Conductive paste, preparation method thereof and application of conductive paste in porous back electrode

By using titanium oxide as conductive dielectric particles in perovskite solar cells, the contact interface between the porous back electrode and the perovskite is improved, the problem of low carrier transfer efficiency is solved, and the perovskite solar cells is significantly improved performance.

CN118942764AActive Publication Date: 2024-11-12HUAZHONG UNIV OF SCI & TECH +1

Patent Information

Application Number
CN202411167303.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The contact interface between the porous back electrode and the perovskite in existing perovskite solar cells is poor, resulting in low carrier transfer efficiency, affecting device performance, and traditional carbon black conductive dielectrics are not sufficient to improve this problem.

Method used

Titanium oxides such as TiO, TiO2, Ti2O3, Ti4O7, Ti5O9 are introduced as conductive dielectric particles. Through strong interaction with perovskites, it provides nucleation sites, improves the contact interface between the back electrode and Pb-based perovskite, and enhances the device. performance.

Benefits of technology

Through the introduction of titanium oxide, the conductivity and carrier transmission efficiency of the back electrode are significantly improved, the resistivity is reduced, the photoelectric conversion efficiency of perovskite solar cells is improved, and high-performance carbon-based perovskite solar energy is achieved Battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942764A_ABST
    Figure CN118942764A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of preparation of electrodes of photoelectric devices, and discloses conductive paste, a preparation method thereof and application of the conductive paste in a porous back electrode, the conductive paste comprises main conductive particles, conductive medium particles and a functional additive which are dispersed in a solvent, and the conductive medium particles are at least one of TiO, TiO2, Ti2O3, Ti4O7 and Ti5O9; the electrode correspondingly formed by the conductive slurry can improve the contact between the electrode and Pb-based perovskite. Titanium oxide is introduced into traditional conductive paste to replace traditional conductive medium particles (such as carbon black), the contact interface between a back electrode formed by the conductive paste and Pb-based perovskite in a mesoscopic perovskite solar cell can be improved, the performance of a device can be improved, and the problems that in the prior art, the back interface of a porous counter electrode is poor in contact, and the performance of the device is poor are solved. And the performance of the mesoscopic perovskite solar cell is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrode preparation of optoelectronic devices, and more specifically, relates to a conductive paste and a preparation method thereof and an application in a porous back electrode. The conductive paste uses TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9 as conductive medium particles, and can improve the contact interface between the back electrode formed by the conductive paste and the Pb-based perovskite in a mesoscopic perovskite solar cell (i.e., improve the back interface contact). In particular, a porous back electrode can be formed by screen printing technology for constructing a high-performance mesoscopic perovskite solar cell. Background Art

[0002] Perovskite solar cells have developed rapidly since their emergence in 2009, with energy conversion efficiency increasing from 3.8% at the beginning to 26.1% at present, showing great commercial potential and the potential huge cost-effectiveness of this emerging photovoltaic technology in solar power generation. The conventional structure of perovskite solar cells has front electrode, perovskite light absorption layer, carrier transport layer and counter electrode.

[0003] As one of the important components of perovskite solar cells, the counter electrode (also known as the back electrode) is mainly made of precious metals, such as gold and silver. The use of metal electrodes is one of the main obstacles that need to be solved in the large-scale process of perovskite solar cells. On the one hand, there are physical and chemical limitations. The ion migration and corrosion of precious metals will endanger the stability of the device. On the other hand, there are technical and financial limitations. The deposition of metal electrodes requires special equipment and high vacuum technology under inert conditions, which makes the deposition conditions on large-area substrates harsh and costly.

