Manufacturing method and application of high-sensitivity and accurately-decoupled flexible pressure / temperature sensor based on carbon nano coil
Through the design of carbon nanocoils and polydimethylsiloxane composite materials, the problem of signal crosstalk and circuit complexity in flexible pressure-temperature sensors is solved, and a high sensitivity and precise decoupling pressure-temperature sensor is achieved, suitable for Wearable and industrial applications.
Patent Information
- Application Number
- CN202410985410.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing flexible pressure-temperature sensors are prone to crosstalk between signals when detecting pressure and temperature at the same time, and the circuit layout of traditional methods is complex and has low sensitivity, making it difficult to achieve efficient decoupling and array device integration.
The carbon nanocoil and polydimethylsiloxane composite material were used to prepare porous and solid layers by salt template sacrificial method and direct stirring, and assembled in combination with lamination method to design a carbon nanocoil/polydimethylsiloxane based on carbon nanocoil/polydimethylsiloxane. Pressure-temperature sensor for high sensitivity and precise decoupling capabilities.
High sensitivity detection of pressure and temperature, low detection limits and cycle stability are achieved, circuit layout is simplified, suitable for subsequent array devices integration, and signal crosstalk is reduced.
Smart Images

Figure CN118936553A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a design method and application of a highly sensitive and precisely decoupled flexible pressure / temperature sensor based on a carbon nano coil, belonging to the technical field of functional nanomaterial preparation. Background Art
[0002] Flexible multifunctional pressure-temperature sensors show great application prospects in the fields of wearable health monitoring, industrial process control, human-computer interaction, etc. In recent years, many researchers have conducted extensive research on temperature-pressure multifunctional sensors. Nevertheless, when detecting pressure and temperature at the same time, the developed sensors usually inevitably have signal crosstalk. In order to overcome this problem, traditional research methods mainly adopt planar integration or vertical integration to integrate multiple sensors that can detect pressure or temperature separately on the same substrate to achieve decoupled detection of pressure and temperature. However, this method has the problem of complex circuit layout, which is not conducive to subsequent array device integration. In addition, when vertically integrated, the performance of the sensor such as sensitivity and low detection limit will also degrade.
[0003] In order to solve the problems of circuit layout complexity and performance degradation, single multimodal sensors are widely used by researchers. For example, based on the piezoelectric and thermoelectric principles, researchers designed a sandwich-shaped pressure and temperature sensor composed of activated carbon materials, which exhibited high pressure sensitivity and high Seebeck coefficient, and showed negligible crosstalk. Similarly, based on MXene materials, researchers also designed pressure and temperature sensors with voltage and resistance as output signals. Despite this, this type of multifunctional sensor still has the problems of low sensitivity and more leads, which is not conducive to further integration and application in the field of weak signal detection. Compared with commonly used carbon materials, such as graphene, metal acetylene, etc., carbon nanocoils exhibit good electrical conductivity and high mechanical strength. In addition, the inherent flexibility and intertwining characteristics of carbon nanocoils will give them higher gas sensing performance. Summary of the invention
[0004] The present invention proposes a design method and application of a highly sensitive and precisely decoupled flexible pressure / temperature sensor based on carbon nanocoils. The carbon nanocoils are compounded with polydimethylsiloxane, and a porous CNCs / PDMS pressure-sensitive layer and a solid CNCs / PDMS temperature-sensitive layer are prepared respectively by a salt template sacrificial method and direct stirring. Subsequently, a pressure-temperature sensor based on carbon nanocoils / polydimethylsiloxane (CNCs / PDMS) is prepared by simple lamination assembly; the design of the sensor achieves high sensitivity, low detection limit and precise decoupling capability.
