Semiconductor epitaxial structure, HEMT device and preparation method of semiconductor epitaxial structure
By setting high and low conductivity doped regions in the semiconductor epitaxial structure of HEMT devices, the problem of difficult to take into account both contact resistance and epitaxial quality in the prior art is solved, and higher device performance and stability are achieved.
Patent Information
- Application Number
- CN202410954427.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art sacrifices the epitaxial quality of the device when reducing the contact resistance of HEMT devices, making it difficult to simultaneously reduce the electrode on-resistance and ensure the epitaxial quality.
By setting electrode regions with different conductivity in the semiconductor epitaxial structure, the first doping region with high conductivity is connected to the two-dimensional electronic gas, thereby reducing the resistivity of the overall electrode region, while using the second doping region with low conductivity is used. Reduce leakage, thereby balancing the quality of the epitaxial layer.
It achieves the reduction of on-resistance while ensuring epitaxial quality, improving the performance and stability of the device.
Smart Images

Figure CN118943162A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure generally relates to the field of semiconductor technology. More specifically, the present disclosure relates to a semiconductor epitaxial structure, a HEMT device, and a method for preparing the semiconductor epitaxial structure. Background Art
[0002] As a representative of the third generation of semiconductor materials, gallium nitride (GaN) has many excellent properties, including high critical breakdown electric field, high electron mobility, high two-dimensional electron gas concentration, and good high-temperature working ability. Third generation semiconductor devices based on GaN, such as high electron mobility transistors (HEMTs) and heterojunction field effect transistors (HFETs), have been applied, especially in the fields of radio frequency and microwaves that require high power and high frequency.
[0003] One of the key factors to achieve high performance of HEMT devices is to reduce contact resistance. However, the existing technology sacrifices the epitaxial quality of the device in order to reduce contact resistance. Therefore, how to ensure epitaxial quality while reducing contact resistance has become a technical problem that needs to be solved urgently. Summary of the invention
[0004] In order to solve some or all of the above problems, the present disclosure provides a semiconductor epitaxial structure, a HEMT device and a method for preparing a semiconductor epitaxial structure, which can reduce the conductive resistance of the electrode while ensuring the epitaxial quality and improving the stability of the device.
[0005] According to a first aspect of the present disclosure, a semiconductor epitaxial structure is provided, comprising: a substrate; a compound semiconductor composite structure arranged on the substrate, the compound semiconductor composite structure comprising a first semiconductor layer and a second semiconductor layer arranged on the first semiconductor layer, and the first semiconductor layer and the second semiconductor layer form a heterojunction having a two-dimensional electron gas; two electrode regions arranged on opposite sides of the compound semiconductor composite structure, the electrode regions extending from the first semiconductor layer to a side of the compound semiconductor composite structure away from the substrate; the electrode regions comprising a first doped region close to the compound semiconductor composite structure and a second doped region away from the compound semiconductor composite structure along a direction from the substrate to the compound semiconductor composite structure, the first doped region being located between the second doped region and the compound semiconductor composite structure, and the conductivity of the first doped region being greater than the conductivity of the second doped region.
[0006] According to a second aspect of the present disclosure, a HEMT device is provided, comprising: a substrate; a compound semiconductor composite structure disposed on the substrate, the compound semiconductor composite structure comprising a first semiconductor layer and a second semiconductor layer disposed on the first semiconductor layer, and the first semiconductor layer and the second semiconductor layer form a heterojunction having a two-dimensional electron gas; two electrode regions disposed on opposite sides of the compound semiconductor composite structure, the electrode regions extending from the first semiconductor layer to a side of the compound semiconductor composite structure away from the substrate; a drain and a source, respectively disposed on the two electrode regions; a gate, disposed on the compound semiconductor composite structure and disposed between the source and the drain; the electrode region, along a direction from the substrate to the compound semiconductor composite structure, comprising a first doped region close to the compound semiconductor composite structure and a second doped region away from the compound semiconductor composite structure, the first doped region being located between the second doped region and the compound semiconductor composite structure, and the conductivity of the first doped region being greater than the conductivity of the second doped region.
[0007] According to a third aspect of the present disclosure, a method for preparing a semiconductor structure is provided, comprising: providing a substrate; forming a prefabricated first semiconductor layer on the substrate; forming a prefabricated second semiconductor layer on the prefabricated first semiconductor layer, and the prefabricated first semiconductor layer and the prefabricated second semiconductor layer form a heterojunction with a two-dimensional electron gas to form a prefabricated compound semiconductor composite structure; forming a first groove in electrode regions on opposite sides of the prefabricated compound semiconductor composite structure to form a compound semiconductor composite structure with the first groove on opposite sides; forming an electrode region in the first groove, the electrode region extending from the first semiconductor layer to a side of the compound semiconductor composite structure away from the substrate; the electrode region, along the direction from the substrate to the compound semiconductor composite structure, comprises a first doped region close to the compound semiconductor composite structure and a second doped region away from the compound semiconductor composite structure, the first doped region is located between the second doped region and the compound semiconductor composite structure, and the conductivity of the first doped region is greater than the conductivity of the second doped region.
[0008] In the semiconductor epitaxial structure, HEMT device and method for preparing the semiconductor epitaxial structure provided in the embodiments of the present disclosure, by setting regions of different conductivity in two relative electrode regions, especially setting a region of higher conductivity in the region where the two-dimensional electron gas is connected, the on-resistance is reduced while the leakage of the entire electrode region is reduced to the greatest extent, thereby reducing the on-resistance while ensuring the quality of the epitaxy, thereby improving the performance of the device prepared using the epitaxial structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0010] Figure 1 A schematic diagram of a semiconductor epitaxial structure provided in some embodiments of the present disclosure;
[0011] Figure 2 A schematic diagram of another semiconductor epitaxial structure provided in some embodiments of the present disclosure;
[0012] Figure 3 A schematic diagram of another semiconductor epitaxial structure provided in some embodiments of the present disclosure;
[0013] Figure 4 A schematic diagram of another semiconductor epitaxial structure provided in some embodiments of the present disclosure;
[0014] Figure 5 A schematic diagram of another semiconductor epitaxial structure provided for some embodiments of the present disclosure;
[0015] Figure 6 A schematic diagram of a HEMT device provided in some embodiments of the present disclosure;
[0016] Figure 7 A schematic diagram of another HEMT device provided in some embodiments of the present disclosure;
[0017] Figure 8 A flow chart of a method for preparing a semiconductor epitaxial structure provided in some embodiments of the present disclosure;
[0018] Figure 9a-9f A structural schematic diagram corresponding to a method for preparing a semiconductor epitaxial structure provided in some embodiments of the present disclosure;
[0019] Figure 10a-Figure 10b A structural schematic diagram corresponding to a method for preparing a semiconductor epitaxial structure provided in some other embodiments of the present disclosure.