[0004] Carbon materials are widely available, with excellent chemical inertness, cost-effectiveness and good conductivity. They also have a work function similar to that of gold. With simple operation and mild preparation processes such as blade coating, screen printing, inkjet printing, etc., carbon electrodes have become the most attractive choice to replace traditional metal electrodes. Carbon electrodes are usually deposited from carbon slurry, and the main components of carbon slurry are carbon particles and binders. Among them, the binder is used as a functional additive to make the carbon particles bond to each other and improve the film-forming property of the slurry itself. It does not help the contact interface between the carbon electrode formed with the carbon slurry after the subsequent perovskite crystallization is completed; the binders known in the prior art are organic (for example: cellulose, polyethylene glycol, starch, polyvinyl pyrrolidone, polyvinyl acetate, polymethyl methacrylate, ionic liquid), and these organic binder materials will be sintered and removed during the subsequent sintering of carbon slurry to form carbon electrodes; in addition, commonly used binders also include zirconium oxide. Carbon slurry using zirconium oxide as a binder can be applied to the ZrO2 spacer layer of mesoscopic perovskite solar cells to form carbon electrodes.

[0005] The role of the counter electrode is to provide a channel for carrier transmission for perovskite solar cells, allowing holes to flow to the external circuit, thereby generating current. Electrical conductivity is an important characteristic for evaluating the performance of carbon electrodes. Low resistance enables the electrode to transport charges more efficiently, and a counter electrode with poor conductivity will hinder the transmission of carriers, further limiting the performance of the device. The current conductivity of carbon electrodes (conductivity of about 4.88×10 3 S / m, as exemplified in Comparative Example 1 below) and 4.10×10 7 There is still a considerable gap between S / m, which is one of the main reasons for the performance difference between carbon-based perovskite solar cells and metal-based perovskite solar cells. The resistance of the carbon electrode mainly comes from the resistance of the carbon material body and the contact resistance between the carbon material particles. There are several standards for carbon materials prepared into carbon slurries: micron-level particle size, uniform distribution, high purity and low light adsorption capacity. Therefore, existing carbon slurries often use graphite as the main component (ie, main conductive particles). Large graphite particles are poorly connected. The existing technology mostly uses carbon black as the conductive medium particles. The addition of carbon black can bridge the space between graphite particles and improve the conductivity between particles. However, the conductivity of carbon black is much worse than that of graphite. If you want to further improve the conductivity of the electrode, you need to select small particles with better conductivity to replace carbon black and reduce the resistance of the material body.

[0006] In addition, when the porous counter electrode is applied to the mesoscopic perovskite solar cell, it will be in direct contact with the perovskite. The back interface contact formed affects the carrier transfer efficiency. Poor back interface contact will increase the carrier transmission barrier and the non-radiative recombination probability, which will affect the performance of the device. As mentioned earlier, the back electrode is composed of particles, which will make the back electrode and the lower layer in micron-level contact, which has a large roughness compared with the atomic-level contact formed by the vacuum-evaporated metal electrode. At the same time, the inert surface of graphite has a low affinity with perovskite and cannot well support the growth of perovskite and fill the gaps. All these lead to the formation of poor back interface contact. Traditional carbon black medium particles are also not sufficient to serve as excellent attachment sites for perovskite to improve the back interface contact. Summary of the invention

[0007] In view of the above defects or improvement needs of the prior art, the purpose of the present invention is to provide a conductive paste and a preparation method thereof and its application in a porous back electrode. By introducing titanium oxides such as TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9 into the traditional conductive paste to replace the traditional conductive medium particles (such as carbon black), the high wettability of titanium oxide promotes the attachment of perovskite on the back electrode and forms a close contact, which can improve the contact interface between the back electrode formed by the conductive paste and the Pb-based perovskite in the mesoscopic perovskite solar cell. There is a strong interaction between the oxygen of the added titanium oxides such as TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9 and the Pb of the perovskite, which is the reason why the titanium oxide and the perovskite have good wettability, which can provide good nucleation sites and provide support for the formation of reliable back interface contact, thereby improving the device performance, thereby solving the technical problem that the back interface contact of the porous counter electrode in the prior art is poor, which reduces the performance of the mesoscopic perovskite solar cell.

[0008] To achieve the above object, according to one aspect of the present invention, a conductive paste is provided, comprising main conductive particles, conductive medium particles and functional additives dispersed in a solvent, wherein the functional additives include a binder and a pore former, the mass proportion of the main conductive particles is higher than the mass proportion of the conductive medium particles, and the conductive medium particles are at least one of TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9;

[0009] The electrode formed corresponding to the conductive paste can improve the contact between the electrode and the Pb-based perovskite.

