Rare earth aluminum alloy high-strength, high-conductivity and high-stability cable and preparation method thereof

By adding specific elements and technical processes to the aluminum alloy, high-strength and high-conductivity aluminum alloy monofilaments were prepared, which solved the problem of low tensile strength and conductivity of aluminum alloy cables, and significantly improved the stability and use of cables. life.

CN118942767AActive Publication Date: 2024-11-12GUANGDONG TENGYUETONG CABLE CO LTD

Patent Information

Application Number
CN202411038886.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The tensile strength, conductivity and creep resistance of existing aluminum alloy cables have low tensile strength, electrical conductivity and creep resistance, which affects its use stability and life.

Method used

High-strength, high-conductivity and high-stability cables are used for rare earth aluminum alloys. High-strength, high-conductivity and high-stability cables are prepared by adding elements such as rhenium, yttrium, cobalt, silicon carbide and nanographene to the aluminum alloy, combined with ball milling and electromagnetic induction furnace smelting technology. Aluminum alloy monofilament is a linear aluminum alloy, and the overall performance of the cable is enhanced by multi-layer insulation and sheathing structure.

Benefits of technology

It improves the tensile strength and conductivity of aluminum alloy monofilaments, enhances the high-temperature stability and creep resistance of the cable, and extends the service life by no less than 45 years.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942767A_ABST
    Figure CN118942767A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth aluminum alloy high-strength, high-conductivity and high-stability cable and a preparation method thereof, and belongs to the technical field of aluminum alloy cables. The rare earth aluminum alloy high-strength high-conductivity high-stability cable comprises aluminum alloy monofilaments, and the aluminum alloy monofilaments comprise, by mass, 2.0%-4.1% of rare earth, 1.0%-1.2% of rhenium, 0.8%-1.5% of copper, 0.5%-0.8% of yttrium, 0.5%-1.0% of cobalt, 0.2%-0.5% of nickel, 0.05%-0.3% of silicon carbide, 0.1%-0.8% of aluminum chloride, the total content of impurity elements smaller than or equal to 0.1% and the balance aluminum. The invention further discloses a preparation method of the rare earth aluminum alloy high-strength, high-conductivity and high-stability cable. By the adoption of the rare earth aluminum alloy high-strength high-conductivity high-stability cable and the preparation method thereof, the problems that an existing aluminum alloy cable is low in tensile strength and conductivity and poor in creep resistance can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy cables, and in particular to a rare earth aluminum alloy high-strength, high-conductivity, high-stability cable and a preparation method thereof. Background Art

[0002] With the continuous development of society, the scope and occasions of cable use are increasing, and the requirements for cables are getting higher and higher. In particular, schools, hospitals, real estate and other projects have stricter fire protection requirements, and higher requirements are put forward for cables in terms of high temperature resistance, high strength, and high conductivity. Domestic cables generally use copper as conductors, and the price of copper is relatively high, and the price of copper cables is relatively high. Aluminum alloy cables have the advantages of light weight and low price, so aluminum alloy cables have been developed. However, the conductivity, heat resistance and tensile strength of aluminum alloys are relatively low, and the problem of broken wires is prone to occur during production and use, which increases the production cost of aluminum alloy cables and affects the service life of aluminum alloy cables.

[0003] The existing patent CN202010720663.6 discloses a rare earth high-iron aluminum alloy cable, which belongs to the technical field of power cable aluminum alloy materials. The monofilament of the rare earth high-iron aluminum alloy cable includes the following components by mass percentage: iron 1.0-1.5%, silicon 0.03-0.08%, copper 0.02-0.08%, manganese 0.02-0.08%, magnesium 0.01-0.05%, titanium 0.01-0.08%, zirconium 0.01-0.08%, chromium 0.05-0.1%, strontium 0.01-0.05%, rare earth 0.8-1.5%, the total impurity content ≤0.1%, and the balance aluminum. The prepared rare earth high iron aluminum alloy monofilament has an elongation of >35%, a tensile strength of >120MPa, a 90° bending number of more than 38 times, a DC resistivity of ≤0.029 at 20°C, a conductivity of ≥62.0%IACS, a bending radius of 7D, a rebound performance of 40% less than that of copper cable, and a creep resistance of 300% greater than that of aluminum core cable, and a service life of not less than 40 years. However, the tensile strength, conductivity and creep resistance of the aluminum alloy cable monofilament in the above patent are relatively low, which affects the stability and service life of the cable. Summary of the invention

