Method for determining lithium precipitation threshold point of battery

By performing specific discharge, charging and lithium plating operations on the lithium-ion battery cell, the lithium-ion battery cell is determined, and the problem of inaccurate identification of lithium-analysis points in the existing technology is solved, and the accurate and lossless lithium-analysis of the battery is achieved. Early warning and judgment of the aging state of the battery cell improve the cycle life and safety of the battery cell.

CN118938037AActive Publication Date: 2024-11-12ZHEJIANG LIWINON ELECTRONIC TECHNOLOGY CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202411023898.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The prior art cannot accurately identify the lithium-ion cell location of lithium-ion battery cells, resulting in the inability to accurately judge the aging state of the battery cells, which may cause safety risks.

Method used

A method for determining the lithium-ion threshold point of the battery is proposed. By performing a series of discharge, charging and lithium plating operations on the three-electrode battery cell, the real-time potential and capacity of the battery cell are recorded, and the capacity when the negative electrode potential is 0 is used as the lithium-ion threshold. combined with the small current micro overcharging mechanism, realizes lossless lithium-ion warning.

Benefits of technology

The battery is accurately damaged lithium-ion warning, helping to obtain the lithium-ion threshold capacity of the aging battery cell during the actual cycle, alleviating the risk of lithium analysis, improving the battery cell cycle life, and reducing the risk of overcharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118938037A_ABST
    Figure CN118938037A_ABST
Patent Text Reader

Abstract

The invention discloses a method for determining a lithium precipitation threshold point of a battery, which comprises the following steps of: carrying out first discharge operation on a three-electrode battery cell to discharge the battery cell to an empty electricity state; performing first charging operation on the battery cell after the first discharging operation, so that the battery cell is charged to a full charge state; second discharging operation is carried out on the battery cell after the first charging operation, so that the battery cell is discharged to an empty electricity state, and the first capacity of the battery cell is obtained; performing second charging operation on the battery cell after the second discharging operation, so that the battery cell is charged until the electric quantity is in a second capacity state; respectively carrying out positive electrode lithium plating and negative electrode lithium plating on the reference electrode of the battery cell after the second charging operation; carrying out third discharge operation on the lithium-plated battery cell to an empty electricity state; and performing third charging operation on the battery cell after the third discharging operation, so that the battery cell is charged to a state that the electric quantity is a third capacity, recording a first negative electrode real-time potential and a first real-time capacity of the battery cell in the third charging operation, and taking the capacity when the first negative electrode real-time potential is 0 as a lithium precipitation threshold point.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for determining a threshold point of lithium deposition in a battery. Background Art

[0002] In the prior art, the aging state of lithium-ion batteries in different cycle processes is different, and it is impossible to accurately and effectively judge the aging state of the battery cells at different stages. Judging by physical detection of expansion or electrochemical signal attenuation after battery aging will lead to inaccuracy, because the battery may have failed, thus causing safety risks.

[0003] However, existing technologies are unable to accurately identify the lithium plating points of battery cells. Summary of the invention

[0004] The main purpose of the present invention is to propose a method for determining a lithium deposition threshold point of a battery, aiming to solve the problem that the prior art cannot accurately identify the lithium deposition point of a battery cell.

[0005] To achieve the above object, the present invention proposes a method for determining a battery lithium deposition threshold point, the determination method comprising:

[0006] Performing a first discharge operation on the three-electrode battery cell to discharge the battery cell to an empty state;

[0007] Performing a first charging operation on the battery cell after the first discharging operation is completed, so that the battery cell is charged to a fully charged state;

[0008] Performing a second discharging operation on the battery cell after the first charging operation is completed, so as to discharge the battery cell to an empty state and obtain a first capacity of the battery cell;

[0009] Performing a second charging operation on the battery cell after the second discharging operation is completed, so that the battery cell is charged to a state where the power is a second capacity;

[0010] Performing positive electrode lithium plating and negative electrode lithium plating on the reference electrode of the battery cell after completing the second charging operation;

[0011] Performing a third discharge operation on the battery cell after lithium plating to an empty state;

[0012] Performing a third charging operation on the battery cell after the third discharging operation, so that the battery cell is charged to a state where the amount of electricity is a third capacity, recording the first negative electrode real-time potential of the battery cell and the first real-time capacity of the battery cell in the third charging operation, and taking the capacity when the first negative electrode real-time potential is 0 as the lithium precipitation threshold point;

[0013] The second capacity is smaller than the first capacity, and the third capacity is larger than the first capacity.

[0014] Preferably, the second charging operation includes:

[0015] Performing constant current charging on the battery cell with a first preset current;

[0016] The first preset current is 0.1C-0.5C.