[0010] As a further preferred embodiment of the present invention, the conductive paste is used to form a back electrode in contact with the Pb-based perovskite in a mesoscopic perovskite solar cell, and the correspondingly formed back electrode can improve the contact with the Pb-based perovskite.

[0011] As a further preferred embodiment of the present invention, the titanium oxide is Ti4O7 or Ti5O9.

[0012] As a further preferred embodiment of the present invention, the main conductive particles are at least one of graphite, carbon black, graphene, carbon nanotubes, and carbon fibers.

[0013] As a further preference of the present invention, the mass percentage of the main conductive particles in the conductive paste is 20-30%, the mass percentage of the conductive medium particles in the conductive paste is 1.5%-6%, the mass percentage of the binder in the conductive paste is 1-5%, the mass percentage of the pore-forming agent in the conductive paste is 1-10%, and the rest is solvent.

[0014] As a further preferred embodiment of the present invention, the binder is one or more of zirconium oxide, cellulose, polyethylene glycol, starch, polyvinyl pyrrolidone, polyvinyl acetate, polymethyl methacrylate, and ionic liquid;

[0015] The pore-forming agent is one or more of cellulose, polystyrene and polyvinyl pyrrolidone;

[0016] The solvent is one or more of n-butanol, terpineol, ethylene glycol, chlorobenzene and ethyl acetate.

[0017] According to another aspect of the present invention, the present invention provides a method for preparing the above-mentioned conductive paste, characterized in that the main conductive particles, conductive medium particles, functional additives and solvents are mixed, wherein the functional additives include a binder and a pore-forming agent, and the solvent is referred to as a first solvent; a second solvent with a low boiling point is added to the mixture system at the same time, and dispersed evenly to obtain a uniform dispersion liquid, and finally only the second solvent is removed by a rotary evaporation method to obtain a conductive paste;

[0018] Wherein, the boiling point of the second solvent is lower than that of the first solvent.

[0019] As a further preferred embodiment of the present invention, the uniform dispersion is achieved by ultrasound, mechanical stirring or ball milling;

[0020] The second solvent is ethanol.

[0021] According to another aspect of the present invention, the present invention provides a porous back electrode, characterized in that it is obtained by printing the above conductive paste by a screen printing method and then removing the binder, pore-forming agent and solvent therein by annealing;

[0022] Preferably, the annealing temperature used in the annealing is 400°C to 450°C.

[0023] According to another aspect of the present invention, the present invention provides a mesoscopic perovskite solar cell, wherein the perovskite material is a Pb-based perovskite, characterized in that it includes the above-mentioned porous back electrode.

[0024] Through the above technical scheme conceived by the present invention, compared with the prior art, titanium oxides such as TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9 are introduced into the traditional conductive paste to replace the traditional conductive medium particles (such as carbon black), thereby improving the affinity with perovskite, improving the back interface contact, and improving the device performance of the mesoscopic perovskite solar cell. Titanium oxides such as TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9 have a strong affinity with perovskite, thereby providing nucleation sites, promoting perovskite crystallization, and improving the back interface contact. In addition, in addition to having high conductivity, the conductive medium particles must also have certain high temperature resistance (temperature resistance must be greater than 400°C). The annealing of conductive slurry often requires an annealing temperature of more than 400°C to remove functional additives in the slurry (i.e., binders and pore-forming agents). The titanium oxides TiO2, Ti4O7, and Ti5O9 used in the present invention can withstand annealing temperatures above 400°C and are compatible with existing binders, pore-forming agents, and annealing processes. Although TiO and Ti2O3 cannot withstand a high temperature of 400°C, they will generate TiO2 after high-temperature oxidation, which is still required.

[0025] Furthermore, based on the present invention, titanium oxides Ti4O7 and Ti5O9 are particularly preferably used as conductive medium particles. They are titanium oxides rich in oxygen vacancy defects. Their introduction can bridge the gaps between the main conductive particles (such as graphite sheets). At the same time, their own high conductivity can reduce the bulk resistance of the material, improve the conductivity of the conductive paste, and obtain a high-conductivity conductive paste, thereby improving the conductivity of the porous counter electrode, promoting the transmission of carriers in the counter electrode, and further improving the device performance.