[0005] In order to solve the above technical problems, the technical solution proposed in the present invention is: a method for manufacturing a flexible pressure / temperature sensor with high sensitivity and accurate decoupling based on carbon nano coils, comprising the following steps:
[0006] (1) Preparation of polydimethylsiloxane (PDMS): polydimethylsiloxane DowCorning Sylgard 184, remove bubbles in vacuum; pour into a mold, solidify and shape; prepare a PDMS film;
[0007] (2) Salt template sacrificial method: the carbon nanocoil, polydimethylsiloxane and sodium chloride are mixed evenly and cured in a mold; a porous pressure-sensitive layer of a carbon nanocoil / polydimethylsiloxane CNCs / PDMS composite material is prepared by soaking, ultrasonication and drying;
[0008] (3) The carbon nanowires and polydimethylsiloxane are mixed evenly, evenly coated on the gold interdigital electrodes and cured to prepare a CNCs / PDMS film as a temperature sensitive layer, and the CNCs / PDMS film and the interdigital electrodes as a whole serve as a temperature sensing part;
[0009] (4) using the prepared CNCs / PDMS porous layer and PDMS film as the intermediate layer;
[0010] The temperature-sensitive layer was used as the lower electrode, and the above functional layers were assembled by lamination to prepare a pressure-temperature sensor based on carbon nanocoils / polydimethylsiloxane (CNCs / PDMS);
[0011] The upper and bottom layers are the Ag film on the PDMS and the interdigitated Au electrodes on the PI substrate, which serve as leads for the output of electrical signals; the middle layers are the CNCs / PDMS porous layer, the PDMS film and the solid CNCs / PDMS film, which serve as capacitance-related pressure sensing units, dielectric layers and resistance-related temperature sensing units, respectively.
[0012] Preferably, the polydimethylsiloxane in steps 1-3 is purchased Dow Corning Sylgard 184, which is prepared in a mass ratio of the main agent to the curing agent of 10:1.
[0013] Preferably, in the step (1), polydimethylsiloxane (purchased Dow Corning Sylgard 184) is prepared in a mass ratio of main agent to curing agent of 10:1, and then placed in a vacuum drying oven to remove bubbles; a certain amount of PDMS is then dropped into the center of a 6×6×0.035 cm mold, allowed to flow freely, and finally cured in an oven at 80° C. for 2 h to prepare a PDMS film;
[0014] In the step (2), the mass ratio of carbon nano coil, polydimethylsiloxane and sodium chloride is 1:30:210, and they are mixed evenly in a mortar; then transferred to a 4×4×0.2 cm mold; cured in an oven at 80° C. for 2 h to form; after forming, soaked in deionized water, ultrasonically removed NaCl, and finally dried in an oven at 80° C. for 1 h to prepare a porous layer of a carbon nano coil / polydimethylsiloxane (CNCs / PDMS) composite material;
[0015] In the step (3), the mass ratio of carbon nano coil to polydimethylsiloxane is 1:30, and the mixture is evenly mixed in a mortar; the composite is evenly drop-coated on the gold interdigital electrode, and the thickness of the polyimide substrate is 13 microns; the interdigital electrode line width is 100 microns, the line spacing is 100 microns, the finger length is 6.3 mm, the number of interdigital pairs is 20, and the interdigital pairs are cured at 80° C. for 2 hours; a temperature-sensitive layer of carbon nano coil / polydimethylsiloxane film is prepared;
[0016] Preparation of the device in step (3); cutting the prepared polydimethylsiloxane film into a 1×1×0.035 cm cuboid, coating it with conductive silver paste and leading it out with copper wire as the upper electrode, and curing it at 80° C. for 10 min;
[0017] The prepared CNCs / PDMS porous layer was cut into 1×1 cm squares and a PDMS film was used as the middle layer; the temperature-sensitive layer was made into the lower electrode, and the above functional layers were assembled by lamination to prepare a pressure-temperature sensor based on carbon nanocoils / polydimethylsiloxane (CNCs / PDMS).
[0018] In order to solve the technical problem of the present invention, another technical solution is proposed: a highly sensitive and precisely decoupled flexible pressure / temperature sensor based on carbon nanocoils prepared by the method described above.
[0019] In order to solve the technical problem of the present invention, another technical solution is proposed: a porous layer of a carbon nano coil / polydimethylsiloxane composite material prepared by the method described above.
[0020] In order to solve the technical problem of the present invention, another technical solution is proposed: a temperature-sensitive layer based on carbon nanocoil / polydimethylsiloxane film prepared by the method described above.
[0021] In order to solve the technical problem of the present invention, another technical solution is proposed: the application of the highly sensitive and precisely decoupled flexible pressure / temperature sensor based on the carbon nanocoil can achieve a high sensitivity to temperature of 3045.95%℃ -1 and 0.05℃ resolution detection.
[0022] Preferably, the pressure detection limit can reach 1.5 Pa, and the cycle stability is good.
[0023] Preferably, the invention can be applied to the design of anti-mistouch switches, the identification of objects of the same type with different weights and temperatures, and the perception of water cups with different temperatures.
