Anti-cracking wear-resistant cable and preparation method thereof

Chemical adsorption of vinyl triethoxysilane with carbon powder in the cable, grinding of polypropylene/carbon composites and melt electrospinning, electron beam irradiation and electrodeposition and thermal pressure of Ag-MoS2 layers in the cable The problem of cracking and wear resistance of cables in high or low temperature environments has been solved, and the cable performance has been significantly improved.

CN118942775AInactive Publication Date: 2024-11-12WUHAN ZHENZANTUO BUILDING MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410995186.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing cables are prone to cracking in high or low temperature environments, resulting in power transmission or signal interruption, and lack of wear resistance and cannot meet production needs.

Method used

Using crack-resistant and wear-resistant cable design including cable blanks, fiber membranes and Ag-MoS2 layers, through chemical adsorption of vinyl triethoxysilane and carbon powder, grinding of polypropylene/carbon composite materials and melt static electricity Spinning, electron beam irradiation treatment, and electrodeposition and hot pressing treatment of Ag-MoS2 layers enhance the cracking and wear resistance of the cable.

Benefits of technology

It significantly improves the wear resistance and crack resistance of the cable, extends the service life of the cable, and expands its application range.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an anti-cracking wear-resistant cable and a preparation method thereof, and relates to the technical field of cables. Vinyltriethoxysilane and carbon powder are subjected to primary grinding and then subjected to secondary grinding with polypropylene powder, polypropylene and carbon powder are combined through external mechanical force and a modifier, the strength of polypropylene is greatly improved, the wear resistance and cracking resistance of a cable are indirectly improved, then melt-blown electrostatic spinning is performed on a cable blank, and the wear resistance and cracking resistance of the cable are improved. A polypropylene / carbon fiber film is formed on the surface of a cable green body, then electron beam irradiation treatment is performed, so that an insulating layer in the cable green body and the polypropylene / carbon fiber film are adhered and crosslinked, interlayer acting force is enhanced, carbon powder and a polypropylene base material are promoted to be further combined, the performance of the cable is improved, and then an Ag-MoS2 layer is electrically deposited on the surface of the fiber film, so that the performance of the cable is improved. And hot pressing treatment is carried out, so that the wear resistance and the cracking resistance of the cable are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cables, and in particular to a crack-resistant and wear-resistant cable and a preparation method thereof. Background Art

[0002] With the rapid development of economy, cables are widely used in the fields of communication and electricity. When cables are used in high or low temperature environments, they will still crack in different occasions after being cabled. In severe cases, it will lead to the interruption of power transmission or signal transmission of cables. Although the cracking performance of materials can be improved by cross-linking, due to the constraints of cable standards, production processes and costs, the complete cross-linking method is not practical and universal. In addition, the existing cables cannot meet the needs of production operations in terms of wear resistance. In actual use, cables with better performance and more complete functions are needed. Summary of the invention

[0003] The object of the present invention is to provide a crack-resistant and wear-resistant cable and a preparation method thereof, so as to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a crack-resistant and wear-resistant cable, wherein the crack-resistant and wear-resistant cable comprises a cable body, a fiber membrane layer, and an Ag-MoS2 layer.

[0005] Furthermore, the cable blank includes a cable core and an insulation layer.

[0006] Furthermore, the cable core is copper wire.

[0007] Furthermore, the insulating layer is a polyethylene insulating layer.

[0008] Furthermore, the preparation method of the fiber membrane layer is: heating the carbon powder to 60-80°C, adding vinyl triethoxysilane in an amount of 0.01-0.1 times the mass of the carbon powder, grinding at 500-1000rpm for 40-60min, and then adding polypropylene particles in an amount of 10-100 times the mass of the carbon powder, and continuing grinding for 24h to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin in a mass ratio of 2-3:7-8, and after completely melting, starting melt electrospinning to the cable blank, spinning until the membrane thickness is 20-40μm, drying at room temperature for 4-6h, and then performing electron beam irradiation treatment.

[0009] Furthermore, the melt electrospinning has the following characteristics: the spinning distance is 4-8 cm, the spinning voltage is 10-30 kV, the cable blank rotation speed is 50-100 rpm, and the spinning temperature is 260°C.

[0010] Furthermore, the melt flow index of the melt-blown polypropylene resin is 1800 g / min.

[0011] Furthermore, the electron beam irradiation treatment: the energy of the electrons is 1.0 to 1.3 MeV, the electron beam current is 10 to 18 mA, the line speed of the cable is 40 to 50 m / min, and the irradiation cross-linking is performed 1 to 3 times.