[0017] Preferably, the second capacity is greater than or equal to 30% and less than or equal to 90% of the first capacity.

[0018] Preferably, after performing a second discharge operation on the battery cell after the first charge operation is completed and before performing a second charge operation on the battery cell after the second discharge operation is completed, the determination method further includes:

[0019] After completing the second discharging operation, the battery cell is left for a first preset time;

[0020] The first preset time is 5 minutes to 30 minutes.

[0021] Preferably, the current of the positive electrode lithium plating and the negative electrode lithium plating are both greater than 0 mA and less than or equal to 1 mA, and the duration of the positive electrode lithium plating and the negative electrode lithium plating are both 2 h to 4 h.

[0022] Preferably, after performing a second charging operation on the battery cell after completing the second discharging operation, and before performing positive electrode lithium plating and negative electrode lithium plating on the reference electrode of the battery cell after completing the second charging operation, the determination method further includes:

[0023] After completing the second charging operation, the battery cell is left for a second preset time;

[0024] The second preset time is 5 minutes to 30 minutes.

[0025] Preferably, performing a third charging operation after completing the third discharging operation to charge the battery cell to a state where the battery cell has a third capacity, and recording the first negative electrode real-time potential and the first real-time capacity of the battery cell in the third charging operation comprises:

[0026] After the third discharge operation is completed, the battery cell is charged with a second preset constant current, so that the battery cell is charged to a state where the power is a third capacity;

[0027] Recording the first negative electrode real-time potential of the battery cell and the first real-time capacity of the battery cell in the third charging operation at a first preset frequency;

[0028] The second preset current is 0.01C to 0.03C, and the first preset frequency is 1 time / s to 10 times / s.

[0029] Preferably, the third capacity is 110% to 130% of the first capacity.

[0030] Preferably, the first discharging operation on the three-electrode battery cell includes: performing constant current discharge on the three-electrode battery cell with a third preset current;

[0031] The performing a first charging operation on the battery cell after the first discharging operation comprises: performing constant current and constant voltage charging on the battery cell after the first discharging operation with a fourth preset current;

[0032] The performing a second discharge operation on the battery cell after the first charging operation includes: performing a constant current discharge on the battery cell after the first charging operation with a fifth preset current;

[0033] The third discharging operation on the battery cell after lithium plating comprises: performing constant current discharge on the battery cell after lithium plating with a sixth preset current;

[0034] Among them, the third preset current is 0.1C to 0.5C, the fourth preset current is 0.4C to 0.6C, the fifth preset current is 0.1C to 0.5C, and the sixth preset current is 0.1C to 0.5C.

[0035] Preferably, before performing the first discharge operation on the three-electrode battery cell, the determination method further comprises: placing the three-electrode battery cell on hold for a third preset time;

[0036] After the first discharge operation is performed on the three-electrode battery cell and before the first charge operation is performed on the battery cell after the first discharge operation, the determination method further includes: placing the battery cell after the first discharge operation on hold for a fourth preset time;

[0037] After performing a first charging operation on the battery cell after the first discharging operation and before performing a second discharging operation on the battery cell after the first charging operation, the determining method further includes: placing the battery cell after the first charging operation on hold for a fifth preset time;

[0038] After the reference electrodes of the battery cell after the second charging operation are respectively subjected to positive lithium plating and negative lithium plating, and before the battery cell after the lithium plating is subjected to a third discharge operation to an empty state, the determination method further comprises: placing the battery cell after the lithium plating for a sixth preset time;

[0039] Among them, the third preset time is 5 minutes to 30 minutes, the fourth preset time is 5 minutes to 30 minutes, the fifth preset time is 5 minutes to 30 minutes, and the sixth preset time is 5 minutes to 30 minutes.

[0040] The beneficial effects of the technical solution of the present invention are: the determination method of the present invention is accurate and reliable, and can realize the non-destructive lithium deposition warning of the battery, help obtain the lithium deposition threshold capacity of the aged battery cell in the actual cycle process, and at the same time obtain the N / P value of the battery cell after aging, which can mitigate the risk of lithium deposition, improve the cycle life of the battery cell, and prevent the battery cell from failing too quickly. The present invention adopts a micro-overcharge and small current mechanism to make the entire charging process tend to be non-polarized, which is conducive to accurately obtaining the lithium deposition threshold point and reducing the risk of overcharging; the capacity when the negative electrode potential of the three-electrode battery cell is 0 is used as the lithium deposition threshold point, combined with the decreasing trend of the negative electrode potential of the three-electrode battery cell, the lithium deposition point of the battery cell can be accurately identified. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 A flow chart of a method for determining a lithium deposition threshold point provided in one embodiment of the present invention;

[0042] Figure 2 dV / dQ curve of the electrode and the whole battery according to the embodiment of the present invention. DETAILED DESCRIPTION

[0043] The scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, top, bottom, side...) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0045] It should also be noted that when an element is referred to as being "fixed on" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element at the same time. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.