[0004] The purpose of the present invention is to provide a rare earth aluminum alloy high-strength, high-conductivity and high-stability cable and a preparation method thereof, so as to solve the problems of low tensile strength, low conductivity and poor creep resistance of existing aluminum alloy cables.

[0005] To achieve the above-mentioned purpose, the present invention provides a rare earth aluminum alloy high-strength, high-conductivity and high-stability cable, comprising an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in mass percentage: rare earth 2.0%-4.1%, rhenium 1.0%-1.2%, copper 0.8%-1.5%, yttrium 0.5%-0.8%, cobalt 0.5%-1.0%, nickel 0.2%-0.5%, silicon carbide 0.05%-0.3%, aluminum chloride 0.1%-0.8%, the total content of impurity elements ≤0.1%, and the balance is aluminum.

[0006] Preferably, the rare earth element is a mixture of cerium, holmium, dysprosium and europium, wherein the mass percentage of cerium is 0.8%-1.5%, the mass percentage of holmium is 0.3%-1.0%, the mass percentage of dysprosium is 0.2%-0.8%, and the mass percentage of europium is 0.2%-0.8%.

[0007] Preferably, it includes an aluminum alloy conductor, which is made of twisted aluminum alloy monofilaments, an insulating layer is arranged on the outside of the aluminum alloy conductor, a plurality of aluminum alloy conductors are wrapped with glass fiber tapes on the outside, a filling layer is arranged between the glass fiber tapes and the insulating layer, an inner sheath layer is arranged on the outside of the glass fiber tapes, an outer sheath layer is arranged on the outside of the inner sheath layer, and an armor layer is arranged between the inner sheath layer and the outer sheath layer.

[0008] Preferably, the insulating layer is a cross-linked polyethylene layer, the armor layer is a galvanized steel strip layer, and the outer sheath layer is a cross-linked polyethylene layer.

[0009] The method for preparing the above-mentioned rare earth aluminum alloy high-strength, high-conductivity and high-stability cable comprises the following steps:

[0010] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition;

[0011] S2, melting the aluminum ingot, placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid;

[0012] S3, grinding, putting silicon carbide, aluminum chloride, nano-graphene, and nano-aluminum powder into a ball mill for grinding and mixing to obtain a mixed powder; using an electromagnetic induction furnace to melt the mixed powder, using argon gas for protection during the melting process, and cooling after the melting is completed to obtain an aluminum-based composite material;

[0013] S4, adding the raw materials and the aluminum-based composite material into aluminum liquid, adding a grain refiner into the aluminum liquid, adding oxidized red sand powder into the aluminum liquid for smelting, refining and degassing, melting evenly and then keeping warm to obtain rare earth aluminum alloy liquid;

[0014] S5, casting, casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars;

[0015] S6, rolling, rolling the rare earth aluminum alloy strip through a rolling mill to form a rare earth aluminum alloy rod with a diameter of Φ9.0 mm;

[0016] S7, drawing, using a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical rare earth aluminum alloy monofilament, and twisting the rare earth aluminum alloy monofilament into a rare earth aluminum alloy conductor on a frame-type stranding machine using a special-shaped stranding die;

[0017] S8, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing;

[0018] S9, insulation, after cooling, the outside of the rare earth aluminum alloy conductor is extruded with a cross-linked polyethylene material for insulation;

[0019] S10, Cabling and sheathing: Place 3-4 insulated cores on a cabling machine for filling. After filling, wrap them with glass fiber tape and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with polyethylene material to form a cable.