[0020] Description of reference numerals:
[0021] Semiconductor epitaxial structure 10, HEMT device 100, substrate 1, compound semiconductor composite structure 2, first semiconductor layer 21, second semiconductor layer 22, two-dimensional electron gas 20, first surface 201, second surface 202, sidewall 203, electrode region 3, first electrode region 31, second electrode region 32, first doping region 301, second doping region 302, first doping portion 3021, second doping portion 3022, third doping region 302, nucleation layer 4, buffer layer 5, source 310, drain 320, gate 330, gate metal 3301, P-type nitride layer 3302, prefabricated compound semiconductor composite structure 2', prefabricated first semiconductor layer 21', prefabricated second semiconductor layer 22', first trench 3', second trench 302', prefabricated first doping region 301'. DETAILED DESCRIPTION
[0022] The present disclosure will be further described below in conjunction with the accompanying drawings.
[0023] In the description of this application, "preparation" refers to preparing a layer structure with certain requirements on the material to be processed. The technology involved in "preparation" may include physical vapor deposition technology (PVD) commonly used in chip manufacturing, such as electron beam evaporation (E-Gun Evaporation / Electron Beam Evaporation), chemical vapor deposition technology (Chemical Vapor Deposition), and organic chemical vapor deposition technology (MOCVD) commonly used for epitaxial growth, liquid phase epitaxy technology (LPE), vapor phase epitaxy technology (VPE), molecular beam epitaxy technology (MBE), atomic layer deposition technology (ALD), etc. For ordinary technicians in this field, appropriate preparation technology can be selected according to actual conditions.
[0024] In the description of this application, "etching" should be understood in a broad sense, that is, a layer of photoresist is grown on the surface of the material to be processed, the photoresist is selectively exposed and developed through a mask to leave a photoresist layer identical to the mask pattern on the surface of the material to be processed, and then the material to be processed is selectively corroded by chemical or physical methods, and finally the photoresist layer is stripped off to form a structure corresponding to the mask pattern on the material to be processed.
[0025] In the description of the present application, the orientation or positional relationship indicated by "upper" or "lower" etc. is based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing the present disclosure and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present disclosure.
[0026] In the description of this application, except for the first embodiment, the other embodiments are written in a way that avoids duplication as much as possible, that is, the key points are recorded as to the differences between each embodiment and other embodiments. In these embodiments, if any technical features are not clearly recorded, refer to the corresponding description of the first embodiment.
[0027] The specific embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.
[0028] For example, please refer to Figure 1 , a semiconductor epitaxial structure 10, comprising:
[0029] A substrate 1; a compound semiconductor composite structure 2 arranged on the substrate 1, the compound semiconductor composite structure 2 comprising a first semiconductor layer and a second semiconductor layer 22 arranged on the first semiconductor layer 21, wherein the first semiconductor layer 21 and the second semiconductor layer 22 form a heterojunction having a two-dimensional electron gas 20; two electrode regions 3 arranged on opposite sides of the compound semiconductor composite structure 2, the electrode regions 3 extending from the inside of the first semiconductor layer 21 to a side of the compound semiconductor composite structure 2 away from the substrate; the electrode regions 3, along the direction from the substrate 1 to the compound semiconductor composite structure 2, comprising a first doping region 301 close to the compound semiconductor composite structure 2 and a second doping region 302 away from the compound semiconductor composite structure 2, the first doping region 301 being located between the second doping region 302 and the compound semiconductor composite structure 2, and the conductivity of the first doping region 301 being greater than the conductivity of the second doping region 302.
[0030] The substrate 110 may be one of various substrates such as a silicon substrate, a silicon carbide substrate, a gallium nitride substrate, a sapphire, a germanium substrate, a SOI (Semiconductor On Insulator, a semiconductor on an insulator, such as silicon on an insulator, germanium on an insulator, or silicon germanium on an insulator) substrate. Those skilled in the art will appreciate that the substrate is not subject to any limitation, but may be selected according to practical applications. Specifically, in this embodiment, a silicon substrate is taken as an example for explanation, and the Si substrate is not limited to high resistance or low resistance, nor is it limited to N-type or P-type.
[0031] The compound semiconductor composite structure 2 here includes: a Group III nitride composite structure, wherein the Group III nitride can be a nitride prepared from wide bandgap semiconductor materials such as gallium nitride (GaN) and aluminum nitride (AlN). Specifically, the nitride layer of this embodiment is illustrated using GaN as an example.
[0032] Exemplarily, the first semiconductor layer 21 in the compound semiconductor composite structure 2 may be a trench layer, and the second semiconductor layer 22 in the compound semiconductor composite structure 2 may be a barrier layer. Exemplarily, the material of the barrier layer may include alloy nitrides, in particular aluminum gallium nitride (AlGaN). Generally, the thickness of the barrier layer is in the range of 5nm-50nm ("nm" means nanometers), for example, 5nm, 25nm or 50nm. Of course, there are different thickness ranges according to different device requirements, and no limitation is made here; the material of the channel layer may include III-V nitrides. It is known that when the material of the trench layer includes III-V nitrides and the material of the barrier layer includes alloy nitrides, due to the large difference in polarization intensity and bandgap width between the two, a two-dimensional electron gas (2DEG) heterojunction is formed at the interface between the two.