[0026] The conductive paste commonly used in the prior art to form the counter electrode often includes components such as main conductive particles, conductive medium particles, binders, pore formers, and solvents (binders and pore formers are sometimes a chemical substance, but they play different roles in different preparation processes); among them, the main conductive particles are the main conductive part of the counter electrode, occupying a high mass ratio in the entire conductive paste; the conductive medium particles are bridges between the main conductive particles that cannot contact each other, providing important conductive channels. The conductive medium particles commonly used in the prior art (for example, including carbon black), although the corresponding conductive paste also has a high conductivity effect, still has room for improvement compared to gold electrodes. However, there are certain limitations on the replacement of the conductive medium. The formation of the porous counter electrode is formed at a high temperature of 400°C, and the pore former and binder are decomposed to form. The high temperature environment requires that the particulate matter cannot change, such as decomposition, oxidation, and reaction with other substances in the conductive paste. Secondly, due to the limitation of the mesoscopic perovskite solar cell, the counter electrode is in direct contact with the perovskite, requiring the particulate matter to have good chemical stability and not to react with the perovskite. Finally, the counter electrode also has a very important influence on the formation of the back interface in the mesoscopic perovskite solar cell. This is closely related to the composition of the counter electrode. The wettability between the perovskite solution and the attachment (the material in the counter electrode at the back interface) has a direct impact on the heterogeneous nucleation of the perovskite. Better wetting (smaller contact angle) means that the perovskite core and the substrate active site have a higher affinity.

[0027] Specifically, the present invention can achieve the following beneficial effects:

[0028] (1) The present invention provides a method for preparing a high-conductivity conductive paste and applies it to a porous counter electrode. The present invention uses titanium oxides such as TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9 to replace the carbon black in the carbon counter electrode of a mesoscopic perovskite solar cell. These titanium oxides TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9 have good wettability with perovskite and provide good nucleation sites. At the same time, there is a strong interaction between the oxygen of the titanium oxide and the Pb of the perovskite, which can improve the contact between the back electrode formed by the conductive paste and the Pb-based perovskite in the mesoscopic perovskite solar cell, thereby improving the performance of the mesoscopic perovskite solar cell. Moreover, taking Ti4O7 as an example, the addition of Ti4O7 can reduce the bulk resistance of the conductive medium particles, effectively improve the conductivity of the porous counter electrode, reduce the difference in conductivity with the metal electrode, enhance the transmission of carriers on the electrode, and further improve the performance of the solar cell.

[0029] (2) Taking the case where the main conductive particles are graphite as an example, as compared with Example 1 and Comparative Example 1 below, based on the present invention, by using titanium dioxide Ti4O7 as the conductive medium particles, the Ti4O7 highly conductive particles can bridge the gaps that are not in contact between the main conductive particles, reduce the contact resistance, and provide additional conductive channels; their own high conductivity reduces the bulk resistance of the component particles, thereby reducing the overall resistivity of the porous back electrode and promoting the collection and transmission of carriers on the porous counter electrode; they have a strong interaction and good wettability with perovskite, are easy to nucleate and grow perovskite, enhance the back interface contact, improve the carrier transfer efficiency, reduce non-radiative recombination, and obtain a high-performance mesoscopic perovskite solar cell.

[0030] As compared with Example 1 and Comparative Example 1 below, based on the present invention, the use of Ti4O7 to replace the carbon black in the porous counter electrode can reduce the resistivity of the electrode from 0.0205Ω·cm to 0.0149Ω·cm, and the resistivity is reduced by nearly 27%; after adding Ti4O7 to the back electrode, it can fill the gaps between graphite to improve the contact between particles and reduce the contact resistance, and it can also provide nucleation sites for the perovskite solution to make it grow and fill the gaps in the contact between the back electrode and the perovskite layer, thereby improving the contact between the back electrode (formed by a conductive slurry) and the Pb-based perovskite in the mesoscopic perovskite solar cell; the photoelectric conversion efficiency of the mesoscopic perovskite solar cell prepared by using the carbon slurry in which Ti4O7 replaces the carbon black in the porous counter electrode can be increased to 19.65%, showing efficient carbon-based device performance.