[0012] Furthermore, the preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 2 to 3.5 A / dm 2 The film was deposited for 30 minutes and then hot pressed at 120-140°C and a pressure of 10 MPa for 5 minutes.

[0013] Furthermore, the electrolyte is: 270 g / L silver nitrate, 35 g / L boric acid, 0.1 g / L sodium dodecyl sulfate, 28 g / L MoS2, and the rest is deionized water.

[0014] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0015] The present invention firstly performs primary grinding with vinyl triethoxysilane and carbon powder, wherein the vinyl triethoxysilane and the carbon powder undergo chemical adsorption, which can promote the close combination of the carbon powder and the polypropylene matrix, and is more conducive to the transmission of stress; then, polypropylene powder is added for secondary grinding, and the polypropylene and the carbon powder are combined by external mechanical force, thereby greatly improving the strength of the polypropylene, and indirectly improving the wear resistance and cracking resistance of the cable; then, melt-spraying electrostatic spinning is performed on the cable blank to form a polypropylene / carbon fiber film on the surface of the cable blank; and then, electron beam irradiation treatment is performed to make the insulating layer in the cable blank adhere to and cross-link the polypropylene / carbon fiber film, thereby strengthening the interlayer force and promoting the further combination of the carbon powder and the polypropylene base material, which is conducive to improving the performance of the cable; then, an Ag-MoS2 layer is electro-deposited on the surface of the fiber film to form a double lubricating phase, and hot pressing treatment is performed to make the interlayer structure dense and smooth, thereby improving the wear resistance of the cable; and at the same time, the Ag-MoS2 layer can be used as a hard layer to improve the cracking resistance of the cable. The present invention improves the performance of the cable by combining material optimization and production process optimization, especially significantly enhancing the wear resistance and crack resistance of the cable, thereby expanding the application range of the cable. DETAILED DESCRIPTION

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe the method in detail. The test methods for various indicators of the cables prepared in the following examples are as follows:

[0018] Wear resistance: Take the embodiment and comparative example with the same mass to test the wear resistance effect. The cable surface is polished with 800-mesh sandpaper (polishing frequency 10 times / min) for 30 hours, and then the mass difference before and after polishing is calculated Δm = (cable weight before polishing - cable weight after polishing) / cable weight before polishing × 100%.

[0019] Example 1

[0020] A crack-resistant and wear-resistant cable, comprising a cable blank, a fiber membrane layer, and an Ag-MoS2 layer;

[0021] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0022] The preparation method of the fiber membrane layer is as follows: heating carbon powder to 60°C, adding vinyl triethoxysilane with a mass of 0.01 times that of the carbon powder, grinding at 500rpm for 60min, then adding polypropylene particles with a mass of 10 times that of the carbon powder, and continuing grinding for 24h to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin at a mass ratio of 2:8, and after completely melting, starting to perform melt electrostatic spinning on a cable blank: the spinning distance is 4cm, the spinning voltage is 10kV, the cable blank rotation speed is 50rpm, the spinning temperature is 260°C, spinning to a film thickness of 20μm, drying at room temperature for 4h, and then performing electron beam irradiation treatment: the electron energy is 1.0Mev, the electron beam current is 10mA, the cable linear speed is 40m / min, and irradiation crosslinking is performed once;

[0023] The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 2A / dm 2 The electrolyte was: 270 g / L silver nitrate, 35 g / L boric acid, 0.1 g / L sodium dodecyl sulfate, 28 g / L MoS2, and the rest was deionized water.

[0024] Example 2

[0025] A crack-resistant and wear-resistant cable, comprising a cable blank, a fiber membrane layer, and an Ag-MoS2 layer;

[0026] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0027] The preparation method of the fiber membrane layer is as follows: heating carbon powder to 70°C, adding vinyl triethoxysilane in an amount of 0.05 times the mass of the carbon powder, grinding at 800rpm for 50min, then adding polypropylene particles in an amount of 70 times the mass of the carbon powder, and continuing grinding for 24h to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin in a mass ratio of 3:7, and after completely melting, starting to perform melt electrostatic spinning on a cable blank: the spinning distance is 6cm, the spinning voltage is 20kV, the cable blank rotation speed is 80rpm, the spinning temperature is 260°C, spinning to a film thickness of 30μm, drying at room temperature for 5h, and then performing electron beam irradiation treatment: the electron energy is 1.1Mev, the electron beam current is 14mA, the cable linear speed is 45m / min, and irradiation cross-linking is performed twice;

[0028] The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 3A / dm 2 The electrolyte was deposited at 130 °C for 30 min and then hot pressed at 10 MPa for 5 min. The electrolyte was: silver nitrate 270 g / L, boric acid 35 g / L, sodium dodecyl sulfate 0.1 g / L, MoS2 28 g / L, and the rest was deionized water.