[0033] It should be added that, in some embodiments, please refer to Figure 2 , between the substrate 1 and the compound semiconductor composite structure 2, a nucleation layer 4 and a buffer layer 5 are sequentially arranged along the direction from the substrate 1 to the compound semiconductor composite structure 2. The nucleation layer 4 can be formed of aluminum carbide (AIN) or gallium nitride (GaN), with a thickness of 10nm-500nm, which is used to improve the growth quality of the buffer layer 5 and has an isolation effect. The buffer layer 5 can be formed of iron-doped gallium nitride, carbon-doped gallium nitride, gallium nitride (GaN) or aluminum gallium nitride (AlGaN), with a thickness of 100nm-10um, which is used to improve the growth quality of III-V group nitrides (or the compound semiconductor composite structure here). The buffer layer 5 can be a one-layer or multi-layer structure. There is no limitation here.
[0034] Here, the electrode region 3 is a region located in the semiconductor composite structure 2 to assist the electrode metal in electrically coupling the two-dimensional electron gas 20 to conduct the device. The electrode regions 3 correspond to the source and drain of the device respectively. It can be understood that the two electrode regions 3 include a first electrode region 31 and a second electrode region 32; the first electrode region 31 is the source region, and the second electrode region 32 is the drain region; or, the first electrode region 31 is the drain region, and the second electrode region 32 is the source region. The following is an example in which the first electrode region 31 is the source region and the second electrode region 32 is the drain region.
[0035] The material of the electrode region may be gallium nitride (GaN), or indium gallium nitride (InGaN), or indium aluminum gallium nitride (InAlGaN), etc. Any material that can be used to form the electrode region is acceptable, and no limitation is made herein.
[0036] Here, the electrode region 3 extends from the inside of the first semiconductor layer 21 to the side of the compound semiconductor composite structure 2 away from the substrate 1. It can be understood that, in some embodiments, the electrode region 3 may extend from the side of the compound semiconductor composite structure 2 away from the substrate 1 to the substrate 1 into the first semiconductor layer 21, or, the electrode region 3 extends from the side of the compound semiconductor composite structure 2 away from the substrate 1 to below the two-dimensional electron gas 20, or, the electrode region 3 extends from below the two-dimensional electron gas 20 to be flush with the surface of the compound semiconductor composite structure 2. The electrode region 3 extends from the inside of the first semiconductor layer 21 to the side of the compound semiconductor composite structure 2 away from the substrate 1. It can also be understood that, in other embodiments, the electrode region 3 extends from below the two-dimensional electron gas 20 beyond the surface of the compound semiconductor composite structure 2. The electrode region 3 extends from the inside of the first semiconductor layer 21 to the side of the compound semiconductor composite structure 2 away from the substrate 1. It can also be understood that, in other embodiments, the electrode region 3 extends from below the two-dimensional electron gas 20 and is lower than the surface of the compound semiconductor composite structure 2. Here, whether the electrode region 3 exceeds or is below or is flush with the surface of the compound semiconductor composite structure 2 can be determined according to actual device requirements and process steps, and does not affect the electrical effect of the electrode region 3 in this embodiment.
[0037] Please continue reading Figure 1 , along the direction from the substrate 1 to the compound semiconductor composite structure 2, that is, along the AA' direction, the electrode region 3 includes a first doping region 301 close to the compound semiconductor composite structure 2 or close to the substrate 1, and a second doping region 302 far away from the compound semiconductor composite structure 2 or far away from the substrate 1, the first doping region 301 is located between the second doping region 302 and the compound semiconductor composite structure 2, and the conductivity of the first doping region 301 is greater than the conductivity of the second doping region 302.
[0038] It should be noted that in the prior art, in order to reduce the contact resistance of the source and drain and improve the conductivity of the device, the source region and the drain region are usually prepared with highly doped materials, that is, materials with higher conductivity. However, the higher the doping concentration, the higher the defects of the material. As the defects increase, there will be many energy gaps in the material to capture normal carriers, resulting in increased leakage and high surface roughness, thereby affecting the quality of the epitaxial layer and the performance of the device. In this embodiment, the electrode region 3 is set as a first doping region 301 and a second doping region 302 of different conductivity, thereby reducing the problem of poor epitaxial quality caused by all high conductivity, and at the same time reducing the problem of large contact resistance of the source and drain caused by all low conductivity. Therefore, in this embodiment, by designing the electrode region 3 as at least a first doping region 301 with high conductivity and a second doping region 302 with low conductivity, it is possible to simultaneously reduce the source and drain contact resistance while ensuring the epitaxial quality of the semiconductor epitaxial structure, thereby improving the performance of the device prepared using the epitaxial structure.
[0039] In some embodiments, please refer to Figure 1 or Figure 2 , the electrode region 3 has a conductive doping medium of the first conductivity type, and when the conductive doping medium of the first doping region 301 and the second doping region 302 are the same, the doping concentration of the conductive doping medium of the first doping region 301 is greater than the doping concentration of the conductive doping medium of the second doping region 302. It can be understood that when the conductive doping medium is the same, the higher the doping concentration, the higher the conductivity.
[0040] It should be noted that doping can be achieved through a variety of techniques, including diffusion and ion implantation. The diffusion method usually involves exposing the semiconductor material to an environment containing a doping source and driving the impurity atoms into the semiconductor crystal at high temperature, while ion implantation uses accelerated impurity atoms to directly bombard the semiconductor surface, followed by annealing to repair possible lattice damage and activate the doping atoms.
[0041] Here, the first conductivity type may be N-type. If the first conductivity type is N-type, the compound semiconductor composite structure may be, for example, a composite structure formed by an AlGaN layer and a GaN layer. In other embodiments, the first conductivity type may be P-type. If the first conductivity type is P-type, the compound semiconductor composite structure may be, for example, a composite structure formed by an InGaN layer and a GaN layer. It should be understood that the addition of the conductive doping medium of the first conductivity type here can reduce the resistivity of the compound semiconductor composite structure itself.
[0042] In other embodiments, the electrode region 3 may also be an N-type or P-type electrode region. For example, the conductivity type of the first doping region 301 may be N-type, and the conductivity type of the second doping region 302 may be P-type, or a combination of P-type and N-type regions. As long as the conductivity of the first doping region 301 is greater than the conductivity of the second doping region 302, no limitation is made here.
[0043] It should be added that, when the first conductivity type is N-type, the conductive doping medium can be silicon (Si), or germanium (Ge), etc. Of course, any single element or a mixture of multiple elements that can form an N-type conductive material can be used, and no limitation is made here. When the first conductivity type is P-type, the conductive doping medium can be magnesium (Mg), or zinc (Zn), etc. Of course, any single element or a mixture of multiple elements that can form a P-type conductive material can be used, and no limitation is made here. The following embodiments are described below taking the first conductivity type as N-type as an example.