[0020] Preferably, in S2, the purity of the aluminum ingot is not less than 99.8%, and the melting temperature is 750°C-800°C.

[0021] Preferably, in S3, the addition amount of nanographene is 0.02%-0.8%, the grinding time is 30 minutes, and the melting temperature of the mixed powder is 750°C-800°C.

[0022] Preferably, in S4, the grain refiner is Al-5Ti-B refiner, and the mass percentage of the grain refiner is 0.5%-1%.

[0023] Preferably, in S8, the annealing temperature is 300°C±10°C, and the annealing time is 6 hours to 9 hours.

[0024] The rare earth aluminum alloy single wire prepared by the above-mentioned method for preparing a rare earth aluminum alloy high-strength, high-conductivity and high-stability cable has an elongation of ≥30% and a tensile strength of 180N / mm 2 -240N / mm 2 , 90° bending times more than 30 times, DC resistivity ≤0.0270Ω / m at 20℃, conductivity 64%-65%, bending radius 7D-10D, compared with copper cable, its rebound performance is reduced by 40%, compared with aluminum core cable, its creep resistance is increased by 380%, and its service life is not less than 45 years.

[0025] The advantages and positive effects of the rare earth aluminum alloy high-strength, high-conductivity, high-stability cable and the preparation method thereof described in the present invention are:

[0026] 1. The present invention adds rare earth elements such as cerium, holmium, dysprosium and europium to the aluminum alloy. The rare earth elements modify the aluminum alloy, which can effectively refine the grains of the aluminum alloy and improve the strength and toughness of the aluminum alloy. The cerium element is mainly used to refine the grains of the aluminum alloy and purify the alloy. The holmium, dysprosium and europium elements can enhance the thermal stability of the aluminum alloy and improve the high temperature performance of the aluminum alloy.

[0027] 2. The present invention adds silicon carbide to the aluminum alloy. Silicon carbide as a hard particle can not only improve the hardness and wear resistance of the aluminum alloy, but also improve the strength of the aluminum alloy. In addition, the good thermal conductivity of silicon carbide can improve the thermal conductivity of the aluminum alloy and improve the high temperature resistance of the aluminum alloy. It can also serve as a heterogeneous nucleation point of the aluminum alloy to promote the crystallization of the aluminum alloy, thereby achieving the effect of grain refinement. In addition, silicon carbide can improve the oxidation resistance or corrosion resistance of the aluminum alloy.

[0028] 3. The good electrical conductivity of the nanographene in the present invention can improve the electrical conductivity of the aluminum alloy and enhance the tensile strength and toughness of the aluminum alloy.

[0029] 4. The present invention adds rhenium, yttrium and cobalt metal elements to the aluminum alloy. The rhenium element increases the high temperature strength and creep resistance of the aluminum alloy and improves the thermal stability of the aluminum alloy cable. The yttrium element can refine the grains of the aluminum alloy and improve the strength, toughness and heat resistance of the aluminum alloy. The cobalt element improves the strength and heat resistance of the aluminum alloy through solid solution strengthening and precipitation phase strengthening.

[0030] 5. The present invention adopts ball milling to mix silicon carbide, nano-graphene and aluminum, which is conducive to achieving uniform dispersion of silicon carbide and nano-graphene in aluminum alloy and improving the uniformity of their dispersion.

[0031] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic diagram of a cable cross-section structure according to an embodiment of the present invention;

[0033] Figure 2 is a flow chart of an embodiment of the present invention.