[0046] In addition, the descriptions involving "first", "second", etc. in the embodiments of the present invention are only for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features.

[0047] In view of the technical defects existing in the related art, an embodiment of the present invention provides a method for determining a threshold point of lithium deposition in a battery, referring to Figure 1 , the determination method includes:

[0048] Step S100, performing a first discharge operation on the three-electrode battery cell to discharge the battery cell to an empty state;

[0049] Step S200, performing a first charging operation on the battery cell after the first discharging operation is completed, so as to charge the battery cell to a fully charged state;

[0050] Step S300, performing a second discharging operation on the battery cell after the first charging operation is completed, so as to discharge the battery cell to an empty state, and obtain a first capacity of the battery cell;

[0051] Step S400, performing a second charging operation on the battery cell after the second discharging operation is completed, so that the battery cell is charged to a state where the power is a second capacity;

[0052] Step S500, performing positive electrode lithium plating and negative electrode lithium plating on the reference electrode of the battery cell after completing the second charging operation;

[0053] Step S600, performing a third discharge operation on the battery cell after lithium plating to an empty state;

[0054] Step S700, performing a third charging operation on the battery cell after the third discharging operation, so that the battery cell is charged to a state of a third capacity, recording the first negative electrode real-time potential and the first real-time capacity of the battery cell in the third charging operation, and taking the first negative electrode real-time potential of 0 as a lithium precipitation threshold point;

[0055] The second capacity is smaller than the first capacity, and the third capacity is larger than the first capacity.

[0056] In this embodiment, the above method can realize the non-destructive lithium deposition warning of the battery, help obtain the lithium deposition threshold capacity of the aged battery cell in the actual cycle process, and obtain the N / P value of the battery cell after aging, which can mitigate the risk of lithium deposition, improve the cycle life of the battery cell, and prevent the battery cell from failing too quickly. The present invention adopts a micro-overcharge and small current mechanism to make the entire charging process tend to be non-polarized, which is conducive to accurately obtaining the lithium deposition threshold point and reducing the risk of overcharging; the capacity when the negative electrode potential of the three-electrode battery cell is 0 is used as the lithium deposition threshold point, combined with the decreasing trend of the negative electrode potential of the three-electrode battery cell, the lithium deposition point of the battery cell can be accurately identified.

[0057] Specifically, the lithium plating threshold point determination method of the present application can be used for batteries with different specifications of positive active materials, and the normal operating voltage ranges corresponding to batteries with different specifications of positive active materials are also different. The normal operating voltage range of the battery in the present application is 2.5V-4.75V. Empty power is the termination voltage when the battery is discharged, and full power is the termination voltage when the battery is charged. Since the battery cells in the present application are battery cells at different aging stages, it is necessary to discharge the battery cells to empty power first to ensure the accuracy of the measured capacity, and then the first capacity of the battery cell can be obtained by charging the battery cell to full power and then discharging it to empty power.

[0058] In some embodiments, the three-electrode battery cell includes a positive electrode, a negative electrode, a reference electrode, and an electrolyte.

[0059] In this embodiment, the battery is configured as a three-electrode cell structure, and a reference electrode is introduced to monitor the change of the internal potential of the battery in real time, thereby providing more accurate information about the battery status.

[0060] In some embodiments, in addition to recording the first negative electrode real-time potential of the battery cell and the first real-time capacity of the battery cell in the third charging operation, the full electrode potential of the battery cell may also be recorded.

[0061] In some embodiments, the second charging operation includes:

[0062] Performing constant current charging on the battery cell with a first preset current;

[0063] The first preset current is 0.1C-0.5C.

[0064] In some embodiments, the second capacity is greater than or equal to 30% and less than or equal to 90% of the first capacity, and preferably the second capacity is 50% of the first capacity.

[0065] Specifically, Li +It migrates from the positive electrode to the negative electrode. If it is in the high SOC range (such as above 90%), the battery cell is in a high voltage state. Although lithium plating can still be completed with a small current, the positive electrode will de-Li under this condition. + It is more likely to induce irreversible structural phase changes, resulting in material loss, as well as negative effects such as SEI consumption on the negative electrode surface and electrolyte consumption. Therefore, it is necessary to avoid lithium plating operations at high SOC, and therefore the battery cell charging capacity is limited to the above range.