[0044] It should be noted that the conductive doping medium is different, and the higher the electron attraction of the conductive doping medium, the lower the doping concentration of the conductive doping medium can be under the same conductivity. It can be understood that the electron attraction of Si is higher than that of germanium (Ge), and under the same conductivity, the concentration of doped silicon (Si) is lower than that of doped germanium (Ge). Therefore, different conductive doping media can be doped according to needs, and it is only necessary to ensure that the conductivity of the first doping region 301 is higher than that of the second doping region 302.
[0045] In some embodiments, please refer to Figure 1 or Figure 2 The conductive doping medium is a first conductive doping medium, and the doping concentration of the first doping region 301 is 1×10 19 ~1×10 20 cm3, the doping concentration of the second doping region is 1×10 17 ~1×10 19 cm3; and / or, the conductive doping medium is a second conductive doping medium, and the doping concentration of the first doping region is 1×10 19 ~5×10 20 cm3, the doping concentration of the second doping region is 1×10 17 ~5×10 19 cm3; wherein the electron attraction of the first conductive doping medium is greater than the electron attraction of the second conductive doping medium. The first conductive doping medium here may be silicon (Si), and the second conductive doping medium here may be germanium (Ge).
[0046] See also Figure 3 ,like Figure 3As shown, the first doping region 301 extends from the side of the two-dimensional electron gas 20 close to the substrate 1 to the side of the compound semiconductor composite structure 2 far from the substrate 1, and the first doping region 301 is connected to the two-dimensional electron gas 20. In this way, since the first doping region 301 with higher conductivity is directly connected to the two-dimensional electron gas 20, that is, the two can be electrically coupled, the overall resistivity of the electrode region can be greatly reduced, thereby reducing the contact resistance of the source and drain. At the same time, due to the low conductivity or low doping concentration of the second doping region, the leakage of the epitaxial layer outside the two-dimensional electron device is further reduced, and the quality of the epitaxial layer is balanced. Therefore, in this embodiment, by designing the first doping region 301 to be connected to the two-dimensional electron gas 20, the contact resistance can be effectively reduced while ensuring the epitaxial quality of the semiconductor epitaxial structure, thereby improving the performance of the device prepared by the epitaxial structure.
[0047] In some other embodiments, see Figure 4 The compound semiconductor composite structure 2 includes a first surface 201 and a second surface 202 relative to each other, and a sidewall 203 connecting the first surface 201 and the second surface 202; the first doped region 301 is located between the substrate 1 and the two-dimensional electron gas 20, and the semiconductor epitaxial structure 10 also includes: a third doped region 303, the third doped region 303 intersects with the second doped region 302 and is connected to the sidewall 203 corresponding to the compound semiconductor composite structure 2.
[0048] It is understandable that the thickness of the barrier layer is between 5nm and 50nm, especially when it is 5nm, since the barrier layer is relatively thin, the etching process may not be controlled to be etched exactly to the two-dimensional electron gas 20, so in many cases, the etching will be below the two-dimensional electron gas 20, therefore, in order to enable the high conductivity region to be electrically connected to the two-dimensional electron gas 20, it can be set at the side wall 203 of the compound semiconductor composite structure 2. In this way, the contact resistance of the electrode can be effectively reduced, and since the second doping region 302 is also included, the epitaxial quality of the semiconductor epitaxial structure can be effectively balanced.
[0049] In some embodiments, please refer to Figure 4 ,like Figure 4 As shown, the first thickness of the first doping region 301 is greater than the second thickness of the third doping region 303, the first thickness direction is the direction from the substrate 1 to the compound semiconductor composite structure 2, that is, the AA' direction mentioned above, and the second thickness direction is the arrangement direction of the two electrode regions 3. It should be noted that in practical applications, if the first doping region 301, the second doping region 302 and the third doping region 303 are all grown by a growth process, since the sidewall growth rate will be lower than the bottom growth rate, therefore, the first thickness of the first doping region 301 will be thicker than the second thickness of the third doping region 302.
[0050] Of course, in other embodiments, when other preparation processes are used, the first thickness of the first doped region 301 may also be the same as the second thickness of the third doped region 303 to facilitate subsequent preparation processes and better ensure the epitaxial quality and device performance of the semiconductor epitaxial structure.
[0051] Please refer to any Figure 1-Figure 4 The first thickness of the electrode region 3 is 10-100 nm, the first thickness of the first doping region 301 is less than or equal to 10 nm, and the first thickness direction is the direction from the substrate 1 to the compound semiconductor composite structure 2, that is, the AA' direction mentioned above.
[0052] Exemplarily, the first thickness of the electrode region 3 may be 10 nm, 50 nm or 100 nm. Exemplarily, when the electrode region 3 is 100 nm, the first thickness of the first doping region 301 is less than or equal to 1 / 5 of the first thickness of the electrode region 3 .
[0053] In this way, the thickness difference between the first doping region 301 and the second doping region 302 can effectively balance the reduction of contact resistance and the improvement of epitaxial quality of the semiconductor epitaxial structure, thereby effectively improving the performance of the device manufactured using the semiconductor epitaxial structure 10 .
[0054] In some embodiments, see Figure 5 ,like Figure 5 As shown, the second doping region 302 includes a first doping portion 3021 and a second doping portion 3022; the first doping portion 3021 and the second doping portion 3022 are arranged along the direction from the substrate 1 to the compound semiconductor composite structure 2, and the conductivity of the first doping portion 3021 is less than that of the second doping portion 3022. It can be understood that the first doping portion 3022 is the side away from the substrate and is in contact with the electrode metal. Since the first doping portion 3022 has a higher conductivity, the ohmic contact resistance of the electrode metal can be effectively reduced, thereby reducing the contact resistance of the entire electrode region. However, due to the low conductivity design of the first doping portion, the epitaxial quality of the semiconductor epitaxial structure of the entire electrode region can be effectively balanced, and leakage in other regions of the electrode region can be reduced; therefore, by further dividing the second doping region into multiple conductivity zones, the contact resistance can be further reduced while ensuring the epitaxial quality of the semiconductor epitaxial structure, thereby improving the performance of the device prepared by the semiconductor epitaxial structure.