[0031] (3) Taking Example 2 as an example, Example 2 uses TiO2 to replace the carbon black in the porous counter electrode. Unlike Ti4O7, TiO2 has poor conductivity due to the lack of oxygen vacancy defects (TiO2 is often used as a semiconductor material). After the introduction of the back electrode, the conductivity of the electrode is not significantly improved (to 0.0209Ω·cm), while its relatively good wettability can improve the back interface contact to a certain extent. Therefore, the photoelectric conversion efficiency of the device is still improved compared with that of Comparative Example 1 (using traditional carbon black material), which is 18.52%.

[0032] (4) Moreover, the titanium oxides TiO2, Ti4O7, and Ti5O9 introduced in the present invention can withstand the process of annealing and sintering at a high temperature of 400°C to 450°C to remove the binder and pore-forming agent, and the TiO2, Ti4O7, and Ti5O9 particle materials do not change. Although TiO and Ti2O3 cannot withstand the high temperature of 400°C to 450°C, they will oxidize and generate TiO2 at this annealing temperature, and the final effect is the same as that of Example 2 below. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1This is a voltage-current density characteristic curve of the printable mesoscopic perovskite solar cell device based on a porous counter electrode obtained in Example 1 of the present invention.

[0034] Figure 2 The following are scanning electron microscope (SEM) images of the cross sections of the perovskite solar cells obtained in Example 1 and Comparative Example 1, including the back interface information. Figure 2 (a) corresponds to the perovskite solar cell obtained in Example 1, Figure 2 (b) corresponds to the perovskite solar cell obtained in Example 1.

[0035] Figure 3 This is a comparison diagram of the O1s orbital of the X-ray photoelectron spectroscopy (XPS) of Ti4O7 and TiO2.

[0036] Figure 4 Ti4O7, CB, TiO2 and perovskite (FA 0.6 MA 0.4 Contact angle test comparison chart of PbI3) solution. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0038] The preparation process of the mesoscopic perovskite solar cell in the following examples and comparative examples is as follows: a dense hole blocking layer, a mesoporous electron transport layer, a mesoporous spacer layer, and a porous counter electrode are sequentially deposited on a transparent conductive substrate, and finally the perovskite is dripped and filled into the three-layer mesoporous film. The porous counter electrode can be obtained by printing the electrode slurry on the substrate using a screen printing method, and removing the binder, pore-forming agent and solvent by high-temperature annealing.

[0039] In addition, the preparation process of the conductive paste, similar to the prior art, can be assisted in dispersing the components by using a second solvent with a low boiling point (such as ethanol).

[0040] Example 1

[0041] The porous counter electrode slurry of the perovskite solar cell of this embodiment includes the following components:

[0042] Graphite: 6.5g;

[0043] Tetratitanium heptoxide: 2g;

[0044] Zirconium oxide: 1.6 g;

[0045] Ethyl cellulose: 1.2 g;

[0046] Terpineol: 23g;

[0047] The preparation method of the porous counter electrode slurry for the perovskite solar cell of this embodiment comprises the following steps: weighing the quantitative graphite, titanium tetraoxide (Ti4O7), zirconium oxide (ZrO2), ethyl cellulose, pinene alcohol, and an appropriate amount of ethanol, and placing these materials in a clean agate ball milling jar, placing them in a star-shaped ball mill and milling them at a speed of 350r / min for 60h. Finally, the excess ethanol is spun out by rotary evaporation to obtain the desired carbon slurry.

[0048] Then, a porous counter electrode was prepared on the substrate by screen printing. After printing, the substrate was transferred to a 75°C hot plate for drying, and then transferred to another hot plate for programmed annealing. Specifically, the hot plate was gradually heated from room temperature to 400°C at a rate of no more than 10°C / min, and then kept at 400°C for 40 minutes and then cooled naturally to obtain a porous counter electrode.