[0034] Reference numerals

[0035] 1. Rare earth aluminum alloy conductor; 2. Insulation layer; 3. Filling layer; 4. Glass fiber tape; 5. Inner sheath layer; 6. Armor layer; 7. Outer sheath layer. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0037] Unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0038] Figure 1 Schematic diagram of the cable cross-section structure of an embodiment of the present invention. Figure 1 As shown, the rare earth aluminum alloy high-strength, high-conductivity, high-stability cable includes an aluminum alloy conductor, which is made of aluminum alloy monofilaments twisted together. The aluminum alloy monofilaments are elliptical structures, and the elliptical aluminum alloy monofilaments enable the aluminum alloy monofilaments to be tightly combined together, thereby increasing the number of aluminum alloy monofilaments per unit area. An insulating layer is arranged on the outside of the aluminum alloy conductor, and the insulating layer is a cross-linked polyethylene layer, which has a good insulation effect. A plurality of aluminum alloy conductors are wrapped with glass fiber tapes on the outside, and the aluminum alloy conductors are wrapped and wound together by the glass fiber tapes. In this embodiment, four aluminum alloy conductors are arranged. A filling layer is arranged between the glass fiber tape and the insulation layer, and the filling layer is an insulating rubber to improve the insulation effect of the cable. An inner sheath layer is arranged on the outside of the glass fiber tape, an outer sheath layer is arranged on the outside of the inner sheath layer, and an armor layer is arranged between the inner sheath layer and the outer sheath layer. The armor layer is a galvanized steel tape layer, and the armor layer protects the inside of the cable. Both the inner sheath layer and the outer sheath layer are cross-linked polyethylene layers, which have a good insulation effect.

[0039] Rare earth aluminum alloy high-strength, high-conductivity and high-stability cable, including aluminum alloy monofilament, the aluminum alloy monofilament includes the following components in mass percentage: rare earth 2.0%-4.1%, rhenium 1.0%-1.2%, copper 0.8%-1.5%, yttrium 0.5%-0.8%, cobalt 0.5%-1.0%, nickel 0.2%-0.5%, silicon carbide 0.05%-0.3%, aluminum chloride 0.1%-0.8%, the total content of impurity elements ≤0.1%, and the balance is aluminum.

[0040] The rare earth element is a mixture of cerium, holmium, dysprosium and europium, wherein the mass percentage of cerium is 0.8%-1.5%, the mass percentage of holmium is 0.3%-1.0%, the mass percentage of dysprosium is 0.2%-0.8%, and the mass percentage of europium is 0.2%-0.8%.

[0041] Figure 2 FIG. 1 is a flow chart of an embodiment of the present invention. Figure 2 As shown, the method for preparing a rare earth aluminum alloy high-strength, high-conductivity, and high-stability cable comprises the following steps:

[0042] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition.

[0043] S2, melting the aluminum ingot, placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid.

[0044] The purity of aluminum ingot is not less than 99.8% and the melting temperature is 750℃-800℃.

[0045] S3, grinding, putting silicon carbide, aluminum chloride, nano-graphene and nano-aluminum powder into a ball mill for grinding and mixing to obtain a mixed powder; using an electromagnetic induction furnace to melt the mixed powder, using argon gas for protection during the melting process, cooling after the melting is completed, and obtaining an aluminum-based composite material.

[0046] The addition amount of nanographene is 0.02%-0.8%, the grinding time is 30 minutes, the particle size after grinding is powdery, and the melting temperature of the mixed powder is 750℃-800℃.

[0047] S4. Add the raw materials and aluminum-based composite materials into aluminum liquid, add a grain refiner into the aluminum liquid, add oxidized red sand powder into the aluminum liquid for smelting, refining and degassing, melt evenly and keep warm to obtain rare earth aluminum alloy liquid.

[0048] The grain refiner is Al-5Ti-B refiner, and the mass percentage of the grain refiner is 0.5%-1%.

[0049] S5. Casting: casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars.

[0050] S6. Rolling: rolling the rare earth aluminum alloy strip through a rolling mill to form a Φ9.0 mm rare earth aluminum alloy rod.