[0066] In some embodiments, after performing a second discharge operation on the battery cell after the first charge operation is completed and before performing a second charge operation on the battery cell after the second discharge operation is completed, the determination method further includes:

[0067] After completing the second discharging operation, the battery cell is left for a first preset time;

[0068] The first preset time is 5 minutes to 30 minutes.

[0069] In some embodiments, the current of the positive electrode lithium plating and the negative electrode lithium plating are both greater than 0 mA and less than or equal to 1 mA, preferably 20 μA; the duration of the positive electrode lithium plating and the negative electrode lithium plating are both 2h to 4h, preferably 3h.

[0070] Specifically, taking the battery cell as a three-electrode battery cell as an example, the specific steps of lithium plating the battery cell include: respectively holding the battery cell pole ears that have been placed in the three electrodes at both ends of the multimeter to measure whether the voltage is in a normal state, adjusting the battery cell SOC not to a high SOC state (> 90%), because the copper wire potential is higher than the negative electrode corresponding to the Ni pole ear, it is necessary to preferentially plate lithium on the positive electrode, the positive electrode clamps the Al pole ear, the negative electrode clamps the reference electrode, the current selected for lithium plating is 20μA, the lithium plating time must not be less than 2h, and the lithium plating is more uniform and dense using a small current, so that the potential of the reference electrode is more stable. After the lithium plating is completed, the copper wire is attached to lithium and the potential is lower than the potential corresponding to the Ni pole ear. In order to ensure that the surface of the copper wire lithium plating is more dense and uniform, the negative electrode needs to be plated with lithium after the positive electrode lithium plating is completed, the positive electrode clamps the Ni pole ear, the negative electrode clamps the reference electrode, the lithium plating time and current are the same as the positive electrode lithium plating, and the voltage is monitored to see if it is in a normal range after the lithium plating is completed. Furthermore, during the lithium plating process, it is necessary to record the potential and capacity of the battery cell during the lithium plating process according to a second preset frequency, so as to determine whether the battery cell is in a normal state. Preferably, the second preset frequency is 10s / point.

[0071] In some embodiments, after performing a second charging operation on the battery cell after completing the second discharging operation, and before performing positive electrode lithium plating and negative electrode lithium plating on the reference electrode of the battery cell after completing the second charging operation, the determining method further includes:

[0072] After completing the second charging operation, the battery cell is left for a second preset time;

[0073] The second preset time is 5 minutes to 30 minutes.

[0074] In some embodiments, performing a third charging operation after completing the third discharging operation to charge the battery cell to a state where the battery cell has a third capacity, and recording the first negative electrode real-time potential and the first real-time capacity of the battery cell in the third charging operation comprises:

[0075] After the third discharge operation is completed, the battery cell is charged with a second preset constant current, so that the battery cell is charged to a state where the power is a third capacity;

[0076] Recording the first negative electrode real-time potential of the battery cell and the first real-time capacity of the battery cell in the third charging operation at a first preset frequency;

[0077] The second preset current is 0.01C to 0.03C, preferably 0.02C, and the first preset frequency is 1 time / s to 10 times / s, preferably 1 time / s.

[0078] In some embodiments, the third capacity is 110% to 130% of the first capacity.

[0079] Specifically, the present application charges the capacity of the battery cell to 110% to 130% of the first capacity through a small current micro-overcharge mechanism, which can make the entire charging process approach a non-polarization process. Polarization refers to the phenomenon that the charge distribution inside the battery is uneven due to the mismatch between the electrochemical reaction rate and the charge transfer rate during the battery charging and discharging process. Polarization will cause a voltage drop inside the battery, affecting the charging efficiency and performance stability of the battery. Therefore, the present application uses a small current to charge to the process state so that the charging process of the battery cell can be approached as a non-polarization process. The real-time potential and real-time capacity of the battery cell during the charging process are recorded to facilitate the accurate judgment of the lithium precipitation threshold point of the battery cell, and the threshold capacity of lithium precipitation of the aged battery cell can be obtained in the actual cycle process. At the same time, the N / P value (negative electrode positive electrode capacity ratio) after aging can be obtained. Its key role is to provide a better solution for designers to prevent the battery cell from failing too quickly. While ensuring that the battery is intact, the corresponding lithium precipitation capacity is captured at the same time, which can alleviate the risk of lithium precipitation and improve the cycle life of the battery cell. Industry pain points and problems. Furthermore, by setting the first preset frequency to 1 time / s to 10 times / s, the phase change peak boundary of the dV / dQ curve drawn in the subsequent calculation of the N / P value can be clear and free of burrs, and the accuracy is higher.