[0049] Preferably, when the substrate is glass, the porous back electrode can be used to test its resistivity; when the substrate is a dense layer / mesoporous electron transport layer / mesoporous spacer layer, the porous counter electrode is used to prepare a perovskite solar cell.

[0050] The perovskite solar cell of this embodiment uses the counter electrode slurry obtained by the method to prepare a porous back electrode, and the specific steps include:

[0051] (1) heating the hot plate to 450°C at a rate not higher than 10°C / min, and at this temperature, spraying a TiO2 dense layer solution uniformly onto a fluorine-doped tin oxide (FTO) transparent conductive glass by spray pyrolysis;

[0052] (2) Using screen printing, the mesoporous TiO2 slurry is evenly coated on the FTO glass with a dense TiO2 layer and annealed on a hot plate at 500°C to form a TiO2 mesoporous layer;

[0053] (3) Using screen printing, the mesoporous ZrO2 slurry is evenly coated on the FTO glass with the mesoporous TiO2 layer and dried at 75°C to form a ZrO2 spacer layer;

[0054] (4) Using screen printing, the carbon slurry is evenly coated on the FTO glass with the mesoporous TiO2 / mesoporous ZrO2 layer, and then annealed at 400°C for 40 minutes to obtain a porous back electrode;

[0055] (5) A methylamine formamidinium lead iodide perovskite precursor solution is dripped onto the surface of the porous back electrode and annealed and crystallized to finally obtain a perovskite solar cell.

[0056] Example 2

[0057] The porous counter electrode slurry of the perovskite solar cell of this embodiment includes the following components:

[0058] Graphite: 6.5g;

[0059] Titanium dioxide: 2g;

[0060] Zirconium oxide: 1.6 g;

[0061] Ethyl cellulose: 1.2 g;

[0062] Terpineol: 23g;

[0063] The preparation method of the perovskite solar cell and the preparation method of the porous counter electrode of this embodiment are exactly the same as those of Embodiment 1, with the only difference being that the conductive medium particles of the porous counter electrode are titanium dioxide.

[0064] Comparative Example 1

[0065] The porous counter electrode slurry of the perovskite solar cell of this comparative example includes the following components:

[0066] Graphite: 6.5g;

[0067] Carbon black: 2g;

[0068] Zirconium oxide: 1.6 g;

[0069] Ethyl cellulose: 1.2 g;

[0070] Terpineol: 23g;

[0071] The preparation method of the perovskite solar cell and the preparation method of the porous counter electrode of this comparative example are exactly the same as those of Example 1, with the only difference being that the conductive medium particles of the porous counter electrode adopt carbon black, a component of the traditional carbon counter electrode.

[0072] Comparative Example 2

[0073] The porous counter electrode slurry of the perovskite solar cell of this comparative example includes the following components:

[0074] Graphite: 6.5g;

[0075] Tetratitanium heptoxide: 6.5g;

[0076] Zirconium oxide: 1.6 g;

[0077] Ethyl cellulose: 1.2 g;

[0078] Terpineol: 23g;

[0079] The preparation method of the perovskite solar cell and the preparation method of the porous counter electrode of this comparative example are exactly the same as those of Example 1, with the only difference being that the amount of tetratitanium heptoxide used is equivalent to that of graphite.

[0080] In this comparative example, the amount of tetratitanium heptoxide used is based on CB and is added with the goal of replacing carbon black. At this time, the amount of tetratitanium heptoxide used is too much (equivalent to graphite), and accordingly, the main conductive particle material changes, which makes the proportion with other substances inconsistent, the film-forming property of the conductive slurry has problems, the printability will also be reduced, and the obtained electrode film will crack, warp, etc.

[0081] Performance Testing

[0082] In order to verify the technical effect of the highly conductive porous counter electrode described in the present invention, the square resistance and film thickness of the porous counter electrode prepared with different counter electrode slurries were obtained by four-probe and step profiler testing. After data processing, the resistivity properties that can be directly compared were obtained. In addition, the high performance of the mesoscopic perovskite solar cell based on the highly conductive porous counter electrode was verified by solar simulator testing. The specific parameters include the open circuit voltage V OC , current density J SC , fill factor FF, photoelectric conversion efficiency PCE.