[0024] The beneficial effects of the present invention are:
[0025] The excellent conductivity, stretchability and intertwining properties of carbon nanocoils make this material suitable for the preparation of multifunctional sensors. In addition, the soft-hard structure design composed of elastic porous layers and solid layers can prevent the crosstalk between pressure and temperature signals and achieve precise decoupling function. In addition, the adoption of the shared electrode strategy greatly simplifies the circuit layout, laying a solid foundation for the design and integration of subsequent array devices.
[0026] 1. The elastic porous CNCs / PDMS layer designed by the present invention can achieve 1.5Pa pressure detection. The sensitivity can be divided into three linear regions, corresponding to 16.47% kPa in the range of 0 to 1.1 kPa. -1 , 2.79% kPa in the range of 1.1~22 kPa -1 , 1.22% kPa in the range of 22-38 kPa -1 .
[0027] 2. The solid CNCs / PDMS layer with adjustable ratio prepared by the present invention exhibits a wide temperature detection range of 20-80°C and ultra-high temperature sensitivity (3045.95%℃ -1 ) and 0.05℃ temperature resolution. In the temperature range of 30~50℃, the sensitivity is 37.75%℃ -1 When the temperature sensor works at 60-80℃, the sensitivity reaches 3045.9%℃ -1 .
[0028] 3. The porous-solid "soft-hard" structure designed by the present invention can greatly reduce the mutual crosstalk between temperature and pressure signals.
[0029] 4. The common electrode strategy adopted by the present invention simplifies the circuit layout and is beneficial to the integration of subsequent array devices.
[0030] 5. The carbon nanocoil used in the present invention exhibits higher temperature sensitivity than other activated carbon materials (graphene, metal acetylene, carbon nanotubes).
[0031] 6. The resistance value of the CNCs / PDMS solid temperature sensing layer prepared in the present invention increases sharply with increasing temperature due to thermal expansion effect and resistance tunneling effect. This resistance change trend, which is opposite to that of a single carbon material temperature sensor, is conducive to the further development of subsequent multifunctional devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The present invention will be further described below in conjunction with the accompanying drawings.
[0033] Figure 1 is a SEM image of the carbon nanocoil / polydimethylsiloxane porous layer.
[0034] Figure 2 This is a locally enlarged SEM image of the carbon nanocoil / polydimethylsiloxane porous layer.
[0035] Figure 3 This is a physical picture of the sensor.
[0036] Figure 4 It is a schematic diagram of the sensor structure.
[0037] Figure 5 It is a graph showing the change in capacitance response of the sensor to different pressures.
[0038] Figure 6 is the pressure sensitivity fitting curve of the sensor.
[0039] Figure 7 is the detection limit of pressure sensing (the weight of a drop of water in a 200μl pipette, equivalent to 1.5Pa).
[0040] Figure 8 The repeatability and stability test of the sensor under 5 kPa pressure for 1000 cycles. The inset shows the enlarged response-recovery curve.
[0041] Fig. 9 It is a graph showing the change in resistance response of the sensor to different temperatures.
[0042] Fig.10 is the temperature sensitivity fitting curve of the sensor.
[0043] Fig.11 This is the resolution detection of the sensor, and the resistance response change during the temperature increase process of 0.05℃ gradient.
[0044] Fig.12 It is the temperature response change of the sensor under different external pressure stimulation.
[0045] Fig.13 It is the change in the pressure response of the sensor under different external temperature stimuli.
[0046] Fig.14 It is the design process of the sensor for preventing accidental touch switches.
[0047] Fig.15 The dynamic response-recovery curve of the sensor to external stimuli during the cyclic grasping experiment of quail eggs, chicken eggs, and goose eggs. I) Initial state; II) Object method (non-contact); III) Picking; IV) Return to the initial state.
[0048] Fig.16 It is the dynamic response-recovery curve of the sensor to external stimuli during the cyclic grasping experiment.
[0049] Fig.17 It is a comparison of the pressure sensing characteristics of sensors with different intermediate dielectric layer thicknesses.
[0050] Fig.18 is the change of relative resistance of CNCs / PDMS films with different CNCs contents with temperature.
[0051] Fig.19 The CNTs content in the CNTs / PDMS film is modulated to make it close to the resistance in the CNCs / PDMS film, and its resistance change in the range of 20-70°C is tested. a) CNTs / PDMS film with a resistance of 6Ω. b) CNTs / PDMS film with a resistance of 37Ω. c) CNTs / PDMS film with a resistance of 527Ω. d) Performance comparison of CNTs / PDMS films with resistances of 6Ω, 37Ω, and 527Ω. DETAILED DESCRIPTION
[0052] In order to better understand the present invention, the technical solution of the present invention is specifically described below through specific embodiments in conjunction with the accompanying drawings.
