Miniature solid-state supercapacitor of patterned electrode and preparation method of miniature solid-state supercapacitor
By using a patterned electrode and current collector layer with fractal structure in the supercapacitor, combining carboxylated multi-walled carbon nanotubes and polyaniline active electrodes, and dilute phosphoric acid polyvinyl alcohol gel electrolyte, the insufficient interface area of the electrode-electrolyte is solved. The problem of high performance and flexibility has been improved, and is suitable for high performance and micro electronic devices.
Patent Information
- Application Number
- CN202411204705.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
The limited electrode-electrolyte interface area of existing planar structure supercapacitors limits their applications in high-performance demand scenarios and lacks flexibility and all-solid state characteristics.
Using a patterned electrode with a fractal structure and a current collector layer, a mixture of carboxylated multi-walled carbon nanotubes and polyaniline is prepared by screen printing, and a solid gel electrolyte made of dilute phosphoric acid and polyvinyl alcohol is achieved. Increase in the contact area of the electrode-electrolyte and improve electrochemical performance.
It significantly improves the specific capacitance and electrochemical performance of supercapacitors, is suitable for high-performance application scenarios, and has flexible and all-solid state characteristics, suitable for integration in micro-flexible electronic devices.
Smart Images

Figure CN118942918A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of supercapacitors, and in particular relates to a micro solid-state supercapacitor with patterned electrodes and a preparation method thereof. Background Art
[0002] In recent years, with the widespread application and development of wearable electronic devices, flexible energy storage devices have gradually become a research hotspot. Among them, supercapacitors have become electrochemical energy storage devices with great development prospects due to their advantages such as long cycle life, fast charging and discharging speed, and large storage capacity. According to the different structures of supercapacitors, they can be divided into sandwich structures and planar structures. Compared with traditional sandwich structure supercapacitors, planar structure supercapacitors no longer require diaphragms, achieving a lower gap between electrodes. By reducing the distance between the electrodes, the resistance of ion transmission can be reduced, allowing electrolyte ions to be quickly and efficiently transferred in small gaps, thereby producing excellent power density. However, since the capacitance of planar structure supercapacitors is highly dependent on the electrode-electrolyte interface area, the electrode-electrolyte interface area of existing planar structure supercapacitors is limited, which affects the electrochemical performance and limits its application in some scenarios with higher performance requirements. Summary of the invention
[0003] The object of the present invention is to provide a micro solid-state supercapacitor with patterned electrodes and a preparation method thereof, so that the microcapacitor has good flexibility and all-solid-state characteristics, as well as excellent electrochemical performance.
[0004] To achieve the above object, the present invention adopts the following technical solution:
[0005] A micro solid-state supercapacitor with a patterned electrode comprises a flexible substrate, a current collector layer, a patterned electrode layer and a gel electrolyte layer stacked in sequence from bottom to top; the current collector layer is a patterned conductive silver paste made by a screen printing process, and the patterned electrode layer is a mixture of carboxylated multi-walled carbon nanotubes and polyaniline, and is a patterned active electrode made by a screen printing process; the patterns of the current collector layer and the patterned electrode layer both adopt a fractal structure, and the patterns of the two are overlapped and aligned.
[0006] Furthermore, the flexible substrate layer is a polyimide (PI) layer, which has many advantages such as high temperature stability, electrical insulation performance, and chemical stability.
[0007] Furthermore, the gel electrolyte layer is a solid gel dielectric layer made of dilute phosphoric acid and polyvinyl alcohol (PVA).