[0083] After the experiment, the results are shown in the following table.

[0084]

[0085] By table and Figure 1 It can be obtained that the resistivity of the porous counter electrode (corresponding to comparative example 1) with carbon black as the conductive medium particles is 0.0205Ω·cm. After replacing the carbon black with highly conductive Ti4O7 particles (corresponding to Example 1), the conductivity of the counter electrode is increased by nearly 27% (0.0149Ω·cm). The resistance of the porous counter electrode film mainly comes from the bulk resistance of the component particles and the contact resistance between the particles. On the one hand, the Ti4O7 particles replacing carbon black play a role in bridging the gaps between the main conductive particles that cannot contact, reducing the contact resistance and providing additional conductive channels. In addition, the complete graphite layer cannot allow the perovskite solution to penetrate, so the conductive medium particles can also destroy the preferential orientation of the graphite sheets. On the other hand, the conductivity of Ti4O7 itself is better than that of carbon black, and can even be comparable to that of graphite, which reduces the bulk resistance of the component particles and further improves the conductivity of the counter electrode.

[0086] Figure 2Scanning electron microscopy (SEM) was used to study the morphology of the perovskite back interface, revealing the effect of the introduction of Ti4O7 on the back interface contact. Figure 2 (a) is a SEM image of the cross section of the device prepared in Comparative Example 1. As shown in the figure, voids are formed when the back electrode film is printed on the ZrO2 layer. Since graphite sheets and carbon black are not good nucleation attachment points for perovskite crystallization, even if the CB part fills the uncontacted area between the graphite and the ZrO2 layer (before the back interface is formed), the voids at the back interface cannot be completely filled after the perovskite crystallization is completed. The introduction of Ti4O7 in Example 1 enhances the connection between the counter electrode and the perovskite and improves the back interface contact, as shown in FIG. Figure 2 As shown in (b), the voids are effectively filled, the contact interface between the electrode and the perovskite is improved, and a close contact interface is obtained.

[0087] The performance of the device responsive to the porous counter electrode prepared based on the conductive paste of the present invention is also significantly improved. Compared with Comparative Example 1, the short-circuit current density of the device in Example 1 is increased from 23.94 mA·cm -2 Increased to 24.57 mA cm -2 The conductivity of the counter electrode is directly related to the series resistance of the device. The series resistance will decrease in response to the improvement of conductivity, and the fill factor FF, which is closely related to the series resistance, will be improved. The specific parameters in the table also show that the FF of the device increased from 0.77 to 0.79, and the reduction of non-radiative recombination caused by the improvement of the back interface contact was directly reflected in the open circuit voltage parameter, which increased from 978mV to 1018mV. Finally, the photoelectric conversion efficiency of the device reached up to 19.65%.

[0088] Similarly, the performance of Example 2 was verified, and the results were as follows:

[0089]

[0090] Similar to the understanding that TiO2 is usually used as a semiconductor material in the prior art, TiO2 has poor conductivity, which does not improve the conductivity of the back electrode. In fact, compared with the carbon electrode obtained in Comparative Example 1, the resistivity is increased and the conductivity is deteriorated. This is mainly because, Figure 3 As shown (the green part in the figure is the oxygen vacancy content; OV marked in the figure, i.e., oxygen vacancies), compared with Ti4O7, the oxygen vacancies of TiO2 are obviously insufficient.

[0091] The reason why Example 2 can still improve the photoelectric conversion efficiency of the device from 17.93% in Comparative Example 1 to 18.52% is mainly because TiO2 still has improved wettability with Pb-based perovskite compared to CB. After pressing Ti4O7, CB, and TiO2 powders into tablets, 0.12 mol / L FA 0.6MA 0.4 PbI3 perovskite solution (solvent: DMF / DMSO, volume ratio: 4:1) was dropped on the pressed powder, and their respective contact angles were measured using a contact angle meter. The results are shown in Figure 4 As shown in the figure: CB has the largest contact angle, which is 31.04°; TiO2 is second, which is 26.47°; and Ti4O7 has the smallest contact angle, which is 18.24°. It can be seen that TiO2 improves the back interface contact to a certain extent, but because its wettability is lower than that of Ti4O7, the performance improvement effect of the final mesoscopic solar cell is lower than that of Example 1.