[0029] Example 3

[0030] A crack-resistant and wear-resistant cable, comprising a cable blank, a fiber membrane layer, and an Ag-MoS2 layer;

[0031] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0032] The preparation method of the fiber membrane layer is as follows: heating carbon powder to 80° C., adding vinyl triethoxysilane in an amount of 0.1 times the mass of the carbon powder, grinding at 1000 rpm for 40 min, then adding polypropylene particles in an amount of 100 times the mass of the carbon powder, and continuing grinding for 24 h to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin in a mass ratio of 3:7, and after completely melting, starting to perform melt electrostatic spinning on a cable blank: the spinning distance is 8 cm, the spinning voltage is 30 kV, the cable blank rotation speed is 100 rpm, the spinning temperature is 260° C., spinning to a film thickness of 40 μm, drying at room temperature for 6 h, and then performing electron beam irradiation treatment: the electron energy is 1.3 MeV, the electron beam current is 18 mA, the cable linear speed is 50 m / min, and irradiation cross-linking is performed 3 times;

[0033] The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 3.5A / dm 2The electrolyte was deposited at 140 °C for 30 min and then hot pressed at 10 MPa for 5 min. The electrolyte was: silver nitrate 270 g / L, boric acid 35 g / L, sodium dodecyl sulfate 0.1 g / L, MoS2 28 g / L, and the rest was deionized water.

[0034] Comparative Example 1

[0035] A crack-resistant and wear-resistant cable, comprising a cable blank, a fiber membrane layer, and an Ag-MoS2 layer;

[0036] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0037] The preparation method of the fiber membrane layer is as follows: carbon powder, polypropylene particles and melt-blown polypropylene resin are mixed in a mass ratio of 0.1:3:7, and after they are completely melted, melt electrostatic spinning is started to the cable blank: the spinning distance is 6 cm, the spinning voltage is 20 kV, the cable blank rotation speed is 80 rpm, the spinning temperature is 260° C., spinning to a film thickness of 30 μm, drying at room temperature for 5 hours, and then electron beam irradiation treatment is performed: the energy of the electrons is 1.1 MeV, the electron beam current is 14 mA, the cable linear speed is 45 m / min, and irradiation cross-linking is performed twice;

[0038] The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 3A / dm 2 The electrolyte was deposited at 130 °C for 30 min and then hot pressed at 10 MPa for 5 min. The electrolyte was: silver nitrate 270 g / L, boric acid 35 g / L, sodium dodecyl sulfate 0.1 g / L, MoS2 28 g / L, and the rest was deionized water.

[0039] Comparative Example 2

[0040] A crack-resistant and wear-resistant cable, comprising a cable blank, a fiber membrane layer, and an Ag-MoS2 layer;

[0041] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0042] The preparation method of the fiber membrane layer is as follows: heating carbon powder to 70° C., adding vinyl triethoxysilane in an amount of 0.05 times the mass of the carbon powder, grinding at 800 rpm for 50 min, then adding polypropylene particles in an amount of 70 times the mass of the carbon powder, and continuing grinding for 24 h to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin in a mass ratio of 3:7, and after completely melting, starting melt electrostatic spinning to a cable blank: the spinning distance is 6 cm, the spinning voltage is 20 kV, the cable blank rotation speed is 80 rpm, the spinning temperature is 260° C., spinning to a membrane layer thickness of 30 μm, and drying at room temperature for 5 h;

[0043] The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 3A / dm 2 The electrolyte was deposited at 130 °C for 30 min and then hot pressed at 10 MPa for 5 min. The electrolyte was: silver nitrate 270 g / L, boric acid 35 g / L, sodium dodecyl sulfate 0.1 g / L, MoS2 28 g / L, and the rest was deionized water.

[0044] Comparative Example 3

[0045] A crack-resistant and wear-resistant cable, comprising a cable blank, and an Ag-MoS2 layer;

[0046] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0047] The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 3A / dm 2 The electrolyte was deposited at 130 °C for 30 min and then hot pressed at 10 MPa for 5 min. The electrolyte was: silver nitrate 270 g / L, boric acid 35 g / L, sodium dodecyl sulfate 0.1 g / L, MoS2 28 g / L, and the rest was deionized water.