[0053] Example 1: Preparation of a porous layer of carbon nanowire / polydimethylsiloxane (CNCs / PDMS) composite material
[0054] First, prepare polydimethylsiloxane (PDMS). Polydimethylsiloxane (purchased Dow Corning Sylgard 184) is prepared at a mass ratio of 10:1 between the main agent and the curing agent. Then put it into a vacuum drying oven to remove bubbles. A certain amount of PDMS is dropped into the center of a 6×6×0.035cm mold, allowing it to flow freely, and finally cured in an oven at 80°C for 2h. A PDMS film is prepared.
[0055] Preparation of porous layer of carbon nanocoil / polydimethylsiloxane (CNCs / PDMS) composite material. Take 0.3g PDMS (purchased Dow Corning Sylgard 184) prepared with a mass ratio of main agent to curing agent of 10:1, 10mg CNC and 2.1g NaCl are mixed in a mortar. The composite is transferred to a 4×4×0.2cm mold and cured at 80℃ for 2h. The cured composite is soaked in deionized water for 10h, ultrasonicated (to remove NaCl), and finally dried at 80℃ for 1h.
[0056] The carbon nanocoil / polydimethylsiloxane composite porous layer prepared in Example (1) was characterized. Figure 2 As shown in Figure 2, the cross-sectional image of the CNCs / PDMS porous layer shows that the pore diameter is about 50 to 500 nm and the pore size is diverse. Figure 2 It can also be found that CNCs are uniformly encapsulated into the PDMS film.
[0057] Example 2: Preparation of a temperature-sensitive layer of carbon nanocoil / polydimethylsiloxane film
[0058] Take 0.3g PDMS (purchased Dow Corning Sylgard 184) and prepare it in a main agent and curing agent mass ratio of 10:1 and mix it with 10mg CNC in a mortar; mix it evenly in a mortar; drop the composite evenly on the gold interdigital electrode (polyimide substrate thickness 13 μm; interdigital electrode line width 100 μm, line spacing 100 μm, finger length 6.3 mm, number of interdigital pairs 20), and cure it at 80°C for 2h.
[0059] Example 3: Preparation of a pressure-temperature sensor based on carbon nanocoils / polydimethylsiloxane (CNCs / PDMS)
[0060] The prepared polydimethylsiloxane film was cut into 1×1×0.035cm cuboids, coated with conductive silver paste and led out with copper wire as the upper electrode, and cured at 80℃ for 10min; the prepared CNCs / PDMS porous layer was cut into 1×1cm squares and the PDMS film was used as the middle layer; the temperature-sensitive layer was used as the lower electrode, and the above functional layers were assembled by lamination to prepare a pressure-temperature sensor based on carbon nanocoil / polydimethylsiloxane (CNCs / PDMS);
[0061] The carbon nanocoil / polydimethylsiloxane-based pressure-temperature sensor prepared in Example 3 is demonstrated. Figure 3 This is a physical picture of the device. Figure 4 The schematic diagram of the device structure is shown in Figure 2. The device structure consists of 5 layers. The upper and lower layers are the Ag film on the PDMS and the interdigitated Au electrodes on the PI substrate, which serve as leads for the output of electrical signals. The middle layers are the CNCs / PDMS porous layer, the PDMS film, and the solid CNCs / PDMS film, which serve as the capacitance-related pressure sensing unit, the dielectric layer, and the resistance-related temperature sensing unit, respectively.
[0062] Example 4: Pressure Sensing Performance of Dual Parameter Sensor
[0063] (1) The upper and lower electrodes of the dual-parameter sensor are connected to the LCR digital bridge, and the sensor is placed on the desktop. The LCR digital bridge records the capacitance signal through the combination of the stepper motor and the pressure gauge. The stepper motor controls the position of the pressure gauge to change the force, and the pressure gauge measures the change in force.
[0064] (2) When the pressure gauge is not in contact with the device, the capacitance of the sensor is recorded as C0.
[0065] (3) Within the range of 0 to 38 kPa, record the applied pressure each time and maintain it for 15 seconds, then unload the pressure and maintain it for 15 seconds.
[0066] (4) Calculate the pressure from the recorded pressure, pressure P = F / S. F is the pressure, S is the contact area 1cm 2 .