[0051] S7. Drawing: Use a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical rare earth aluminum alloy monofilament, and use a special-shaped wire stranding die on a frame-type stranding machine to strand the rare earth aluminum alloy monofilament into a rare earth aluminum alloy conductor.

[0052] S8, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing.

[0053] The annealing temperature is 300°C ± 10°C, and the annealing time is 6 hours to 9 hours.

[0054] S9, insulation, after cooling, the outside of the rare earth aluminum alloy conductor is extruded with a cross-linked polyethylene material for insulation;

[0055] S10, Cabling and sheathing: Place 3-4 insulated cores on a cabling machine for filling. After filling, wrap them with glass fiber tape and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with polyethylene material to form a cable.

[0056] Example 1

[0057] A rare earth aluminum alloy high-strength, high-conductivity, high-stability cable comprises an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in mass percentage: rare earth 2.2%, rhenium 1.0%, copper 1.4%, yttrium 0.7%, cobalt 0.6%, nickel 0.5%, silicon carbide 0.2%, aluminum chloride 0.3%, the total content of impurity elements ≤0.1%, and the balance is aluminum.

[0058] The mass percentage of cerium in the rare earth elements is 1.0%, the mass percentage of holmium is 0.4%, the mass percentage of dysprosium is 0.6%, and the mass percentage of europium is 0.2%.

[0059] The method for preparing a rare earth aluminum alloy high-strength, high-conductivity and high-stability cable comprises the following steps:

[0060] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition.

[0061] S2, melting the aluminum ingot, placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid.

[0062] The purity of aluminum ingot is not less than 99.8% and the melting temperature is 750℃.

[0063] S3, grinding, putting silicon carbide, aluminum chloride, nano-graphene and nano-aluminum powder into a ball mill for grinding and mixing to obtain mixed powder; using an electromagnetic induction furnace to melt the mixed powder, using argon gas for protection during the melting process, cooling after the melting is completed, and obtaining an aluminum-based composite material.

[0064] The addition amount of nano-graphene is 0.6%, the grinding time is 30 minutes, the particle size after grinding is powdery, and the melting temperature of the mixed powder is 760°C.

[0065] S4. Add the raw materials and aluminum-based composite materials into aluminum liquid, add a grain refiner into the aluminum liquid, add oxidized red sand powder into the aluminum liquid for smelting, refining and degassing, melt evenly and keep warm to obtain rare earth aluminum alloy liquid.

[0066] The grain refiner is Al-5Ti-B refiner, and the mass percentage of the grain refiner is 0.5%.

[0067] S5. Casting: casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars.

[0068] S6. Rolling: rolling the rare earth aluminum alloy strip through a rolling mill to form a Φ9.0 mm rare earth aluminum alloy rod.

[0069] S7. Drawing: Use a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical rare earth aluminum alloy monofilament, and use a special-shaped wire stranding die on a frame-type stranding machine to strand the rare earth aluminum alloy monofilament into a rare earth aluminum alloy conductor.

[0070] S8, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing.

[0071] The annealing temperature is 300°C ± 10°C, and the annealing time is 8 hours.

[0072] S9, insulation, after cooling, the outside of the rare earth aluminum alloy conductor is extruded with a cross-linked polyethylene material for insulation;

[0073] S10, cabling and sheathing: Place 4 insulated cores on a cabling machine for filling. After filling, wrap them with glass fiber tape and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with polyethylene material to form a cable.

[0074] Example 2

[0075] A rare earth aluminum alloy high-strength, high-conductivity, high-stability cable comprises an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in mass percentage: rare earth 3%, rhenium 1.0%, copper 1.2%, yttrium 0.6%, cobalt 0.8%, nickel 0.3%, silicon carbide 0.1%, aluminum chloride 0.6%, the total content of impurity elements ≤0.1%, and the balance is aluminum.

[0076] The mass percentage of cerium in the rare earth elements is 1.0%, the mass percentage of holmium is 0.7%, the mass percentage of dysprosium is 0.7%, and the mass percentage of europium is 0.6%.