[0080] In some embodiments, the first discharge operation on the three-electrode battery cell includes: performing a constant current discharge on the three-electrode battery cell with a third preset current;

[0081] The performing a first charging operation on the battery cell after the first discharging operation comprises: performing constant current and constant voltage charging on the battery cell after the first discharging operation with a fourth preset current;

[0082] The performing a second discharge operation on the battery cell after the first charging operation includes: performing a constant current discharge on the battery cell after the first charging operation with a fifth preset current;

[0083] The third discharging operation on the battery cell after lithium plating comprises: performing constant current discharge on the battery cell after lithium plating with a sixth preset current;

[0084] Among them, the third preset current is 0.1C to 0.5C, the fourth preset current is 0.4C to 0.6C, the fifth preset current is 0.1C to 0.5C, and the sixth preset current is 0.1C to 0.5C.

[0085] Specifically, since the battery cell has been charged to 50% of the first capacity before lithium plating, the battery cell also needs to be discharged to empty, so as to facilitate the subsequent small current micro-overcharge operation.

[0086] In some embodiments, before performing the first discharge operation on the three-electrode battery cell, the determination method further includes: placing the three-electrode battery cell on hold for a third preset time;

[0087] After the first discharge operation is performed on the three-electrode battery cell and before the first charge operation is performed on the battery cell after the first discharge operation, the determination method further includes: placing the battery cell after the first discharge operation on hold for a fourth preset time;

[0088] After performing a first charging operation on the battery cell after the first discharging operation and before performing a second discharging operation on the battery cell after the first charging operation, the determining method further includes: placing the battery cell after the first charging operation on hold for a fifth preset time;

[0089] After the reference electrodes of the battery cell after the second charging operation are respectively subjected to positive lithium plating and negative lithium plating, and before the battery cell after the lithium plating is subjected to a third discharge operation to an empty state, the determination method further comprises: placing the battery cell after the lithium plating for a sixth preset time;

[0090] Among them, the third preset time is 5 minutes to 30 minutes, the fourth preset time is 5 minutes to 30 minutes, the fifth preset time is 5 minutes to 30 minutes, and the sixth preset time is 5 minutes to 30 minutes.

[0091] In the embodiments of the present application, during the charge and discharge process, the concentration of a certain ion near the electrode changes due to the electrode reaction, and the diffusion rate of ions in the bulk solution cannot keep up with this change, resulting in a concentration gradient between the concentration of the solution near the electrode and the bulk solution. The change in electrode potential caused by this concentration difference is called concentration polarization. Therefore, the shelving operations in the present application are all for eliminating this concentration polarization, reducing the polarization voltage, restoring the equilibrium potential, and making the electrode exhibit the best performance curve during discharge, thereby facilitating the data obtained in subsequent steps to be more accurate.

[0092] In some embodiments, the positive electrode of the three-electrode battery cell includes a positive electrode active material, and the positive electrode active material is selected from at least one of lithium cobalt oxide, sodium-containing lithium cobalt oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium iron phosphate, lithium-rich manganese-based material, lithium iron manganese phosphate, lithium titanate, lithium nickel manganese oxide, lithium nickel oxide, lithium manganese oxide, and nickel-manganese binary material; the negative electrode material of the three-electrode battery cell includes graphite.

[0093] In some embodiments, after obtaining the lithium precipitation threshold point, the method further includes:

[0094] The effectiveness of the lithium precipitation threshold point is judged.

[0095] Specifically, since the aging state of the battery cell cannot be determined, the accuracy of the lithium deposition threshold point cannot be known, and therefore the effectiveness of the obtained lithium deposition threshold point also needs to be judged.

[0096] In some embodiments, the determining of the effectiveness of the lithium precipitation threshold point includes:

[0097] Obtaining a charging curve of the three electrodes according to the recorded first real-time voltage and the first real-time capacity;

[0098] Differentiating the charging curve to obtain a differential curve with the SOC value as the abscissa and dV / dQ as the ordinate;

[0099] Obtaining the negative electrode capacity and the positive electrode capacity of the three-electrode battery cell according to the differential curve, calculating the ratio of the negative electrode capacity to the positive electrode capacity, and obtaining the N / P value of the three-electrode battery cell after aging;

[0100] Comparing the N / P value of the three-electrode battery cell after aging with the experimental simulation value to determine the effectiveness of the lithium precipitation threshold point;

[0101] The experimental simulation value is the N / P value obtained by testing when the positive electrode, the negative electrode and the electrolyte of the three-electrode battery cell are assembled into a button battery.