[0067] (5) The measured pressure response is recorded as ΔC / C0, where C0 is the baseline capacitance when there is no pressure and ΔC is the change in capacitance relative to the baseline capacitance when pressure is applied.
[0068] Analyzing the above test results, Figure 5 These are the dynamic response-recovery curves of the pressure sensor in the range of 0 to 38 kPa. They exhibit stable sensing characteristics under different pressure conditions and have a faster response-recovery rate.
[0069] Figure 6 The pressure sensitivity of the pressure sensor is calculated by fitting the curve based on the relationship between pressure and capacitance change. The sensitivity can be divided into three linear regions, corresponding to 16.47% kPa in the range of 0 to 1.1 kPa. -1 , 2.79% kPa in the range of 1.1~22 kPa -1 , 1.22% kPa in the range of 22-38 kPa -1 .
[0070] Figure 7 The capacitance change caused by a drop of water in a 200-μl pipette on the device surface is equivalent to a detection limit of 1.5 Pa and shows a repeatable response.
[0071] Figure 8 The sensor exhibited stable pressure sensing performance under repeated loading of 5 k Pa and did not drift after 1000 cycles, confirming its long-term stability and durability in practical applications.
[0072] Example 5: Temperature Sensing Performance of Dual Parameter Sensor
[0073] (1) The temperature-sensitive layer electrode at the bottom of the dual-parameter sensor is connected to the probe on the semiconductor hot and cold probe station. The temperature change is controlled by the semiconductor hot and cold probe station, and the resistance signal is recorded by a data acquisition device.
[0074] (2) When the temperature is 20°C, the resistance of the sensor is recorded as R0.
[0075] (3) Within the range of 20-80°C, raise the temperature to the target temperature and maintain it for 5 minutes each time, then cool it down to 20°C and maintain it for another 5 minutes.
[0076] (4) Resolution test method: The device runs a baseline at 37.8°C to make it stable. Raise the temperature to the target temperature of 37.85°C and maintain the target temperature for 10 seconds; raise the temperature by 0.05°C each time, and raise the temperature 5-6 times in sequence;
[0077] (5) The measured resistance response is recorded as ΔR / R0, where R0 is the baseline resistance at 20°C and ΔR is the change in resistance relative to the baseline resistance when the temperature changes.
[0078] Analyzing the above test results, Fig. 9 The dynamic response-recovery curves of the sensor in the temperature range of 20-80℃ are given, and it exhibits a stable temperature sensing behavior with unchanged initial resistance when detecting different temperatures.
[0079] Fig.10 The temperature sensitivity of the sensor is calculated by fitting based on the relationship between temperature and resistance change. In the temperature range of 30-50℃, the sensitivity is 37.75%℃ -1 Interestingly, when the temperature sensor works at 60-80℃, the sensitivity reaches 3045.9%℃ -1 .
[0080] Fig.11 It is a sensor resolution test, based on a continuous temperature test with a 0.05℃ gradient, the sensor can distinguish a temperature change of 0.05℃ and has a significant response, with a signal-to-noise ratio far exceeding 3.
[0081] Example 6: Decoupling of dual parameter sensors
[0082] (1) The temperature-sensitive layer electrode of the dual-parameter sensor is connected to the probe on the semiconductor hot and cold probe station, and the upper electrode and the temperature-sensitive layer electrode are connected to the LCR digital bridge. The semiconductor hot and cold probe station controls the temperature change. The data acquisition device records the resistance signal. The LCR digital bridge records the capacitance signal; the stepper controls the position of the pressure gauge, thereby changing the force; the pressure gauge measures the change in force.
[0083] (2) Set four constant pressures of 0 kPa, 0.2 kPa, 5.2 kPa and 64 kPa, and test the effect of different temperatures on resistance at each constant pressure.
[0084] (3) Set four constant temperatures of 20°C, 30°C, 50°C and 70°C, and test the effect of different pressures on capacitance at each constant temperature.
[0085] Analyzing the above test results, Fig.12 It is a test of the sensor's resistance to pressure interference. Under different pressures, the resistance signal changes with temperature. Regardless of whether there is additional pressure stimulation (0, 0.2, 5.2 and 64kPa), the resistance change at different temperatures remains almost unchanged, indicating that pressure changes have little effect on temperature sensing.