[0055] Exemplarily, the conductivity type of the first doping region 301 may be N-type, the conductivity type of the first doping portion 3021 may be N-type, and the conductivity type of the third doping portion 3022 may be P-type, as long as the conductivity of the first doping portion 3021 is less than the conductivity of the second doping portion 3022. Exemplarily, the first doping region 301 may be N-type InGaN, the first doping portion 3021 may be N-type GaN, and the second doping portion may be P-type InGaN. The material combination of each region of the electrode region is not limited here, as long as the conductivity of the first doping portion 3021 is less than the conductivity of the second doping portion 3022, and the conductivity of the first doping region 301 is greater than the conductivity of the second doping region 302.
[0056] Of course, in some other embodiments, the electrode region 3 may include the first doping region 301 , the first doping portion 3021 and the second doping portion 3022 , and the third doping region 303 .
[0057] It is known that the above embodiments can be implemented individually or in any combination, and no limitation is made here.
[0058] In some embodiments, when the conductive doping medium of the first doping portion 3021 and the second doping portion 3022 are the same, the doping concentration of the conductive doping medium of the first doping portion 3021 is greater than the doping concentration of the conductive doping medium of the second doping portion 3022 .
[0059] It should be noted that the conductive doping medium is different, and the higher the electron attraction of the conductive doping medium, the lower the doping concentration of the conductive doping medium can be under the same conductivity. It can be understood that the electron attraction of silicon (Si) is higher than that of germanium (Ge), and under the same conductivity, the concentration of doped silicon (Si) is lower than that of doped germanium (Ge). Therefore, different conductive doping media can be doped according to needs, and it is only necessary to ensure that the conductivity of the first doping part 3021 is higher than that of the second doping part 3022.
[0060] In some embodiments, please refer to Figure 5 The conductive doping medium is a first conductive doping medium, and the doping concentration of the first doping part 3021 is 1×10 19 ~1×10 20 cm3, the doping concentration of the second doping part is 1×10 17 ~1×10 19 cm3; and / or, the conductive doping medium is a second conductive doping medium, and the doping concentration of the first doping part 3021 is 1×10 19 ~5×10 20 cm3, the doping concentration of the second doping part is 1×10 17 ~5×1019 cm3; wherein the electron attraction of the first conductive doping medium is greater than the electron attraction of the second conductive doping medium. The first conductive doping medium here may be silicon (Si), and the second conductive doping medium here may be germanium (Ge).
[0061] In some embodiments, the first thickness of the electrode region 3 is 10-100nm, the first thickness of the first doping region 301 is less than or equal to 10nm, and the first thickness of the second doping portion 3022 is less than or equal to 10nm. The first thickness direction is the direction from the substrate 1 to the compound semiconductor composite structure 2, that is, the AA' direction mentioned above.
[0062] Exemplarily, the first thickness of the electrode region 3 may be 10 nm, 50 nm or 100 nm. Exemplarily, when the electrode region 3 is 100 nm, the first thickness of the second doping portion 3022 is less than or equal to 1 / 5 of the first thickness of the electrode region 3 .
[0063] In some embodiments, in order to further improve the epitaxial quality of the semiconductor epitaxial structure, the second doping region is Al x In y Ga z N superlattice structure, the second doping region 302 is Al x In y Ga z N superlattice structure, x is greater than or equal to 0 and less than or equal to 1, y is greater than or equal to 0 and less than or equal to 1, and z is greater than 0.
[0064] In other embodiments, in order to further improve the epitaxial quality of the semiconductor epitaxial structure, the first doping region and the second doping region can both be superlattice structures alternately formed by different conductive doping media, such as a superlattice structure alternately formed by silicon (Si) doping and germanium (Ge) doping.
[0065] In some specific embodiments, please refer to Figure 1 and Figure 2 The material of the substrate 1 is silicon (Si), the material of the nucleation layer 4 is AlN, the material of the first semiconductor layer is GaN, the material of the second semiconductor layer is AlGaN, the material of the first doping region 301 is N-type heavily doped (N++) GaN, and the material of the second doping region 302 is N-type lightly doped (N+) GaN, and the above doping is all silicon (Si) doping.
[0066] In other specific embodiments, please refer to 2 and Figure 5The material of the substrate 1 is silicon (Si), the material of the nucleation layer 4 is AlN, the material of the first semiconductor layer is GaN, the material of the second semiconductor layer is AlGaN, the material of the first doping region 301 is N-type heavily doped (N++) GaN, the material of the first doping part 3021 is N-type lightly doped (N+) GaN, and the material of the second doping part 3022 is N-type heavily doped (N++) GaN, and the above doping is all silicon (Si) doping.
[0067] In other specific embodiments, please refer to 2 and Figure 5 The material of the substrate 1 is silicon (Si), the material of the nucleation layer 4 is AlN, the material of the first semiconductor layer is GaN, the material of the second semiconductor layer is AlGaN, the material of the first doping region 301 is N-type heavily doped (N++) GaN, the material of the first doping part 3021 is a superlattice structure of N-type lightly doped (N+) GaN, and the material of the second doping part 3022 is N-type heavily doped (N++) GaN. All of the above doping is silicon (Si) doping.
[0068] In other specific embodiments, please refer to 1 and Figure 2 The material of the substrate 1 is silicon (Si), the material of the nucleation layer 4 is AlN, the material of the first semiconductor layer is GaN, the material of the second semiconductor layer is AlGaN, the material of the first doping region 301 is germanium (Ge)-doped N-type heavily doped (N++) GaN, and the material of the second doping region 302 is silicon (Si)-doped N-type lightly doped (N+) GaN.
[0069] In other specific embodiments, please refer to 2 and Figure 5 The material of the substrate 1 is silicon (Si), the material of the nucleation layer 4 is AlN, the material of the first semiconductor layer is GaN, the material of the second semiconductor layer is AlGaN, the material of the first doping region 301 is germanium (Ge)-doped N-type heavily doped (N++) GaN, the material of the first doping part 3021 is silicon (Si)-doped N-type lightly doped (N+) GaN, and the material of the second doping part 3022 is silicon (Si)-doped N-type heavily doped (N++) GaN.