[0092] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A conductive paste comprising main conductive particles, conductive medium particles and functional additives dispersed in a solvent, wherein: The functional additives include a binder and a pore former, the mass proportion of the main conductive particles is higher than the mass proportion of the conductive medium particles, and the conductive medium particles are at least one of TiO, TiO2, Ti2O3, Ti4O7, and Ti5O9; The electrode formed corresponding to the conductive paste can improve the contact between the electrode and the Pb-based perovskite.

2. The conductive paste according to claim 1, characterized in that: The conductive paste is used to form a back electrode in contact with a Pb-based perovskite in a mesoscopic perovskite solar cell, and the correspondingly formed back electrode can improve the contact with the Pb-based perovskite.

3. The conductive paste according to claim 1, characterized in that: The titanium oxide is Ti4O7 or Ti5O9.

4. The conductive paste according to claim 1, characterized in that: The main conductive particles are at least one of graphite, carbon black, graphene, carbon nanotubes, and carbon fibers.

5. The conductive paste according to claim 1, characterized in that: The mass percentage of the main conductive particles in the conductive paste is 20-30%, the mass percentage of the conductive medium particles in the conductive paste is 1.5%-6%, the mass percentage of the binder in the conductive paste is 1-5%, the mass percentage of the pore former in the conductive paste is 1-10%, and the rest is solvent.

6. The conductive paste according to claim 1, characterized in that: The binder is one or more of zirconium oxide, cellulose, polyethylene glycol, starch, polyvinyl pyrrolidone, polyvinyl acetate, polymethyl methacrylate, and ionic liquid; The pore-forming agent is one or more of cellulose, polystyrene and polyvinyl pyrrolidone; The solvent is one or more of n-butanol, terpineol, ethylene glycol, chlorobenzene and ethyl acetate.

7. The method for preparing the conductive paste according to any one of claims 1 to 6, characterized in that: The main conductive particles, conductive medium particles, functional additives and solvent are mixed, wherein the functional additives include a binder and a pore former, and the solvent is referred to as a first solvent; a second solvent with a low boiling point is added to the mixture system, and dispersed evenly to obtain a uniform dispersion; finally, only the second solvent is removed by a rotary evaporation method to obtain a conductive paste; Wherein, the boiling point of the second solvent is lower than that of the first solvent.

8. The preparation method according to claim 7, characterized in that: The uniform dispersion is achieved by ultrasound, mechanical stirring or ball milling; The second solvent is ethanol.

9. A porous back electrode, characterized in that: The conductive paste is obtained by printing the conductive paste according to any one of claims 1 to 6 by a screen printing method and then removing the binder, pore-forming agent and solvent therein by annealing; Preferably, the annealing temperature used in the annealing is 400°C to 450°C.

10. A mesoscopic perovskite solar cell, wherein the perovskite material is a Pb-based perovskite, characterized in that: Comprising the porous back electrode as claimed in claim 9.

Citation Information

Patent Citations

  • Perovskite solar cell and preparation method for thermoplastic carbon counter electrode

    CN104134752A

  • Electrically conductive coating composition, electrically conductive material, method for producing the electrically conductive coating composition, and method for producing the electrically conductive material

    CN107849395A

  • Cheap stable perovskite solar energy cell and driven photocatalytic device

    CN108258120A

  • Conductive paste, preparation method thereof and application of conductive paste in porous back electrode

    CN116313219A

  • Mesoporous titanium dioxide slurry and application thereof in preparation of printable mesoscopic perovskite solar cell electron transport layer

    CN117790045A

Cited By

  • Gold electrode conductive paste and electronic circuit

    CN119724680A

  • A gold electrode conductive paste and an electronic circuit

    CN119724680B