[0008] A method for preparing a micro solid-state supercapacitor with a patterned electrode comprises the following steps:
[0009] Step 1: prepare a flexible substrate layer using polyimide; select a fractal structure as a pattern to draw a screen printing screen; prepare a gel electrolyte solution, and configure an active electrode material;
[0010] Step 2: Using the screen printing screen obtained in step 1, a conductive silver paste is printed on a flexible substrate by a screen printing process, and after printing, the conductive silver paste is placed in a drying oven for drying to complete the preparation of the current collector layer;
[0011] Step 3, placing the screen printing plate obtained in step 1 above the current collector layer, and aligning the pattern with the current collector layer pattern, then printing the active electrode material on the current collector layer using a screen printing process, and drying it naturally at room temperature after printing, thereby completing the preparation of the patterned electrode layer;
[0012] Step 4: evenly coat the gel electrolyte on the patterned electrode layer and dry it, repeat this operation several times, and then place it at room temperature for 12h-15h to complete the preparation of the solid gel electrolyte layer;
[0013] Step 5: Use wires to lead out the positive and negative electrodes of the supercapacitor to obtain a micro solid-state supercapacitor with patterned electrodes.
[0014] Furthermore, the preparation method of the gel electrolyte solution is:
[0015] Polyvinyl alcohol (PVA) powder was added to a 1 mol / L phosphoric acid solution in a mass ratio of 1:0.98. The solution was stirred at 300 rpm at 85°C until the solution became clear. The solution was then placed at room temperature for 12 hours to remove bubbles, thereby obtaining a PVA / H3PO4 gel electrolyte solution.
[0016] Furthermore, the configuration method of the active electrode material is:
[0017] (1) dissolving thermoplastic polyurethane elastomer (TPU) particles in N-methylpyrrolidone (NMP) with a mass ratio of TPU to NMP being 1:11, stirring at a temperature of 50° C. and a speed of 400 rpm for 1 h to mix the mixture evenly, thereby obtaining a first mixed solution;
[0018] (2) adding carboxylated multi-walled carbon nanotubes (MWCNT-COOH) of the same mass as TPU to the first mixed solution, stirring at a speed of 400 rpm for 1 hour and ultrasonically treating for 15 minutes, so that the MWCNT-COOH is fully dispersed in the first mixed solution, to obtain a second mixed solution;
[0019] (3) grinding polyaniline (PANI) and camphorsulfonic acid (CSA) in a mortar at a mass ratio of 1:3 to obtain a first mixture, wherein the mass percentage of PANI in the active material is 10 wt %;
[0020] (4) adding the first mixture to the second mixed solution, stirring at 400 rpm for 1 h and ultrasonically treating for 15 min to fully disperse the PANI, thereby obtaining a third mixed solution;
[0021] (5) Adding polyvinylidene fluoride (PVDF) and acetylene black (AB) to the third mixed solution at a mass ratio of active material: polyvinylidene fluoride: acetylene black of 8:1:1, stirring at a speed of 400 rpm for 1 hour, a mixed ink of carboxylated multi-walled carbon nanotubes and polyaniline as active electrode materials can be obtained.
[0022] Furthermore, the drying temperature for preparing the current collector layer in step 2 is 150° C., and the drying time is 15 min; the single drying temperature for preparing the gel electrolyte layer in step 4 is 40° C., and the drying time is 15 min.
[0023] The present invention provides a micro solid-state supercapacitor with a patterned electrode and a preparation method thereof. On the basis of the existing planar structure supercapacitor, a fractal structure is introduced into the current collector layer and the active electrode layer for pattern design, and the patterns of the two overlap and align. The designed fractal structure patterned electrode increases the electrode-electrolyte contact area, enhances the absorption of electrolyte ions, and obtains a larger specific capacitance; the active electrode material made of a mixture of carboxylated multi-walled carbon nanotubes and polyaniline is used, so that it has the advantages of excellent reversibility and cycle stability of double-layer capacitors and high energy density of pseudocapacitors, greatly improving the performance of supercapacitors.
[0024] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:
[0025] 1. The patterned electrode structure proposed in the present invention has better electrochemical performance than the traditional interdigitated electrode structure and is suitable for application scenarios with high performance requirements.