[0070] In other specific embodiments, please refer to 2 and Figure 5 The material of the substrate 1 is silicon (Si), the material of the nucleation layer 4 is AlN, the material of the first semiconductor layer is GaN, the material of the second semiconductor layer is AlGaN, the material of the first doping region 301 is germanium (Ge)-doped N-type heavily doped (N++) GaN, the material of the first doping part 3021 is silicon (Si)-doped N-type lightly doped (N+) GaN, and the material of the second doping part 3022 is germanium (Ge)-doped N-type heavily doped (N++) GaN.
[0071] In other specific embodiments, please refer to 2 and Figure 5 The material of the substrate 1 is silicon (Si), the material of the nucleation layer 4 is AlN, the material of the first semiconductor layer is GaN, the material of the second semiconductor layer is AlGaN, the first doping region 301 is an N-type heavily doped (N++) GaN superlattice structure doped with germanium (Ge) and silicon (Si), the first doping part 3021 is an N-type lightly doped (N+) GaN superlattice structure doped with germanium (Ge) and silicon (Si), and the second doping part 3022 is an N-type heavily doped (N++) GaN superlattice structure doped with germanium (Ge) and silicon (Si).
[0072] It should be noted that the electrode area 3 can be the above Figures 1 to 6 Any one or more combinations of layouts or some other suitable layouts.
[0073] See also Figure 6 ,like Figure 6 As shown, another aspect of the embodiment of the present application further provides a HEMT device 100, including:
[0074] A substrate 1; a compound semiconductor composite structure 2 disposed on the substrate 1, the compound semiconductor composite structure 2 comprising a first semiconductor layer 21 and a second semiconductor layer 22 disposed on the first semiconductor layer 21, wherein the first semiconductor layer 21 and the second semiconductor layer 22 disposed on the first semiconductor layer 21, and the first semiconductor layer 21 and the second semiconductor layer 22 form a heterojunction having a two-dimensional electron gas 20; two electrode regions 3 disposed on opposite sides of the compound semiconductor composite structure 2, the electrode regions 3 extending from the first semiconductor layer 21 to a side of the compound semiconductor composite structure 2 away from the substrate 1 The source 310 and the drain 320 are respectively arranged on the two electrode regions; the gate 330 is arranged on the compound semiconductor composite structure 2 and between the source 310 and the drain 320; the electrode region 3 includes a first doping region 301 close to the compound semiconductor composite structure 1 and a second doping region 302 away from the compound semiconductor composite structure 2 along the direction from the substrate 1 to the compound semiconductor composite structure 2, the first doping region 301 is located between the second doping region 302 and the compound semiconductor composite structure 2, and the conductivity of the first doping region 301 is greater than the conductivity of the second doping region.
[0075] The source electrode 310 and / or the drain electrode 320 are or include titanium, aluminum, nickel, gold, some other suitable metals or any combination thereof. In some embodiments, the source electrode 310 and / or the drain electrode 320 may include one or more layers of a titanium (Ti) layer, an aluminum (Al) layer, a nickel (Ni) layer and a gold (Au) layer connected in sequence.
[0076] In the present embodiment, the electrode region 3 is configured as a first doping region 301 and a second doping region 302 of different conductivities, thereby reducing the problem of poor epitaxial quality due to all high conductivity, and at the same time reducing the problem of large source-drain contact resistance due to all low conductivity. Therefore, in the present embodiment, by designing the electrode region 3 as at least a first doping region 301 of high conductivity and a second doping region 302 of low conductivity, it is possible to simultaneously reduce the source-drain contact resistance while ensuring the epitaxial quality of the semiconductor epitaxial structure, thereby improving the performance of the HEMT device 100.
[0077] Please refer to Figure 1-Figure 5 The semiconductor epitaxial structure of the HEMT device 100 is the semiconductor epitaxial structure 10 described in the above embodiment. The semiconductor epitaxial structure 10 can be applied to any embodiment of the HEMT device 100 and will not be described in detail herein.
[0078] In some other embodiments, see Figure 7 ,like Figure 7 As shown, the gate 330 may include a P-type nitride layer 3302 and a gate metal 3301. The gate metal 3301 may be or include nickel, gold, platinum, titanium nitride, aluminum copper, palladium, some other suitable metal and / or metal material or any combination of the foregoing. In some embodiments, the gate metal 3301 may mainly include one or both of a nickel (Ni) layer and a gold (Au) layer.
[0079] See also Figure 8 And refer to Figure 9a-9f Another aspect of the present application embodiment further provides a method for preparing a semiconductor epitaxial structure, which is used to prepare the semiconductor epitaxial structure 10, such as Figure 8 Said method comprises:
[0080] S81: Provide a substrate 1; in this embodiment, the substrate 1 may be a silicon (Si) substrate. It should be noted that the silicon (Si) substrate is not limited to high resistance or low resistance, and is not limited to N-type or P-type.
[0081] S82: forming a prefabricated first semiconductor layer 21' on the substrate 1;
[0082] S83: forming a prefabricated second semiconductor layer 22 ′ on the prefabricated first semiconductor layer 21 ′, and the prefabricated first semiconductor layer 21 ′ and the prefabricated second semiconductor layer 22 ′ form a heterojunction having a two-dimensional electron gas 20 to form a prefabricated compound semiconductor composite structure 2 ′.
[0083] It should be noted that the prefabricated compound semiconductor composite structure 2' that generates the two-dimensional electron gas can be formed as a channel layer and a barrier layer. In practical applications, before preparing the prefabricated compound semiconductor composite structure 2', other epitaxial layer structures, such as a nucleation layer and a buffer layer, are also prepared on the substrate 1, which will not be repeated here.
[0084] S84: forming first trenches 3 ′ in electrode regions on two opposite sides of the prefabricated compound semiconductor composite structure 2 ′, so as to form a compound semiconductor composite structure 2 having first trenches 3 ′ on two opposite sides.
