the improvement effect of the rigidity of the outer peripheral surface side.
[0127] As one embodiment of the in-furnace component of the present invention, an undried blanket 15 with an inorganic binder attached is wound around the outer periphery of the thermal insulation protection component 10 for construction. The undried blanket 15 with an inorganic binder attached is dried and fired by undergoing a temperature increase and heating process after the heating furnace starts to operate, and becomes a blanket containing an oxide-based refractory composition. By winding the above-mentioned blanket 15, it is possible to effectively prevent hot air from invading the thermal insulation protection component assembled on the chute pipe 1, so it is preferred. As the undried blanket 15 with an inorganic binder attached, it is preferred that the needle-punched blanket of the above-mentioned inorganic fibers with a thickness of about 10 to 30 mm is impregnated with the above-mentioned inorganic binder in a ratio of 2 to 50 parts by mass relative to 100 parts by mass of the inorganic fibers.
[0128] One embodiment of the furnace internal component of the present invention is a furnace internal component formed by inserting pins into holes of adjacent heat insulating protection members that butt against each other's end faces using heat insulating protection members having pins inserted into their end faces.
[0129] As one embodiment of the furnace internal component of the present invention, there is a sheet-like inorganic fiber covering the thermal insulation protection component of the present invention assembled on the furnace internal component. That is, a layer of inorganic fibers can be formed on the outer side of the outer peripheral surface of the inorganic fiber molding constituting the thermal insulation protection component of the present invention to form the outermost layer. In this case, the packing density of the outermost layer can be equal to the packing density (Da) of the peripheral part, or it can be less than or greater than the packing density (Da) of the peripheral part. It should be noted that from the perspective of exerting the effect of improving the physical strength based on contact, the packing density of the outermost layer in the case of further forming the outermost layer is preferably greater than the packing density (Da) of the peripheral part.
[0130] [Heating furnace]
[0131] The heating furnace of the present invention has a furnace internal structure to which the heat insulating protective member of the present invention is mounted.
[0132] Example
[0133] In the following Examples and Comparative Examples, the following ball drop test was performed in order to evaluate the rigidity of the outer peripheral surface side of the heat insulating protective member, assuming that the physical strength of the furnace internal member was evaluated.
[0134] [Definition of the drop ball test]
[0135] The sample was processed into an area of 100 mm×50 mm×30 mm thick, and a steel ball of 550 g was dropped from a height of 60 cm into the center of the sample. The difference in thickness of the center of the sample before and after the test was taken as the depth of the dent.
[0136] [Example 1]
[0137] Polycrystalline alumina / silica fibers containing 72% by mass of alumina and 28% by mass of silica, with an average fiber diameter of 5.5 μm and substantially no fibers with a fiber diameter of 3 μm or less, were accumulated and needle-punched to prepare a needle-punched blanket (trade name: Mitsubishi Chemical MAFTEC MLS-2, thickness 7.5 mm, bulk density 155 kg / m 3 ), and the needle punched blanket is processed into a size of 40 mm in width × 1150 mm in length to form a needle punched blanket 30.
[0138] like Figures 1 to 8 As shown, a glass cloth with a thickness of 0.5 mm (manufactured by Chukoh Chemical Industry Co., Ltd.: CHUKOH FLO (registered trademark) G type fabric) as a release sheet is wound around the inner mold once. Thereafter, the needle punched blanket 30 is stacked in multiple stages between the inner mold 20 and the outer mold 40 .
[0139] Next, the jig 60 was used to compress the laminated material to form an integrated product 80. The integrated product 80 was immersed in a liquid L containing an inorganic binder and composed of alumina sol (Nissan Chemical Co., Ltd. Alumina Sol 200) with a solid content concentration of 9.6% by weight for 24 hours, so that 17 kg of the liquid was impregnated into the entire needle punched blanket.
[0140] Then, the integrated object 80 is pulled up from the liquid L and placed in a container (case) 70, and the liquid is removed at a negative pressure of -13.5 to -8.5 kPa for 15 minutes. Then, while continuing to suck, hot air at 100 to 150°C is introduced into the container (box) for 4 hours to dry. After drying, it is taken out from the container 70 and demolded. Then, the temperature is raised to 1000°C at a heating rate of 3°C / min and kept for 3 hours for firing, which is Example 1.