[0077] The method for preparing a rare earth aluminum alloy high-strength, high-conductivity and high-stability cable comprises the following steps:

[0078] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition.

[0079] S2, melting the aluminum ingot, placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid.

[0080] The purity of aluminum ingot is not less than 99.8% and the melting temperature is 780℃.

[0081] S3, grinding, putting silicon carbide, aluminum chloride, nano-graphene and nano-aluminum powder into a ball mill for grinding and mixing to obtain a mixed powder; using an electromagnetic induction furnace to melt the mixed powder, using argon gas for protection during the melting process, cooling after the melting is completed, and obtaining an aluminum-based composite material.

[0082] The addition amount of nano-graphene is 0.3%, the grinding time is 30 minutes, the particle size after grinding is powdery, and the melting temperature of the mixed powder is 780°C.

[0083] S4. Add the raw materials and aluminum-based composite materials into aluminum liquid, add a grain refiner into the aluminum liquid, add oxidized red sand powder into the aluminum liquid for smelting, refining and degassing, melt evenly and keep warm to obtain rare earth aluminum alloy liquid.

[0084] The grain refiner is Al-5Ti-B refiner, and the mass percentage of the grain refiner is 0.8%.

[0085] S5. Casting: casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars.

[0086] S6. Rolling: rolling the rare earth aluminum alloy strip through a rolling mill to form a Φ9.0 mm rare earth aluminum alloy rod.

[0087] S7. Drawing: Use a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical rare earth aluminum alloy monofilament, and use a special-shaped wire stranding die on a frame-type stranding machine to strand the rare earth aluminum alloy monofilament into a rare earth aluminum alloy conductor.

[0088] S8, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing.

[0089] The annealing temperature is 300°C ± 10°C, and the annealing time is 7 hours.

[0090] S9, insulation, after cooling, the outside of the rare earth aluminum alloy conductor is extruded with a cross-linked polyethylene material for insulation;

[0091] S10, cabling and sheathing: Place 4 insulated cores on a cabling machine for filling. After filling, wrap them with glass fiber tape and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with polyethylene material to form a cable.

[0092] Example 3

[0093] A rare earth aluminum alloy high-strength, high-conductivity, high-stability cable comprises an aluminum alloy monofilament, wherein the aluminum alloy monofilament comprises the following components in mass percentage: rare earth 4.0%, rhenium 1.2%, copper 1.4%, yttrium 0.5%, cobalt 0.9%, nickel 0.2%, silicon carbide 0.2%, aluminum chloride 0.5%, the total content of impurity elements ≤0.1%, and the balance is aluminum.

[0094] The mass percentage of cerium in the rare earth elements is 1.5%, the mass percentage of holmium is 1.0%, the mass percentage of dysprosium is 0.7%, and the mass percentage of europium is 0.8%.

[0095] The method for preparing a rare earth aluminum alloy high-strength, high-conductivity and high-stability cable comprises the following steps:

[0096] S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition.

[0097] S2, melting the aluminum ingot, placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid.

[0098] The purity of aluminum ingot is not less than 99.8% and the melting temperature is 800℃.

[0099] S3, grinding, putting silicon carbide, aluminum chloride, nano-graphene and nano-aluminum powder into a ball mill for grinding and mixing to obtain a mixed powder; using an electromagnetic induction furnace to melt the mixed powder, using argon gas for protection during the melting process, cooling after the melting is completed, and obtaining an aluminum-based composite material.

[0100] The addition amount of nano-graphene is 0.1%, the grinding time is 30 minutes, the particle size after grinding is powdery, and the melting temperature of the mixed powder is 750°C.

[0101] S4. Add the raw materials and aluminum-based composite materials into aluminum liquid, add a grain refiner into the aluminum liquid, add oxidized red sand powder into the aluminum liquid for smelting, refining and degassing, melt evenly and keep warm to obtain rare earth aluminum alloy liquid.