[0026] 2. The supercapacitor proposed in the present invention has an independent structure, does not require additional packaging, has a small device size and a thin thickness, and can be integrated into micro-flexible electronic devices.
[0027] 3. The supercapacitor proposed in the present invention has high flexibility and all-solid-state characteristics, and the preparation method is simple. It has great application prospects in the fields of flexible electronic products and wearable electronic products. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of the structure of a micro solid-state supercapacitor with patterned electrodes of the present invention;
[0029] Figure 2 This is a cyclic voltammetry curve test diagram of Example 1 of the present invention;
[0030] Figure 3 This is a constant current charge and discharge curve test diagram of Example 1 of the present invention;
[0031] The descriptions of the symbols in the accompanying drawings are as follows:
[0032] 1-flexible substrate layer, 2-current collector layer, 3-patterned active electrode layer, 4-gel electrolyte layer. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0034] like Figure 1 As shown, a micro solid-state supercapacitor with a patterned electrode provided in this embodiment includes a flexible substrate, a current collector layer, a patterned electrode layer and a gel electrolyte layer stacked in sequence from bottom to top.
[0035] The flexible substrate is a polyimide layer with a thickness of 0.2 mm; it has many advantages such as high temperature stability, electrical insulation performance, and chemical stability.
[0036] The current collector layer is a patterned conductive silver paste made by screen technology, the conductive silver paste is imported silver paste-8301, and the resistance value is 25 milliohms. The patterned electrode layer is a mixture of carboxylated multi-walled carbon nanotubes and polyaniline, and the patterned active electrode is made by screen printing technology. The active material is carboxylated multi-walled carbon nanotubes and polyaniline, wherein the mass percentage of polyaniline is 10wt%, and the carboxylated multi-walled carbon nanotubes used have a diameter of 3-15nm and a length of 15-30μm; the overall size of the patterned electrode is 31*31mm, and the electrode gap is 1mm. The patterns of the current collector layer and the patterned electrode layer both adopt Sierpinski fractal structure, and the patterns of the two overlap and align. In this embodiment, the graphic structure of the collector layer and the patterned electrode layer can also adopt more complex electrical geometric shapes. The gel electrolyte layer is a solid gel dielectric layer made of dilute phosphoric acid and polyvinyl alcohol (PVA).
[0037] In view of the above structure, this embodiment also provides a method for preparing a micro solid-state supercapacitor with a patterned electrode, comprising the following steps:
[0038] Step 1: Use polyimide to prepare a flexible substrate layer; select a Sierpinski fractal structure as a pattern to draw a silk screen, prepare a gel electrolyte solution, and configure an active electrode material.
[0039] In this embodiment, the preparation method of the gel electrolyte solution is:
[0040] Take 6 g of polyvinyl alcohol (PVA) powder and add it to 60 mL of 1 mol / L phosphoric acid solution. Stir it at 300 rpm at 85 °C until the solution becomes clear. Then let it stand at room temperature for 12 h to remove bubbles, and obtain a PVA / H3PO4 gel electrolyte solution.
[0041] The active electrode material of this embodiment is a mixed ink of carboxylated multi-walled carbon nanotubes and polyaniline, and its preparation method includes the following steps:
[0042] (1) dissolving 600 g of thermoplastic polyurethane elastomer (TPU) particles in 6500 mg of N-methylpyrrolidone (NMP), stirring at 400 rpm for 1 h at 50° C. to mix uniformly, thereby obtaining a first mixed solution;
[0043] (2) adding 600 mg of carboxylated multi-walled carbon nanotubes (MWCNT-COOH) to the first mixed solution, stirring at 400 rpm for 1 h and ultrasonically treating for 15 min, so that the MWCNT-COOH is fully dispersed in the first mixed solution, to obtain a second mixed solution;
[0044] (3) 66.67 mg of polyaniline (PANI) and 200 mg of camphorsulfonic acid (CSA) were put into a mortar and ground for 15 min to obtain a first mixture;
[0045] (4) adding the first mixture to the second mixed solution, stirring at 400 rpm for 1 h and ultrasonically treating for 15 min to fully disperse the PANI, thereby obtaining a third mixed solution;
[0046] (5) 83.33 mg of polyvinylidene fluoride (PVDF) and 83.33 mg of acetylene black (AB) were added to the third mixed solution and stirred at 400 rpm for 1 h to obtain a mixed ink of carboxylated multi-walled carbon nanotubes and polyaniline as active electrode materials.