[0086] Fig.13 The sensor's resistance to temperature interference is tested. The capacitance signal changes with pressure at different temperatures. It can be found that under additional heating at temperatures of 20, 30, 50, and 70°C, the capacitance remains unchanged for different pressures. This shows that the capacitive pressure sensor has good decoupling ability for temperature crosstalk.
[0087] Embodiment 7: Design of anti-mistouch switch for dual parameter sensor
[0088] (1) Prepare the Arduino Uno control board, breadboard, resistors, LEDs, and male and female connecting wires. One end of the resistor is connected to the same digital pin, and the other end of the resistor is connected to a different digital pin, as well as a sensor that acts as a touch switch.
[0089] Analyzing the above test results, Fig.14 a is the design circuit of the sensor for preventing accidental touch of the switch; Fig.14 b, c, d) The states of the red LED under different external stimuli, corresponding to pressure stimulation, temperature stimulation, and pressure / temperature stimulation. When a weight with a temperature of 23.2°C is placed on the switch ( Fig.14 b), the LED does not light up. When a finger with a temperature of 34.5°C approaches the switch ( Fig.14 c), the LED remains off. The LED will light up only when the finger applies both temperature and pressure stimulation to the switch ( Fig.14 d).
[0090] Example 8: Dual parameter sensor for identifying objects of the same type with different weights and temperatures.
[0091] (1) Fix the dual-parameter sensor on the thumb, connect the temperature-sensitive layer electrode to the data logger, and connect the upper electrode and the temperature-sensitive layer electrode to the LCR digital bridge. The data logger records the resistance signal. The LCR digital bridge records the capacitance signal. Prepare quail eggs, chicken eggs, and goose eggs with similar temperatures.
[0092] Analyzing the above test results, Fig.15 The figure shows the dynamic response-recovery curve of the sensor to external stimuli when cyclically grasping three targets (quail eggs, chicken eggs, and goose eggs). For each target, the entire grasping process can be divided into four steps: the hand moves away from the target (Ⅰ), the hand approaches the target (Ⅱ), the hand picks up the target (Ⅲ), and the hand puts down the target (Ⅳ). As shown in the figure, the temperature response signal can be observed in the approach stage (Ⅱ) and the picking stage (Ⅲ), while the pressure response signal only appears in the picking stage (Ⅲ), which means the precise decoupling of temperature and pressure. In addition, as the weight of the target increases, the pressure response signal gradually increases, indicating that the sensor has potential application value in identifying target species of different weights.
[0093] Example 9: Dual-parameter sensor sensing of water cups at different temperatures
[0094] 1) Fix the dual parameter sensor on the desktop, connect the temperature sensitive layer electrode to the data logger, and connect the upper electrode and the temperature sensitive layer electrode to the LCR digital bridge. The data logger records the resistance signal. The LCR digital bridge records the capacitance signal; prepare the sample bottle and hot water.
[0095] Analyzing the above test results, Fig.16 It is the dynamic response-recovery curve of the sensor to external excitation during the cyclic grasping experiment. As shown in the figure, the dual-parameter sensor is fixed on the table and set to the initial state (Ⅰ). When an empty sample bottle is applied to the sensor (Ⅱ), the pressure response signal can be monitored, and there is no temperature-induced resistance signal. After pouring hot water into the sample bottle (Ⅲ), a temperature response signal appears, and the capacitance change increases. The capacitance change increases further when additional hot water is continuously added (Ⅳ). Subsequently, the resistance and capacitance return to the initial state when the sample bottle is removed (Ⅴ), and then we put the sample bottle filled with cold water on the sensor (Ⅵ), and only the pressure response signal can be observed. When the sample bottle filled with cold water is recovered (Ⅶ), the capacitance returns to the initial state. When the hot sample bottle is close to the sensor (Ⅷ), an approximate signal appears, and the resistance change caused by the thermal radiation effect appears. When the hot sample bottle is away from the sensor, the resistance and capacitance also return to the initial state (Ⅸ). The whole test process shows that the designed flexible dual-parameter sensor has stable sensing characteristics and can accurately decouple pressure and temperature signals.
[0096] Comparative Example 1: Comparison of pressure sensing characteristics of sensors with different intermediate dielectric layer thicknesses.