[0085] Here, the etching process may be an in-situ etching process. It should be noted that the in-situ etching process is an important step for surface treatment of semiconductor materials before the start of a chemical vapor doping (CVD) growth process. The in-situ etching technology is used to improve the surface morphology and flatness of the semiconductor layer, creating conditions for the subsequent growth of the passivation layer, thereby improving the performance and reliability of the device. Of course, the formation of the first groove 3' may also be other processes, not limited to the in-situ etching process, which is well known to those skilled in the art, and the preparation method can be selected according to actual needs, which will not be repeated here.
[0086] S85: An electrode region 3 is formed in the first trench 3', and the electrode region 3 extends in the direction from the two-dimensional electron gas 20 to the compound semiconductor composite structure 2; along the direction from the substrate 1 to the compound semiconductor composite structure 2, the electrode region 3 includes a first doping region 301 close to the compound semiconductor composite structure 2 and a second doping region 302 away from the compound semiconductor composite structure 2, the first doping region 301 is located between the second doping region 302 and the compound semiconductor composite structure 2, and the conductivity of the first doping region 301 is greater than the conductivity of the second doping region 302.
[0087] In some embodiments, please refer to Figure 9d-9f Step S85, namely, forming the electrode region 3 in the first trench 3', may include:
[0088] Deposition is performed in the first trench 3' to form a prefabricated first doping region 301';
[0089] Etching the prefabricated first doping region 301 ′, retaining the threshold first doping region 301 ′ close to the compound semiconductor composite structure 2 to form the first doping region 301 ;
[0090] The second doping region 302 is deposited on the first doping region 301 .
[0091] The deposition process here can be PVD (Physical Vapor Deposition) or MOCVD (Metal-organic Chemical Vapor Deposition). Among them, PVD technology refers to the technology of using physical methods under vacuum conditions to vaporize the surface of the material source (solid or liquid) into gaseous atoms or molecules, or partially ionize into ions, and deposit a thin film with certain special functions on the surface of the substrate through a low-pressure gas (or plasma) process. MOCVD uses organic compounds of group III and group II elements and hydrides of group V and VI elements as crystal growth source materials, and performs vapor phase epitaxy on the substrate in a thermal decomposition reaction to grow various thin-layer single crystal materials of group III-V, group II-VI compound semiconductors and their multi-component solid solutions.
[0092] Of course, in some embodiments, please refer to FIG. 10 again, step S85, that is, forming the electrode region 3 in the first trench 3', includes:
[0093] Depositing a first doped region 301 in the first trench 3';
[0094] The second doping region 302 is formed by deposition on the first doping region 301 .
[0095] Furthermore, depositing and forming the first doping region 301 in the first trench 3 ′ may include: depositing and forming the first doping region 301 in the first trench 3 ′ and also forming the third doping region 303 on the sidewall 203 of the compound semiconductor composite structure 2 .
[0096] In this way, the electrode region 3 can be electrically connected to the two-dimensional electron gas 20 by forming the third doping region 303 on the sidewall, thereby effectively reducing the overall contact resistance of the electrode region.
[0097] In this embodiment, after the electrode region 3 is etched, a first doping region 301 and a second doping region 302 of different conductivities are formed by physical vapor or chemical deposition, thereby reducing the problem of poor epitaxial quality due to all high conductivity, and at the same time reducing the problem of large source and drain contact resistance due to all low conductivity. Therefore, the semiconductor epitaxial structure prepared by this process in this embodiment can achieve the simultaneous reduction of source and drain contact resistance and guarantee of epitaxial quality of the semiconductor epitaxial structure, thereby improving the performance of the HEMT device prepared using the semiconductor epitaxial structure.
[0098] Although the reference method describes Figure 8 , Figures 9 and 10, but it will be understood that Figure 8 9 and 10 are not limited to this method, but can be independently independent of this method. Figure 89 and 10 are described as a series of actions, but it will be understood that the order of the actions may be changed in other embodiments. Figure 8 9 and 10 show and describe a set of specific actions, but some actions shown and / or described may be omitted in other embodiments. In addition, actions not shown and / or described may be included in other embodiments.
[0099] In some embodiments, a method for preparing a semiconductor epitaxial structure may further include:
[0100] providing a substrate;
[0101] forming a prefabricated first semiconductor layer on the substrate;
[0102] forming a prefabricated second semiconductor layer on the prefabricated first semiconductor layer, wherein the prefabricated first semiconductor layer and the prefabricated second semiconductor layer form a heterojunction having a two-dimensional electron gas to form a prefabricated compound semiconductor composite structure;
[0103] Ion implantation is performed on opposite sides of a prefabricated semiconductor composite structure to form electrode regions, wherein the electrode regions, along a direction from the substrate to the compound semiconductor composite structure, include a first doped region close to the compound semiconductor composite structure and a second doped region away from the compound semiconductor composite structure, wherein the first doped region is located between the second doped region and the compound semiconductor composite structure, and the conductivity of the first doped region is greater than the conductivity of the second doped region.
[0104] In the present embodiment, two ion implantations are performed to form a first doping region and a second doping region of two different conductivities in the electrode region, thereby reducing the problem of poor epitaxial quality due to all high conductivity, and at the same time reducing the problem of large source and drain contact resistance due to all low conductivity. Therefore, the semiconductor epitaxial structure prepared by this process in the present embodiment can achieve the simultaneous reduction of source and drain contact resistance and the guarantee of epitaxial quality of the semiconductor epitaxial structure, thereby improving the performance of the HEMT device prepared using the semiconductor epitaxial structure.
[0105] The above description is only a preferred embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any technician in the field can easily make changes or variations within the technical scope disclosed in the present disclosure, and such changes or variations should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure shall be based on the protection scope of the claims. As long as there is no structural conflict, the various technical features mentioned in each embodiment can be combined in any way. The present disclosure is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A semiconductor epitaxial structure, characterized in that: include: substrate; A compound semiconductor composite structure disposed on the substrate, the compound semiconductor composite structure comprising a first semiconductor layer and a second semiconductor layer disposed on the first semiconductor layer, wherein the first semiconductor layer and the second semiconductor layer form a heterojunction having a two-dimensional electron gas; two electrode regions disposed on opposite sides of the compound semiconductor composite structure, the electrode regions extending from within the first semiconductor layer to a side of the compound semiconductor composite structure away from the substrate; The electrode region, along the direction from the substrate to the compound semiconductor composite structure, includes a first doped region close to the compound semiconductor composite structure and a second doped region far away from the compound semiconductor composite structure, the first doped region is located between the second doped region and the compound semiconductor composite structure, and the conductivity of the first doped region is greater than the conductivity of the second doped region.