[0047] Step 2: Use the screen printing screen obtained in step 1 to print the conductive silver paste on the flexible substrate using a screen printing process. After printing, place it in a drying oven and bake it at 150° C. for 15 minutes to complete the preparation of the current collector layer.
[0048] Step 3, placing the screen printing plate obtained in step 1 above the current collector layer, and aligning the pattern with the current collector layer pattern, then printing the active electrode material on the current collector layer using a screen printing process, and drying it naturally at room temperature after printing, thereby completing the preparation of the patterned electrode layer;
[0049] Step 4: evenly coat the gel electrolyte on the patterned electrode layer and dry it in a drying oven at 40° C. for 15 min; repeat this operation several times, and then place it at room temperature for 12 h to complete the preparation of the solid gel electrolyte layer;
[0050] Step 5: Use wires to lead out the positive and negative electrodes of the supercapacitor to obtain a micro solid-state supercapacitor with patterned electrodes.
[0051] The micro solid-state supercapacitor with a patterned electrode prepared in this embodiment was measured using an electrochemical workstation for easy measurement. Before the measurement, the positive and negative ends of the patterned electrode were led out through wires to perform the following performance tests:
[0052] Cyclic voltammetry test:
[0053] Cyclic voltammetry can effectively reflect the double-layer capacitance behavior and pseudocapacitance behavior to characterize supercapacitors and determine the reversibility of capacitance behavior. Under room temperature, place the micro solid-state supercapacitor to be measured on the test platform, and set the starting voltage and ending voltage to 0V and 1V respectively. Then, the real-time voltage and current curves of the supercapacitor can be observed on the electrochemical workstation. Figure 2 As shown, the measured cyclic voltammetry curve is a relatively symmetrical closed loop shape, indicating that the supercapacitor has strong reversibility. According to the measured cyclic voltammetry curve, the specific area capacitance of the supercapacitor can be obtained by the following formula. The specific area capacitance calculated at a scan rate of 10mV / s is the largest, and its value is 115.43mF / cm 2 .
[0054]
[0055] Where C is the total capacitance, K is the scan rate, ΔV is the set scan voltage difference, I(V) is the current density function, A is the area of the capacitor, and C A is the specific area capacitance.
[0056] Constant current charge and discharge curve:
[0057] In this embodiment, a square wave current is applied in the electrochemical test, and the change of electrode potential over time is measured to analyze the performance of the device. Under room temperature, the micro solid-state supercapacitor to be measured is placed on the test platform, and the maximum potential value is set to 1V. The capacitor is discharged first and then charged, and then the voltage change of the supercapacitor is observed in real time on the electrochemical workstation. Figure 3 As shown, the supercapacitor is charged relatively steadily at the beginning, and when it reaches the maximum potential, it discharges steadily after a rapid voltage drop.
[0058] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A micro solid-state supercapacitor with patterned electrodes, characterized in that: It includes a flexible substrate, a current collector layer, a patterned electrode layer and a gel electrolyte layer stacked in sequence from bottom to top; the current collector layer is a patterned conductive silver paste made by screen printing technology, and the patterned electrode layer is a mixture of carboxylated multi-walled carbon nanotubes and polyaniline, and is a patterned active electrode made by screen printing technology; the patterns of the current collector layer and the patterned electrode layer both adopt fractal structures, and the patterns of the two are overlapped and aligned.