[0102] The grain refiner is Al-5Ti-B refiner, and the mass percentage of the grain refiner is 1%.

[0103] S5. Casting: casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars.

[0104] S6. Rolling: rolling the rare earth aluminum alloy strip through a rolling mill to form a Φ9.0 mm rare earth aluminum alloy rod.

[0105] S7. Drawing: Use a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical rare earth aluminum alloy monofilament, and use a special-shaped wire stranding die on a frame-type stranding machine to strand the rare earth aluminum alloy monofilament into a rare earth aluminum alloy conductor.

[0106] S8, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing.

[0107] The annealing temperature is 300°C ± 10°C, and the annealing time is 9 hours.

[0108] S9, insulation, after cooling, the outside of the rare earth aluminum alloy conductor is extruded with a cross-linked polyethylene material for insulation;

[0109] S10, cabling and sheathing: Place 4 insulated cores on a cabling machine for filling. After filling, wrap them with glass fiber tape and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with polyethylene material to form a cable.

[0110] The properties of the rare earth aluminum alloy monofilaments prepared in Examples 1-3 were tested, and the test results are shown in Table 1.

[0111] Table 1 Properties of rare earth aluminum alloy monofilaments prepared in Examples 1-3

[0112] project Example 1 Example 2 Example 3 Elongation(%) 31% 34% 33% <![CDATA[Tensile strength (N / mm 2 )]]> 224 238 195 90° bending times 35 40 38 DC resistivity at 20℃(Ω / m) 0.0268 0.0263 0.0270 Electrical conductivity (%IACS) 64 65 64

[0113] The cable bending radius obtained in Examples 1-3 is 7D-10D, the cable rebound performance is reduced by 40% compared with copper cables, the creep resistance is increased by 380% compared with aluminum core cables, and the service life is not less than 45 years, which improves the service life and creep resistance of the cable and has very good high temperature stability.

[0114] Therefore, the use of the rare earth aluminum alloy high-strength, high-conductivity, high-stability cable and the preparation method thereof described in the present invention can solve the problems of low tensile strength, low conductivity and poor creep resistance of existing aluminum alloy cables.

[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A rare earth aluminum alloy high-strength, high-conductivity, high-stability cable, characterized by: Including aluminum alloy monofilament, the aluminum alloy monofilament includes the following components in mass percentage: rare earth 2.0%-4.1%, rhenium 1.0%-1.2%, copper 0.8%-1.5%, yttrium 0.5%-0.8%, cobalt 0.5%-1.0%, nickel 0.2%-0.5%, silicon carbide 0.05%-0.3%, aluminum chloride 0.1%-0.8%, the total content of impurity elements ≤0.1%, and the balance is aluminum.

2. The rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to claim 1, characterized in that: The rare earth element is a mixture of cerium, holmium, dysprosium and europium, wherein the mass percentage of cerium is 0.8%-1.5%, the mass percentage of holmium is 0.3%-1.0%, the mass percentage of dysprosium is 0.2%-0.8%, and the mass percentage of europium is 0.2%-0.8%.

3. The rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to claim 1, characterized in that: It includes an aluminum alloy conductor, which is made of twisted aluminum alloy monofilaments. An insulating layer is arranged on the outside of the aluminum alloy conductor. A plurality of aluminum alloy conductors are wrapped with glass fiber tapes on the outside. A filling layer is arranged between the glass fiber tapes and the insulating layer. An inner sheath layer is arranged on the outside of the glass fiber tapes. An outer sheath layer is arranged on the outside of the inner sheath layer. An armor layer is arranged between the inner sheath layer and the outer sheath layer.

4. The rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to claim 1, characterized in that: The insulating layer is a cross-linked polyethylene layer, the armor layer is a galvanized steel belt layer, and the outer sheath layer is a cross-linked polyethylene layer.