[0097] Pour the PDMS prepared in Example 1 into the center of a mold with a length × width of 6 × 6 cm and a thickness of 0.35 mm, 0.5 mm, and 1 mm, respectively, and allow it to flow freely. Finally, cure it in an oven at 80°C for 2 hours. Prepare PDMS films with thicknesses of 0.35 mm, 0.5 mm, and 1 mm. Cut the PDMS film into two 1 × 1 squares, one of which is coated with conductive silver paste and led out with copper wire as the upper electrode, and the other as the dielectric layer. Prepare pressure-temperature sensors with different intermediate dielectric layer thicknesses using the method in Example 3. Perform pressure tests on the sensor using the method in Example 4.
[0098] Fig.17 Its capacitance value changes with external pressure. As the external pressure increases, the change amplitude of its capacitance increases. In particular, as the thickness of the dielectric layer decreases, the pressure sensing characteristics gradually enhance. It can be found that the capacitance change of the sensor with a dielectric thickness of 0.5mm at 38kPa (75%) is higher than that of the sensor with a dielectric thickness of 1mm (45%). The possible reason is that with the increase of the thickness of the dielectric layer, the deformation resistance is enhanced, resulting in a decrease in the change of the electrode spacing under the same pressure. However, further reducing the thickness of the dielectric layer (0.35mm) does not lead to a significant enhancement of the sensing performance (78%). It should be noted that the pressure sensing tests are all based on the optimal pressure sensing characteristics when the dielectric thickness is 0.35mm.
[0099] Comparative Example 2: Effect of the temperature response of the CNCs / PDMS thin film thermosensitive layer prepared with different CNCs contents.
[0100] The content of CNCs was adjusted to CNCs:PDMS = 1:30, 2:30, 1:10, and three portions of 0.3 g PDMS were prepared, and 30 mg, 20 mg, and 10 mg CNCs were added, respectively. CNCs / PDMS films with different CNCs contents were successfully prepared according to the method in Example 2, and the temperature test of the sensor was performed according to the method in Example 4.
[0101] Based on the principle of thermal expansion effect, CNCs / PDMS solid films with different mass ratios were prepared for temperature sensing. Fig.18 It can be seen from the analysis that when the mass ratio of CNCs to PDMS decreases from 30mg, 20mg to 10mg, the resistance change rate of CNCs / PDMS increases from 321%, 622% to 22359% in the temperature range of 20-70°C. The analysis shows that the CNCs / PDMS solid film with a lower CNCs content has a larger thermal expansion coefficient, which leads to a significant reduction in the cross-linking points between CNCs under the same temperature stimulus, thus forming a high resistance state.
[0102] Comparative Example 3: Comparison of the temperature performance of CNTs / PDMS film and the temperature performance of CNCs / PDMS film.
[0103] Adjust the content of CNTs, prepare three portions of 0.2g PDMS, add 17.4mg (8%), 12.8mg (6%), 8.3mg (4%) CNTs respectively. Successfully prepare CNTs / PDMS films with different CNTs contents according to the method in Example 2, and perform temperature tests on the sensor according to the method in Example 4. Fig.19 It can be seen that the resistance corresponding to 8% CNTs is 6Ω, the resistance corresponding to 6% CNTs is 37Ω, and the resistance corresponding to 4% CNTs is 527Ω. It is found that the resistance change of CNTs / PDMS in the temperature range of 20-70°C (8%, 45%, 63%) is much lower than that of CNCs / PDMS in the same resistance range.
[0104] The present invention is not limited to the specific technical solutions described in the above embodiments, and all technical solutions formed by equivalent replacement are within the protection scope required by the present invention.
Claims
1. A method for manufacturing a highly sensitive and precisely decoupled flexible pressure / temperature sensor based on a carbon nanocoil, characterized in that: The steps include: (1) Preparation of polydimethylsiloxane (PDMS): polydimethylsiloxane DowCorning Sylgard 184 was degassed in a vacuum, poured into a mold, and cured to form; Prepare a PDMS film; (2) Salt template sacrificial method: the carbon nanocoil, polydimethylsiloxane and sodium chloride are mixed evenly and cured in a mold; a porous pressure-sensitive layer of a carbon nanocoil / polydimethylsiloxane CNCs / PDMS composite material is prepared by soaking, ultrasonication and drying; (3) The carbon nanowires and polydimethylsiloxane are mixed evenly, evenly coated on the gold interdigital electrodes and cured to prepare a CNCs / PDMS film as a temperature sensitive layer, and the CNCs / PDMS film and the interdigital electrodes as a whole serve as a temperature sensing part; (4) using the prepared CNCs / PDMS porous layer and PDMS film as the intermediate layer; The temperature-sensitive layer was used as the lower electrode, and the above functional layers were assembled by lamination to prepare a pressure-temperature sensor based on carbon nanocoils / polydimethylsiloxane (CNCs / PDMS); The upper and bottom layers are the Ag film on the PDMS and the interdigitated Au electrodes on the PI substrate, which serve as leads for the output of electrical signals; the middle layers are the CNCs / PDMS porous layer, the PDMS film and the solid CNCs / PDMS film, which serve as capacitance-related pressure sensing units, dielectric layers and resistance-related temperature sensing units, respectively.