[0048] Comparative Example 4

[0049] A crack-resistant and wear-resistant cable, comprising a cable blank, a fiber membrane layer, and a MoS2 layer;

[0050] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0051] The preparation method of the fiber membrane layer is as follows: heating carbon powder to 70°C, adding vinyl triethoxysilane in an amount of 0.05 times the mass of the carbon powder, grinding at 800rpm for 50min, then adding polypropylene particles in an amount of 70 times the mass of the carbon powder, and continuing grinding for 24h to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin in a mass ratio of 3:7, and after completely melting, starting to perform melt electrostatic spinning on a cable blank: the spinning distance is 6cm, the spinning voltage is 20kV, the cable blank rotation speed is 80rpm, the spinning temperature is 260°C, spinning to a film thickness of 30μm, drying at room temperature for 5h, and then performing electron beam irradiation treatment: the electron energy is 1.1Mev, the electron beam current is 14mA, the cable linear speed is 45m / min, and irradiation cross-linking is performed twice;

[0052] The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 3A / dm 2 The electrolyte was deposited at 130 °C for 30 min and then hot pressed at 10 MPa for 5 min. The electrolyte was: boric acid 35 g / L, sodium dodecyl sulfate 0.1 g / L, MoS2 28 g / L, and the rest was deionized water.

[0053] Comparative Example 5

[0054] A crack-resistant and wear-resistant cable, comprising a cable blank, a fiber membrane layer, and an Ag layer;

[0055] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0056] The preparation method of the fiber membrane layer is as follows: heating carbon powder to 70°C, adding vinyl triethoxysilane in an amount of 0.05 times the mass of the carbon powder, grinding at 800rpm for 50min, then adding polypropylene particles in an amount of 70 times the mass of the carbon powder, and continuing grinding for 24h to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin in a mass ratio of 3:7, and after completely melting, starting to perform melt electrostatic spinning on a cable blank: the spinning distance is 6cm, the spinning voltage is 20kV, the cable blank rotation speed is 80rpm, the spinning temperature is 260°C, spinning to a film thickness of 30μm, drying at room temperature for 5h, and then performing electron beam irradiation treatment: the electron energy is 1.1Mev, the electron beam current is 14mA, the cable linear speed is 45m / min, and irradiation cross-linking is performed twice;

[0057] The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 3A / dm 2The electrolyte was deposited at 130°C for 30 minutes and then hot-pressed at a pressure of 10 MPa for 5 minutes. The electrolyte was: 270 g / L silver nitrate, 35 g / L boric acid, 0.1 g / L sodium dodecyl sulfate, and the rest was deionized water.

[0058] Comparative Example 6

[0059] A crack-resistant and wear-resistant cable, comprising a cable blank and a fiber membrane layer;

[0060] The cable blank comprises a cable core and an insulating layer, wherein the cable core is a copper wire and the insulating layer is a polyethylene insulating layer;

[0061] The preparation method of the fiber membrane layer is as follows: heating carbon powder to 70°C, adding vinyl triethoxysilane in an amount of 0.05 times the mass of the carbon powder, grinding at 800rpm for 50min, adding polypropylene particles in an amount of 70 times the mass of the carbon powder, and continuing grinding for 24h to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin in a mass ratio of 3:7, and after completely melting, starting melt electrostatic spinning to a cable blank: the spinning distance is 6cm, the spinning voltage is 20kV, the cable blank rotation speed is 80rpm, the spinning temperature is 260°C, spinning to a membrane layer thickness of 30μm, drying at room temperature for 5h, and then performing electron beam irradiation treatment: the electron energy is 1.1Mev, the electron beam current is 14mA, the cable linear speed is 45m / min, and irradiation cross-linking is performed twice.

[0062] Effect example

[0063] Table 1 below shows the performance analysis results of the cables using Examples 1 to 3 of the present invention and Comparative Examples 1 to 6.