[0141] [Bulk density ratio]
[0142] The inorganic fiber molded sintered body of Example 1 was cut into three equal parts (12×13×45 mm) into the outer surface (a), the middle part (b), and the inner surface (c). The weight of each sample was measured and divided by the volume to obtain the bulk density (kg / m 3 ). Three samples were prepared and their average values were calculated. The bulk density ratio was calculated based on the bulk density of the inner peripheral surface showing the lowest bulk density among the obtained bulk densities. The results are recorded in Table 1.
[0143] [Distribution of content (adhesion amount) of inorganic binder]
[0144] Similarly, the Al2O3 conversion adhesion amount of the inorganic adhesive on the outer surface (a), the middle part (b), and the inner surface (c) is measured. Three samples are made and the average value of each adhesion amount is calculated. First, the inorganic adhesive adhesion amount of the outer surface (Ba), the inorganic adhesive adhesion amount of the middle part (Bb), and the inorganic adhesive adhesion amount of the inner surface (Bc) are measured. Then, taking the adhesion amount of the inner surface (Bc) showing the lowest weight as the reference value, the adhesion amount of the inner surface (Bc) is subtracted from the adhesion amount of the adhesive on the outer surface (Ba) and the adhesion amount of the adhesive in the middle part (Bb), and the difference in the adhesion amount of the inorganic adhesive is calculated. The results are recorded in Table 1.
[0145] [Comparative Example 1]
[0146] The same measurements as in Example 1 were performed on a hard ceramic fiber thermal insulation material obtained by vacuum forming, which is equivalent to the annular thermal insulation material of Japanese Patent Application Laid-Open No. 2004-043918. The results are shown in Table 1.
[0147] [Table 1]
[0148]
[0149] [Investigation]
[0150] In the inorganic fiber molded sintered body of Example 1 as the heat insulating protective member of the present invention, the damage depth caused by the steel ball due to the ball drop test is very shallow, and it can be seen that the physical strength is excellent. That is, since the closer to the outer peripheral surface side, the higher the packing density, it is considered that the physical strength set for damage due to contact is significantly improved. In addition, according to the distribution result of the attachment amount of the inorganic binder particles calculated from the weight measurement value, it is confirmed that in Example 1, the inorganic binder particles are added in a gradient from the inside to the outside.
[0151] The inorganic fiber molded sintered body of Example 1 in which an inorganic binder is selectively attached to the outer peripheral surface means that more inorganic binder particles are attached to the outer peripheral surface side of the thermal insulation protection component where strength is required, and a smaller amount of inorganic binder particles are attached to the inner peripheral surface side where tightness (buffering properties) with the furnace internal components is required during construction. It is believed that this can reduce damage caused by contact and make the protection and fixation of the furnace internal components more secure.
[0152] In addition, the inorganic fiber molded sintered body of Example 1 is a structure in which the inorganic fiber blanket is layered and compressed in a direction approximately perpendicular to the direction in which the falling ball contacts. Therefore, the impact of the falling ball is dispersed in the layered interface and can be released between the layers. Therefore, it is believed that the physical strength is significantly improved.
[0153] In addition, in the inorganic fiber molded and fired body of Example 1, small cracks were confirmed to have occurred between the layers along the stacking direction of the inorganic fiber blanket by visual observation after the ball drop test. It is believed that when it is constructed as a heat insulating protective member of a furnace internal member, it is compressed and squeezed in the vertical direction of the stacking, so that the physical strength can be further improved and cracks will not occur.
[0154] On the other hand, many large cracks were generated in various directions in the inorganic fiber molded and fired body of Comparative Example 1, and pulverization occurred significantly. Since the inorganic fiber molded and fired body of Comparative Example 1 used inorganic fiber blocks (a block formed by simply gathering fibers) as the raw material, it is believed that there would be no entanglement between the fibers, and cracks were easily generated, resulting in pulverization.
[0155] Although the present invention has been described in detail using specific embodiments, it will be apparent to one skilled in the art that various modifications can be made without departing from the spirit and scope of the present invention.
[0156] This application is based on Japanese Patent Application No. 2019-133919 filed on Jul. 19, 2019, the entire contents of which are incorporated herein by reference.
[0157] Explanation of symbols
[0158] 10 Thermal insulation protection components
[0159] 13. Stuffing
[0160] 20 Inner mold
[0161] 30 Needle punch blanket
[0162] 40,50 outer mold
[0163] 80 all in one
Claims
1. A pair of heat insulating protective members, which are a pair of heat insulating protective members composed of inorganic fiber molded bodies having a split shape of a hollow cylinder, characterized in that: The inorganic fiber molded body has an inner peripheral surface (c) facing the hollow, and an outer peripheral surface (a) constituting the outer periphery, In the inorganic fiber molded body, the packing density increases as the outer peripheral surface (a) is approached. The pair of heat insulating protective members have cut surfaces extending parallel to the core line of the cylindrical shaft, The pair of heat insulating protection members are disposed in a plurality of vertical stages in a state where the cut surfaces are butted against each other, and the positions of the cut surfaces are arranged differently in each stage.