2. The method for manufacturing a highly sensitive and precisely decoupled flexible pressure / temperature sensor based on a carbon nanocoil according to claim 1, characterized in that: The polydimethylsiloxane in steps 1-3 is purchased DowCorning Sylgard 184, which is prepared in a mass ratio of the main agent to the curing agent of 10:
1.
3. The method for manufacturing a highly sensitive and precisely decoupled flexible pressure / temperature sensor based on a carbon nanocoil according to claim 1, characterized in that: In the step (1), polydimethylsiloxane (purchased Dow Corning Sylgard184) is prepared in a mass ratio of main agent to curing agent of 10:1, and then placed in a vacuum drying oven to remove bubbles; a certain amount of PDMS is then dropped into the center of a 6×6×0.035 cm mold, allowed to flow freely, and finally cured in an oven at 80° C. for 2 h to prepare a PDMS film; In the step (2), the mass ratio of carbon nano coil, polydimethylsiloxane and sodium chloride is 1:30:210, and they are mixed evenly in a mortar; then transferred to a 4×4×0.2 cm mold; cured in an oven at 80° C. for 2 h to form; after forming, soaked in deionized water, ultrasonically removed NaCl, and finally dried in an oven at 80° C. for 1 h to prepare a porous layer of a carbon nano coil / polydimethylsiloxane (CNCs / PDMS) composite material; In the step (3), the mass ratio of carbon nano coil to polydimethylsiloxane is 1:30, and the mixture is evenly mixed in a mortar; the composite is evenly drop-coated on the gold interdigital electrode, and the thickness of the polyimide substrate is 13 microns; the interdigital electrode line width is 100 microns, the line spacing is 100 microns, the finger length is 6.3 mm, the number of interdigital pairs is 20, and the interdigital pairs are cured at 80° C. for 2 hours; a temperature-sensitive layer of carbon nano coil / polydimethylsiloxane film is prepared; Preparation of the device in step (3); cutting the prepared polydimethylsiloxane film into a 1×1×0.035 cm cuboid, coating it with conductive silver paste and leading it out with copper wire as the upper electrode, and curing it at 80° C. for 10 min; The prepared CNCs / PDMS porous layer was cut into 1 × 1 cm squares and the PDMS film was used as the middle layer; The temperature-sensitive layer is made into a lower electrode, and the above functional layers are assembled by lamination to prepare a pressure-temperature sensor based on carbon nanocoils / polydimethylsiloxane (CNCs / PDMS).
4. A highly sensitive and precisely decoupled flexible pressure / temperature sensor based on carbon nanocoils prepared according to the method of claim 3.
5. A carbon nano coil / polydimethylsiloxane composite porous layer prepared according to the method of claim 3.
6. A temperature-sensitive layer based on carbon nanocoil / polydimethylsiloxane film prepared according to the method of claim 3.
7. The application of the highly sensitive and precisely decoupled flexible pressure / temperature sensor based on carbon nano coils according to claim 4, characterized in that: Achieve high sensitivity to temperature 3045.95%℃ -1 and 0.05℃ resolution detection.
8. The application of the highly sensitive and precisely decoupled flexible pressure / temperature sensor based on carbon nano coils according to claim 4, characterized in that: The pressure detection limit can reach 1.5Pa, and the cycle stability is good.
9. The application of the highly sensitive and precisely decoupled flexible pressure / temperature sensor based on carbon nano coils according to claim 4, characterized in that: It can be applied to the design of anti-false touch switches, the identification of objects of the same type with different weights and temperatures, and the perception of water cups with different temperatures.
Citation Information
Cited By
Temperature and pressure dual-mode decoupling flexible sensor based on full resistance type response mechanism
CN119688153A
Decoupling design of high-sensitivity flexible temperature-pressure dual-function sensor and preparation method of high-sensitivity flexible temperature-pressure dual-function sensor
CN119958756A
Flexible electrode based on coal-based laser-induced graphene and preparation method and application thereof
CN120314392A