5. A method for preparing a rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Prepare materials: weigh and prepare the raw materials according to the set chemical composition; S2, melting the aluminum ingot, placing the aluminum ingot into a melting furnace for melting, and keeping the temperature after melting to obtain aluminum liquid; S3, grinding, putting silicon carbide, aluminum chloride, nano-graphene, and nano-aluminum powder into a ball mill for grinding and mixing to obtain a mixed powder; using an electromagnetic induction furnace to melt the mixed powder, using argon gas for protection during the melting process, and cooling after the melting is completed to obtain an aluminum-based composite material; S4, adding the raw materials and the aluminum-based composite material into aluminum liquid, adding a grain refiner into the aluminum liquid, adding oxidized red sand powder into the aluminum liquid for smelting, refining and degassing, melting evenly and then keeping warm to obtain rare earth aluminum alloy liquid; S5, casting, casting the rare earth aluminum alloy liquid into rare earth aluminum alloy bars; S6, rolling, rolling the rare earth aluminum alloy strip through a rolling mill to form a rare earth aluminum alloy rod with a diameter of Φ9.0 mm; S7, drawing, using a 13-die wire drawing machine to draw the rare earth aluminum alloy rod into an elliptical rare earth aluminum alloy monofilament, and twisting the rare earth aluminum alloy monofilament into a rare earth aluminum alloy conductor on a frame-type stranding machine using a special-shaped stranding die; S8, annealing, placing the rare earth aluminum alloy conductor into an annealing furnace for annealing; S9, insulation, after cooling, the outside of the rare earth aluminum alloy conductor is extruded with a cross-linked polyethylene material for insulation; S10, Cabling and sheathing: Place 3-4 insulated cores on a cabling machine for filling. After filling, wrap them with glass fiber tape and extrude the inner sheath layer. After extruding the inner sheath layer, use galvanized steel tape armor, and then extrude the outer sheath layer with polyethylene material to form a cable.

6. The method for preparing a rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to claim 5, characterized in that: In the S2, the purity of the aluminum ingot is not less than 99.8%, and the melting temperature is 750°C-800°C.

7. The method for preparing a rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to claim 5, characterized in that: In the S3, the addition amount of nanographene is 0.02%-0.8%, the grinding time is 30 minutes, and the melting temperature of the mixed powder is 750°C-800°C.

8. The method for preparing a rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to claim 5, characterized in that: In the S4, the grain refiner is Al-5Ti-B refiner, and the mass percentage of the grain refiner is 0.5%-1%.

9. The method for preparing a rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to claim 5, characterized in that: In the S8, the annealing temperature is 300°C±10°C, and the annealing time is 6 hours to 9 hours.

10. A method for preparing a rare earth aluminum alloy high-strength, high-conductivity, high-stability cable according to any one of claims 6 to 9, characterized in that: The elongation of the prepared rare earth aluminum alloy monofilament is ≥30%, and the tensile strength is 180N / mm 2 -240N / mm 2 , 90° bending times more than 30 times, DC resistivity ≤0.0270Ω / m at 20℃, conductivity 64%-65%, bending radius 7D-10D, compared with copper cable, its rebound performance is reduced by 40%, compared with aluminum core cable, its creep resistance is increased by 380%, and its service life is not less than 45 years.

Citation Information

Patent Citations

  • Al-Fe-Co-RE aluminum alloy, and preparation method and power cable thereof

    CN102978461A

  • Cable aluminum alloy wire stock and preparation method thereof

    CN102994818A

  • Rare earth aluminum alloy power cable and production technology thereof

    CN103474153A

  • Rare earth high-iron aluminum alloy cable conductor and manufacturing method thereof

    CN104008786A

  • Aluminum alloy material and preparation method thereof

    CN104388763A

Cited By

  • Rare earth aluminum alloy flat wire and preparation method and application thereof

    CN122511669A

  • A rare earth aluminum alloy flat wire, a preparation method and application thereof

    CN122511669B