[0102] In some embodiments, comparing the N / P value of the three-electrode battery cell after aging with an experimental simulation value to determine the validity of the lithium precipitation threshold point includes:

[0103] When the error between the N / P value of the three-electrode battery cell after aging and the experimental simulation value is within a preset range, the lithium precipitation threshold point is effective;

[0104] And / or, when the error between the N / P value of the three-electrode battery cell after aging and the experimental simulation value is not within a preset range, the lithium deposition threshold point is not valid.

[0105] In some embodiments, the preset range is -0.5% to 0.5%.

[0106] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.

[0107] Example 1

[0108] The battery cell is a three-electrode battery cell, wherein the positive electrode active material of the three-electrode battery cell is lithium cobalt oxide, and the negative electrode active material is graphite.

[0109] A method for determining a battery lithium deposition threshold point, comprising:

[0110] Step S100, leaving the battery cell for 5 minutes, and discharging it at a constant current of 0.2C until it is empty;

[0111] Step S200, leaving the battery cell for 5 minutes, and charging it to full power at 0.5C constant current and constant voltage;

[0112] Step S300, leaving the battery cell for 5 minutes, discharging it to empty at a constant current of 0.2C, and obtaining a first capacity Q1 of the battery cell;

[0113] Step S400, leaving the battery cell for 5 minutes, and charging the battery cell to a second capacity Q2 at a constant current of 0.2C, where Q2 = 50% Q1;

[0114] Step S500, the battery cell is left for 5 minutes, and the positive electrode and negative electrode of the reference electrode of the battery cell are plated with lithium in sequence with a lithium plating current of 20 μA, and the lithium plating time is 3 hours for the positive electrode and the negative electrode respectively, and the battery cell is left for 10 minutes after the lithium plating;

[0115] Step S600, leaving the battery cell for 5 minutes, and discharging the battery cell again at a constant current of 0.2C until the battery cell is empty;

[0116] Step S700, the battery cell is placed for 5 minutes, and the battery cell is charged to a third capacity Q3 at a constant current of 0.02C, Q3=120% Q1, and the first real-time potential and the first real-time capacity of the battery cell during the charging process are recorded at a frequency of 1 time / s, and the negative electrode potential is 0 as the lithium precipitation threshold point, and the SOC value and capacity corresponding to the lithium precipitation threshold point are recorded.

[0117] like Figure 2 As shown, it is the charging curve of the battery cell in Example 1, and the dV / dQ curve, wherein, Figure 2 The circled portion in (a) is the lithium deposition area of ​​the battery cell. Figure 2 The marked point in (b) is the capacity corresponding to the negative electrode lithium deposition threshold point. Figure 2 (d) is Figure 2 The enlarged view of the box part (c) Figure 2 Point C in (d) is the capacity Q corresponding to the negative electrode lithium deposition threshold point C , draw a straight line parallel to the X-axis from point C to the Y-axis, and mark the adjacent intersection of the straight line and the dV / dQ curve as point A, which is the capacity Q of the positive electrode at the lithium precipitation threshold point. A , the N / P value of the battery cell = Q C / Q A .

[0118] Accuracy verification: The accuracy of the method of the present invention is verified by measuring the N / P value of fresh button batteries of the same system. Since button batteries eliminate the consistency influence of soft-pack cells, the test results are more accurate and have reference value.

[0119] Button cell battery preparation

[0120] 1. Pole piece production: The formula needs to be determined before the pole piece is produced. The cathode and anode pieces obtained in this process are linked to the final button battery N / P value. The positive pole piece contains active substances, conductive carbon black, PVDF, NMP and other chemical substances; the negative pole piece mixing material contains active substances, CMC, SBR and other chemical substances. According to the stirring, coating, baking, rolling and other operations, the final pole piece morphology should meet the requirements of uniform color, uniform thickness, no obvious scratches, no particles, no powder loss and no bottom exposure. The button battery uses the same positive and negative active substances as the three-electrode battery cell in Example 1.

[0121] 2. Select samples: Use an analytical balance to weigh the pole piece and record its original data. Calculate the N / P value under the condition that the cathode and anode have the same area. The N / P value corresponds to the design value in the embodiment. Take 3 parallel samples of the selected pole piece at the same time and use a punching machine to punch discs for use. After punching, dry the pole piece at 60°C for 2 hours and weigh it. Take a weight close to the disc and prepare for the assembly step.