2. The semiconductor epitaxial structure according to claim 1, characterized in that: Two electrode regions, including: a first electrode region and a second electrode region; The first electrode region is a source region, and the second electrode region is a drain region; or, The first electrode region is a drain region, and the second electrode region is a source region.
3. The semiconductor epitaxial structure according to claim 1, characterized in that: The electrode region has a conductive doping medium of a first conductivity type; when the conductive doping medium of the first doping region and the second doping region are the same, the doping concentration of the conductive doping medium of the first doping region is greater than the doping concentration of the conductive doping medium of the second doping region.
4. The semiconductor epitaxial structure according to claim 1, characterized in that: The first doping region extends from a side of the two-dimensional electron gas close to the substrate to a side of the compound semiconductor composite structure away from the substrate, and the first doping region is connected to the two-dimensional electron gas.
5. The semiconductor epitaxial structure according to claim 1, characterized in that: The compound semiconductor composite structure includes a first surface and a second surface relative to each other, and a side wall connecting the first surface and the second surface; the first doped region is located between the substrate and the two-dimensional electron gas, and the semiconductor epitaxial structure also includes: a third doped region, the third doped region intersects with the second doped region and is connected to the corresponding side wall of the compound semiconductor composite structure.
6. The semiconductor epitaxial structure according to claim 5, characterized in that: The first thickness of the first doping region is greater than the second thickness of the third doping region, the first thickness direction is the direction from the substrate to the compound semiconductor composite structure, and the second thickness direction is the arrangement direction of the two electrode regions.
7. The semiconductor epitaxial structure according to claim 1 or 5, characterized in that: The first thickness of the electrode region is 10-100 nm, the first thickness of the first doping region is less than or equal to 10 nm, and the first thickness direction is the direction from the substrate to the compound semiconductor composite structure.
8. The semiconductor epitaxial structure according to claim 1, characterized in that: The conductive doping medium is a first conductive doping medium, and the doping concentration of the first doping region is 1×10 19 ~1×10 20 cm3, the doping concentration of the second doping region is 1×10 17 ~1×10 19 cm3; and / or, The conductive doping medium is a second conductive doping medium, and the doping concentration of the first doping region is 1×10 19 ~5×10 20 cm3, the doping concentration of the second doping region is 1×10 17 ~5×10 19 cm3; The electron attraction of the first conductive doping medium is greater than the electron attraction of the second conductive doping medium.
9. The semiconductor epitaxial structure according to claim 1, characterized in that: The second doping region includes a first doping portion and a second doping portion; the first doping portion and the second doping portion are arranged along a direction from the substrate to the compound semiconductor composite structure, and the conductivity of the first doping portion is smaller than the conductivity of the second doping portion.
10. The semiconductor epitaxial structure according to claim 9, characterized in that: When the conductive doping medium of the first doping portion and the conductive doping medium of the second doping portion are the same, the doping concentration of the conductive doping medium of the first doping portion is greater than the doping concentration of the conductive doping medium of the second doping portion.
11. The semiconductor epitaxial structure according to claim 1, characterized in that: The second doping region is Al x In y Ga z N superlattice structure, x is greater than or equal to 0 and less than or equal to 1, y is greater than or equal to 0 and less than or equal to 1, and z is greater than 0.
12. The semiconductor epitaxial structure according to claim 9, characterized in that: A first thickness of the second doped portion is less than or equal to 10 nm.
13. A HEMT device, comprising: substrate; A compound semiconductor composite structure disposed on the substrate, the compound semiconductor composite structure comprising a first semiconductor layer and a second semiconductor layer disposed on the first semiconductor layer, wherein the first semiconductor layer and the second semiconductor layer form a heterojunction having a two-dimensional electron gas; two electrode regions disposed on opposite sides of the compound semiconductor composite structure, the electrode regions extending from within the first semiconductor layer to a side of the compound semiconductor composite structure away from the substrate; A source electrode and a drain electrode are respectively arranged on the two electrode regions; A gate electrode, disposed on the compound semiconductor composite structure and between the source electrode and the drain electrode; The electrode region, along the direction from the substrate to the compound semiconductor composite structure, includes a first doped region close to the compound semiconductor composite structure and a second doped region far away from the compound semiconductor composite structure, the first doped region is located between the second doped region and the compound semiconductor composite structure, and the conductivity of the first doped region is greater than the conductivity of the second doped region.
14. A method for preparing a semiconductor epitaxial structure, characterized in that: include: providing a substrate; forming a prefabricated first semiconductor layer on the substrate; forming a prefabricated second semiconductor layer on the prefabricated first semiconductor layer, wherein the prefabricated first semiconductor layer and the prefabricated second semiconductor layer form a heterojunction having a two-dimensional electron gas to form a prefabricated compound semiconductor composite structure; forming first grooves in electrode regions on two opposite sides of the prefabricated compound semiconductor composite structure to form a compound semiconductor composite structure having the first grooves on two opposite sides; forming an electrode region in the first trench, wherein the electrode region extends from within the first semiconductor layer toward a side of the compound semiconductor composite structure away from the substrate; The electrode region, along the direction from the substrate to the compound semiconductor composite structure, includes a first doped region close to the compound semiconductor composite structure and a second doped region far away from the compound semiconductor composite structure, the first doped region is located between the second doped region and the compound semiconductor composite structure, and the conductivity of the first doped region is greater than the conductivity of the second doped region.
15. The method for preparing a semiconductor epitaxial structure according to claim 14, characterized in that: The forming of the electrode region in the first groove comprises: Depositing a prefabricated first doped region in the first trench; Etching the prefabricated first doping region to retain the prefabricated first doping region close to the compound semiconductor composite structure to form the first doping region; The second doped region is deposited on the first doped region.
16. The method for preparing a semiconductor epitaxial structure according to claim 14, characterized in that: The forming of the electrode region in the first groove comprises: Depositing the first doped region in the first trench; A second doping region is formed by deposition on the first doping region.
Citation Information
Cited By
Recessed p-type gate structure for iii-nitride transistors
WO2026187841A1