2. A pair of heat insulating protective members according to claim 1, wherein: The middle point between the outer peripheral surface (a) and the inner peripheral surface (c) of the inorganic fiber molded body is defined as the middle portion (b). The bulk density Da of the outer peripheral surface, the bulk density Db of the middle portion, and the bulk density Dc of the inner peripheral surface are in the relationship of Da>Db>Dc.
3. A pair of heat insulating protective members according to claim 1 or 2, wherein: The inorganic fiber molded body contains an inorganic binder, The content of the inorganic binder increases as the area is closer to the outer peripheral surface (a).
4. A pair of heat insulating protective members according to any one of claims 1 to 3, characterized in that: The inorganic fiber molded body is an inorganic fiber molded sintered body containing inorganic binder particles for bonding the inorganic fibers together. The number of inorganic binder particles increases as the surface is closer to the outer peripheral surface (a).
5. A pair of heat insulating protective members according to any one of claims 1 to 4, characterized in that: The cut surface is an oblique cut surface.
6. The pair of heat insulating protective members according to any one of claims 1 to 5, wherein: Holes for inserting pins are provided on the upper end surface and the lower end surface of the thermal insulation protection member.
7. A pair of heat insulating protective members according to claim 6, wherein: At least two holes are provided on the upper end surface and the lower end surface of the pair of heat insulating protection components, respectively. In the pair of vertically adjacent heat insulating protective members, The holes respectively provided in one and the other of the pair of thermal insulation protection members located on the upper side are opposed to the holes provided in one and the other of the pair of thermal insulation protection members located on the lower side so as to sandwich the cut surfaces of the pair of thermal insulation protection members located on the lower side.
8. A furnace internal member having a pair of heat insulating protective members according to any one of claims 1 to 7 mounted on an outer surface thereof.
9. The furnace internals according to claim 8, wherein: The pair of heat insulating protection members is the pair of heat insulating protection members according to claim 7, and pins are inserted into the holes of the adjacent heat insulating protection members that butt the end faces together. 10 . The furnace internal member according to claim 8 , comprising sheet-like inorganic fibers covering the pair of heat insulating protective members mounted on the furnace internal member.
11. A method for constructing a pair of heat insulating protective members, comprising the step of attaching the pair of heat insulating protective members according to any one of claims 1 to 7 to the outer surface of a furnace internal member.
12. The method for constructing a pair of heat insulating protective members according to claim 11, wherein: The pair of heat insulating protection members is the pair of heat insulating protection members according to claim 7, and pins are inserted into the holes of both adjacent heat insulating protection members that butt the end faces together.
13. The method for installing a pair of heat insulating protective members according to claim 11 or 12, comprising the step of filling a filler of inorganic fibers in the gap between the end faces of the pair of heat insulating protective members and the furnace internal member after assembling the pair of heat insulating protective members.
14. The method for installing a pair of heat insulating protective members according to any one of claims 11 to 13, comprising the step of covering the pair of heat insulating protective members with sheet-like inorganic fibers after assembling the pair of heat insulating protective members.
15. A heating furnace comprising the furnace internal member according to any one of claims 8 to 10.
16. The heating furnace according to claim 15, wherein The furnace internal component is a slideway column.
17. A method for manufacturing a pair of heat insulating protective members, the method comprising the following steps: The process of laminating an inorganic fiber blanket between an inner mold and an outer mold to form a hollow cylindrical molded body; Thereafter, the hollow cylindrical molded body is immersed in a liquid containing an inorganic binder; The hollow cylindrical molded body is pulled up from a liquid containing an inorganic binder. A step of removing the liquid containing the inorganic binder by suction from the inner peripheral surface side to the outer peripheral surface side of the hollow cylindrical molded body; and A step of drying the hollow cylindrical molded body. 18 . The method for producing a pair of heat insulating protective members according to claim 17 , comprising the step of pressing and compressing the hollow cylindrical molded body of the stacked inorganic fiber blankets.
19. The method for manufacturing a pair of heat insulating protective members according to claim 17 or 18, characterized in that: The inner mold and the outer mold are arranged in a suction dehydration container, and The inner mold and the outer mold have a plurality of holes penetrating in a direction orthogonal to an axial core line of the inner mold.