2. The micro solid-state supercapacitor with patterned electrodes according to claim 1, characterized in that: The flexible base layer is a polyimide layer.
3. The micro solid-state supercapacitor with patterned electrodes according to claim 2, characterized in that: The gel electrolyte layer is a solid gel dielectric layer made of dilute phosphoric acid and polyvinyl alcohol (PVA).
4. The method for preparing a micro solid-state supercapacitor with a patterned electrode according to claim 3, characterized in that: The following steps are involved: Step 1: prepare a flexible base layer using polyimide; select a fractal structure as a pattern to draw a silk screen; Preparation of gel electrolyte solution and configuration of active electrode materials; Step 2: Using the screen printing screen obtained in step 1, a conductive silver paste is printed on a flexible substrate by a screen printing process, and after printing, the conductive silver paste is placed in a drying oven for drying to complete the preparation of the current collector layer; Step 3, placing the screen printing plate obtained in step 1 above the current collector layer, and aligning the pattern with the current collector layer pattern, then printing the active electrode material on the current collector layer using a screen printing process, and drying it naturally at room temperature after printing, thereby completing the preparation of the patterned electrode layer; Step 4: evenly coat the gel electrolyte on the patterned electrode layer and dry it, repeat this operation several times, and then place it at room temperature for 12h-15h to complete the preparation of the solid gel electrolyte layer; Step 5: Use wires to lead out the positive and negative electrodes of the supercapacitor to obtain a micro solid-state supercapacitor with patterned electrodes.
5. The method for preparing a micro solid-state supercapacitor with a patterned electrode according to claim 4, characterized in that: The preparation method of the gel electrolyte solution is: Polyvinyl alcohol (PVA) powder was added to a 1 mol / L phosphoric acid solution in a mass ratio of 1:0.
98. The solution was stirred at 300 rpm at 85°C until the solution became clear. The solution was then placed at room temperature for 12 hours to remove bubbles, thereby obtaining a PVA / H3PO4 gel electrolyte solution.
6. The method for preparing a micro solid-state supercapacitor with a patterned electrode according to claim 4, characterized in that: The configuration method of the active electrode material is: (1) dissolving thermoplastic polyurethane elastomer (TPU) particles in N-methylpyrrolidone (NMP) with a mass ratio of TPU to NMP being 1:11, stirring at a temperature of 50° C. and a speed of 400 rpm for 1 h to mix the mixture evenly, thereby obtaining a first mixed solution; (2) adding carboxylated multi-walled carbon nanotubes (MWCNT-COOH) of the same mass as TPU to the first mixed solution, stirring at a speed of 400 rpm for 1 hour and ultrasonically treating for 15 minutes, so that the MWCNT-COOH is fully dispersed in the first mixed solution, to obtain a second mixed solution; (3) grinding polyaniline (PANI) and camphorsulfonic acid (CSA) in a mortar at a mass ratio of 1:3 to obtain a first mixture, wherein the mass percentage of PANI in the active material is 10 wt %; (4) adding the first mixture to the second mixed solution, stirring at 400 rpm for 1 h and ultrasonically treating for 15 min to fully disperse the PANI, thereby obtaining a third mixed solution; (5) Adding polyvinylidene fluoride (PVDF) and acetylene black (AB) to the third mixed solution at a mass ratio of active material: polyvinylidene fluoride: acetylene black of 8:1:1, stirring at a speed of 400 rpm for 1 hour, a mixed ink of carboxylated multi-walled carbon nanotubes and polyaniline as active electrode materials can be obtained.
7. The method for preparing a micro solid-state supercapacitor with a patterned electrode according to claim 4, characterized in that: The drying temperature for preparing the flow device layer in step 2 is 150° C. and the drying time is 15 min. The single drying temperature for preparing the gel electrolyte layer in step 4 is 40° C. and the drying time is 15 min.