[0122] 3. Button battery assembly: Control the water oxygen value in the glove box to be less than 0.1ppm to assemble button batteries. Six button battery parallel samples need to be assembled synchronously under different N / P values. Prepare the required number of steel shells, diaphragms, electrolytes and other auxiliary materials in advance. Place the negative electrode shell on the dust-free paper, place the shrapnel mouth down in the negative electrode shell, place a gasket on the shrapnel (the smooth side of the gasket faces up), take the positive electrode shell on the dust-free paper, place the electrode coated side up in the center of the positive electrode shell, and use a pipette to suck 50μL of electrolyte and drip it in. Take the isolation film and place it on top of the electrode, adjust the isolation film so that it completely covers the positive electrode shell, and drip an equal amount of electrolyte on the isolation film. Place the negative electrode sheet coated area down on the isolation film, then turn the positive electrode shell upside down and align it with the negative electrode shell for assembly. Use insulated tweezers to place the assembled button battery with the negative electrode facing up on the hydraulic sealing machine, pad with dust-free paper to absorb the electrolyte, and the assembly is completed after sealing. The assembled button cell was placed in a dust-free bag and transferred outside the glove box. Its internal resistance was recorded and then allowed to stand at room temperature for >6 h.

[0123] 4. Button battery test:

[0124] Step 1: Set aside for 5 minutes;

[0125] Step 2: 0.5C constant current and constant voltage charging until fully charged;

[0126] Step 3: Set aside for 5 minutes;

[0127] Step 4: Discharge at a constant current of 0.04C until empty, set the sampling interval to 1s / point, and record its capacity as Q4;

[0128] Step 5: Set aside for 5 minutes;

[0129] Step 6: Charge at 0.02C constant current and constant voltage to 110% Q4, set the sampling interval to 1s / point, and record the capacity corresponding to the lithium precipitation threshold point;

[0130] Step 7: Set aside for 5 minutes.

[0131] According to the test results of the button battery, the charging curve and dV / dQ curve were made, and the N / P value was calculated, which was the N / P experimental simulation value. Four sets of parallel samples were made. The results are shown in Table 1.

[0132] Table 1 Test results of N / P value of battery cells in the embodiment

[0133] Sample 1 Sample 2 Sample 3 Sample 4 N / P Design Value 1.065 1.054 1.044 1.026 N / P experimental simulation value 1.062 1.057 1.042 1.032 N / P measured value 1.058 1.052 1.039 1.028

[0134] Note: The N / P design values ​​in Table 1 are given values ​​of the battery cell design parameters (if laser drilling technology is added to the battery cell, the actual N / P value has been taken into account), the N / P experimental simulation value is the actual N / P value determined by testing when the positive and negative electrodes and the electrolyte of the battery cell are assembled into a button battery, and the N / P measured value is the N / P value obtained by measuring the negative electrode potential of the three-electrode battery cell and analyzing the lithium precipitation threshold point through differential curve analysis using the method of Example 1.

[0135] As can be seen from Table 1, the errors between all the measured values ​​of Example 1 and the experimental simulation values ​​of the power-off are controlled within 0.5%, which proves that the method of the present application is effective and the errors are within the allowable range, and the lithium precipitation threshold points determined are accurate and effective. Therefore, the method of the present invention can realize the non-destructive lithium precipitation warning of the battery, help obtain the lithium precipitation threshold capacity of the aged battery cell during the actual cycle process, and obtain the N / P value of the battery cell after aging, which can mitigate the risk of lithium precipitation, improve the cycle life of the battery cell, and prevent the battery cell from failing too quickly.

[0136] The above description is only a partial or preferred embodiment of the present invention. Neither the text nor the drawings can limit the scope of protection of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the overall concept of the present invention, or direct / indirect application in other related technical fields are included in the scope of protection of the present invention.

Claims

1. A method for determining a battery lithium deposition threshold point, characterized in that: include: Performing a first discharge operation on the three-electrode battery cell to discharge the battery cell to an empty state; Performing a first charging operation on the battery cell after the first discharging operation is completed, so that the battery cell is charged to a fully charged state; Performing a second discharging operation on the battery cell after the first charging operation is completed, so as to discharge the battery cell to an empty state and obtain a first capacity of the battery cell; Performing a second charging operation on the battery cell after the second discharging operation is completed, so that the battery cell is charged to a state where the power is a second capacity; Performing positive electrode lithium plating and negative electrode lithium plating on the reference electrode of the battery cell after completing the second charging operation; Performing a third discharge operation on the battery cell after lithium plating to an empty state; Performing a third charging operation on the battery cell after the third discharging operation, so that the battery cell is charged to a state where the amount of electricity is a third capacity, recording the first negative electrode real-time potential of the battery cell and the first real-time capacity of the battery cell in the third charging operation, and taking the capacity when the first negative electrode real-time potential is 0 as the lithium precipitation threshold point; The second capacity is smaller than the first capacity, and the third capacity is larger than the first capacity.

2. The method for determining the battery lithium deposition threshold point according to claim 1, characterized in that: The second charging operation includes: Performing constant current charging on the battery cell with a first preset current; The first preset current is 0.1C-0.5C.