[0064] Table 1

[0065] Quality difference (%) -40℃ low temperature shock 150℃×1h thermal shock Example 1 0.02 No cracks No cracks Example 2 0.01 No cracks No cracks Example 3 0.01 No cracks No cracks Comparative Example 1 0.05 No cracks No cracks Comparative Example 2 0.12 No cracks No cracks Comparative Example 3 0.16 No cracks No cracks Comparative Example 4 0.18 No cracks No cracks Comparative Example 5 0.28 No cracks No cracks Comparative Example 6 0.30 No cracks No cracks

[0066] From the comparison of the experimental data of the embodiment and the comparative example, it can be found that the present invention first uses vinyl triethoxysilane and carbon powder for initial grinding, and vinyl triethoxysilane and carbon powder undergo chemical adsorption, which can promote the close combination of carbon powder and polypropylene matrix, and is more conducive to the transmission of stress. Then, polypropylene powder is added for secondary grinding. Through the action of external mechanical force, polypropylene and carbon powder are combined, which greatly improves the strength of polypropylene, and indirectly improves the wear resistance and cracking resistance of the cable. Then, melt-blown electrostatic spinning is performed on the cable blank to form a polypropylene / carbon fiber film on the surface of the cable blank, and then electron beam irradiation treatment is performed to make the insulating layer in the cable blank adhere to and cross-link the polypropylene / carbon fiber film, strengthen the interlayer force, and promote the further combination of carbon powder and polypropylene base material, which is beneficial to improving the performance of the cable. Then, an Ag-MoS2 layer is electro-deposited on the surface of the fiber membrane to form a double lubricating phase, and hot pressing treatment is performed to make the interlayer structure dense and smooth, improve the wear resistance of the cable, and at the same time, the Ag-MoS2 layer can be used as a hard layer to improve the cracking resistance of the cable. The present invention achieves improved performance of the cable by combining material optimization and production process optimization, especially significantly enhancing the wear resistance and crack resistance of the cable, thereby expanding the application range of the cable.

[0067] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A crack-resistant and wear-resistant cable, characterized in that: The crack-resistant and wear-resistant cable comprises a cable body, a fiber membrane layer and an Ag-MoS2 layer.

2. The anti-cracking and wear-resistant cable according to claim 1, characterized in that: The cable blank comprises a cable core and an insulating layer.

3. The anti-cracking and wear-resistant cable according to claim 2, characterized in that: The cable core is copper wire.

4. The anti-cracking and wear-resistant cable according to claim 2, characterized in that: The insulating layer is a polyethylene insulating layer.

5. The anti-cracking and wear-resistant cable according to claim 1, characterized in that: The preparation method of the fiber membrane layer is as follows: heating carbon powder to 60-80° C., adding vinyl triethoxysilane in an amount of 0.01-0.1 times the mass of the carbon powder, grinding at 500-1000 rpm for 40-60 min, adding polypropylene particles in an amount of 10-100 times the mass of the carbon powder, and continuing grinding for 24 hours to obtain a polypropylene / carbon composite material, mixing the polypropylene / carbon composite material and melt-blown polypropylene resin in a mass ratio of 2-3:7-8, and starting melt electrostatic spinning on a cable blank after they are completely melted, spinning until the membrane layer has a thickness of 20-40 μm, drying at room temperature for 4-6 hours, and then performing electron beam irradiation treatment.

6. The anti-cracking and wear-resistant cable according to claim 5, characterized in that: The melt electrostatic spinning has the following characteristics: the spinning distance is 4-8 cm, the spinning voltage is 10-30 kV, the cable blank rotation speed is 50-100 rpm, and the spinning temperature is 260°C.

7. The anti-cracking and wear-resistant cable according to claim 5, characterized in that: The melt flow index of the melt-blown polypropylene resin is 1800 g / min.

8. The anti-cracking and wear-resistant cable according to claim 5, characterized in that: The electron beam irradiation treatment comprises: the electron energy is 1.0 to 1.3 MeV, the electron beam current is 10 to 18 mA, the line speed of the cable is 40 to 50 m / min, and the irradiation cross-linking is performed 1 to 3 times.

9. The anti-cracking and wear-resistant cable according to claim 1, characterized in that: The preparation method of the Ag-MoS2 layer is as follows: using the fiber membrane layer cable as the working electrode and the platinum electrode as the anode, placing the electrolyte in the electrolytic cell with a current density of 2 to 3.5 A / dm 2 The film was deposited for 30 minutes and then hot pressed at 120-140°C and a pressure of 10 MPa for 5 minutes.

10. The anti-cracking and wear-resistant cable according to claim 9, characterized in that: The electrolyte is: 270 g / L silver nitrate, 35 g / L boric acid, 0.1 g / L sodium dodecyl sulfate, 28 g / L MoS2, and the rest is deionized water.

Citation Information

Cited By

  • Urban underground corrosion-resistant and wear-resistant power cable

    CN121601306A