3. The method for determining the battery lithium deposition threshold point according to claim 1 or 2, characterized in that: The second capacity is greater than or equal to 30% and less than or equal to 90% of the first capacity.

4. The method for determining the battery lithium deposition threshold point according to claim 1, characterized in that: After performing a second discharge operation on the battery cell after the first charge operation is completed and before performing a second charge operation on the battery cell after the second discharge operation is completed, the determination method further includes: After completing the second discharging operation, the battery cell is left for a first preset time; The first preset time is 5 minutes to 30 minutes.

5. The method for determining the battery lithium deposition threshold point according to claim 1, characterized in that: The current of the positive electrode lithium plating and the negative electrode lithium plating are both greater than 0 mA and less than or equal to 1 mA, and the duration of the positive electrode lithium plating and the negative electrode lithium plating are both 2h to 4h.

6. The method for determining the battery lithium deposition threshold point according to claim 1 or 5, characterized in that: After performing a second charging operation on the battery cell after the second discharging operation, and before performing positive electrode lithium plating and negative electrode lithium plating on the reference electrode of the battery cell after the second charging operation, the determining method further includes: After completing the second charging operation, the battery cell is left for a second preset time; The second preset time is 5 minutes to 30 minutes.

7. The method for determining the battery lithium deposition threshold point according to claim 1, characterized in that: The performing a third charging operation after completing the third discharging operation to charge the battery cell to a state where the battery cell has a third capacity, and recording the first negative electrode real-time potential and the first real-time capacity of the battery cell in the third charging operation comprises: After the third discharge operation is completed, the battery cell is charged with a second preset constant current, so that the battery cell is charged to a state where the power is a third capacity; Recording the first negative electrode real-time potential of the battery cell and the first real-time capacity of the battery cell in the third charging operation at a first preset frequency; The second preset current is 0.01C to 0.03C, and the first preset frequency is 1 time / s to 10 times / s.

8. The method for determining the battery lithium deposition threshold point according to claim 1 or 7, characterized in that: The third capacity is 110% to 130% of the first capacity.

9. The method for determining the battery lithium deposition threshold point according to claim 1, characterized in that: The first discharging operation on the three-electrode battery cell includes: performing a constant current discharge on the three-electrode battery cell with a third preset current; The performing a first charging operation on the battery cell after the first discharging operation comprises: performing constant current and constant voltage charging on the battery cell after the first discharging operation with a fourth preset current; The performing a second discharge operation on the battery cell after the first charging operation includes: performing a constant current discharge on the battery cell after the first charging operation with a fifth preset current; The third discharging operation on the battery cell after lithium plating comprises: performing constant current discharge on the battery cell after lithium plating with a sixth preset current; Among them, the third preset current is 0.1C to 0.5C, the fourth preset current is 0.4C to 0.6C, the fifth preset current is 0.1C to 0.5C, and the sixth preset current is 0.1C to 0.5C.

10. The method for determining the battery lithium deposition threshold point according to claim 1 or 9, characterized in that: Before performing the first discharge operation on the three-electrode battery cell, the determination method further includes: placing the three-electrode battery cell on hold for a third preset time; After the first discharge operation is performed on the three-electrode battery cell and before the first charge operation is performed on the battery cell after the first discharge operation, the determination method further includes: placing the battery cell after the first discharge operation on hold for a fourth preset time; After performing a first charging operation on the battery cell after the first discharging operation and before performing a second discharging operation on the battery cell after the first charging operation, the determining method further includes: placing the battery cell after the first charging operation on hold for a fifth preset time; After the reference electrodes of the battery cell after the second charging operation are respectively subjected to positive lithium plating and negative lithium plating, and before the battery cell after the lithium plating is subjected to a third discharge operation to an empty state, the determination method further comprises: placing the battery cell after the lithium plating for a sixth preset time; Among them, the third preset time is 5 minutes to 30 minutes, the fourth preset time is 5 minutes to 30 minutes, the fifth preset time is 5 minutes to 30 minutes, and the sixth preset time is 5 minutes to 30 minutes.

Citation Information

Patent Citations

  • Three-electrode system-based quantitative analysis method for lithium precipitation of lithium ion batteries

    CN110161417A

  • Method for analyzing internal resistance constituent elements of battery cell and change characteristics of internal resistance constituent elements

    CN114114026A

  • Preparation method of three-electrode battery and lithium precipitation test method of three-electrode battery

    CN114497693A

  • Method for testing excess ratio of battery cell

    CN114966443A

  • Method for testing stability of lithium ion battery system

    CN115656849A