Nitride semiconductor device and method of manufacturing same
By designing vertical gate trench and annular source trench in GaN devices, combining the control layer and semiconductor layer, the problem of uneven electric field and current distribution is solved, the risk of gate breakdown is reduced, and the risk of gate breakdown is improved. Device performance and reliability.
Patent Information
- Application Number
- CN202411024853.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-29
AI Technical Summary
GaN devices with vertical structures are prone to uneven electric field and current distribution when integrating Schottky barrier diodes, resulting in premature gate breakdown and reducing the performance and reliability of power devices.
A nitride semiconductor device is designed. By setting a vertical gate trench and an annular source trench in the device, the gate metal is prepared in the gate trench and the source metal is prepared in the source trench. In the groove, a circular structure is formed to wrap the gate, reduce the electric field strength of the gate region, and optimize the electric field distribution through the regulation layer and the semiconductor layer.
It effectively reduces the risk of gate breakdown, improves the performance and reliability of the device, ensures a more uniform electric field distribution, and prevents premature breakdown.
Smart Images

Figure CN118943181A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of semiconductor devices, and in particular to a nitride semiconductor device and a method for manufacturing the same. Background Art
[0002] The third generation of wide bandgap semiconductor materials represented by GaN (gallium nitride) materials and SiC (silicon carbide) materials have advantages such as high breakdown electric field strength and higher electron saturation velocity. Compared with SiC materials, GaN materials have the advantages of large bandgap width, high saturated electron drift velocity, small dielectric constant, strong corrosion resistance, and relatively easy preparation of high-quality heterojunctions, and are widely used in power semiconductor devices.
[0003] Gallium nitride Schottky barrier diodes (SBDs) have broad application prospects in mobile communications, semiconductor lighting, and consumer electronics due to their advantages such as high blocking voltage, high switching speed, and low power consumption.
[0004] However, vertically structured GaN devices usually produce uneven electric field and current distribution when integrating SBDs. In addition, since the gate is not effectively protected in the GaN device structure with integrated SBDs, the gate is prematurely broken down due to electric field concentration, thereby reducing the performance and reliability of the power device. Summary of the invention
[0005] The present application provides a nitride semiconductor device and a manufacturing method thereof, which can solve the breakdown problem existing in existing power devices. The technical solution is as follows:
[0006] A nitride semiconductor device comprises a first metal layer, an auxiliary layer, a drift layer, a channel layer, a barrier layer and a second metal layer which are sequentially arranged along the vertical direction of the device.
[0007] The nitride semiconductor device further includes a first trench and a second trench, wherein the first trench and the second trench both penetrate the barrier layer and the channel layer and extend into the drift layer;
[0008] The first trench is provided with a dielectric layer covering the bottom and sidewalls of the trench and a third metal layer filled in the first trench; the second trench is filled with the second metal layer;
[0009] The second groove is arranged around the first groove, and the second groove is in a circular ring shape.
[0010] In one of the embodiments, a regulating layer is provided between the drift layer and the channel layer;
[0011] The first trench sequentially penetrates the barrier layer, the channel layer, and the regulating layer and then extends into the drift layer.
[0012] In one of the embodiments, the nitride semiconductor device further includes a third trench, wherein the third trench penetrates the regulating layer and extends into the drift layer;
[0013] The third trench is filled with a first semiconductor layer, and the first semiconductor layer is flush with the upper surface of the regulating layer.
[0014] In one embodiment, the third groove is arranged around the first groove, the projection of the second groove on the regulating layer is entirely located on the first semiconductor layer, and the second groove penetrates the barrier layer and the channel layer and then extends into the first semiconductor layer.
[0015] In one embodiment, the third groove is in a circular ring shape, and the ring width of the third groove is greater than the ring width of the second groove.
[0016] In one embodiment, the first trench extends into the drift layer to a first depth, the third trench extends into the drift layer to a second depth, and the second depth is greater than the first depth.
[0017] In one embodiment, the second trench extends into the first semiconductor layer to a third depth, and the third depth is less than the thickness of the regulating layer.
[0018] In one of the embodiments, the first trench is further filled with a second semiconductor layer;
[0019] The first dielectric layer, the second semiconductor layer and the third metal layer are sequentially formed in the first trench along the vertical direction of the device.
[0020] In one embodiment, the first semiconductor layer and the second semiconductor layer are made of the same material.
[0021] In one embodiment, a fourth metal layer is further disposed on the periphery of the third trench, and the fourth metal layer is located between the barrier layer and the second metal layer;
[0022] The fourth metal layer and the drift layer together form a Schottky diode.
[0023] In one embodiment, the third metal layer and the fourth metal layer are made of the same material.
[0024] A method for manufacturing a nitride semiconductor device comprises the following steps:
[0025] Providing a substrate, and sequentially stacking an auxiliary layer and a drift layer on the substrate;
[0026] preparing a regulating layer on the drift layer;
[0027] Etching the regulating layer to form a third groove, and depositing the first semiconductor layer in the third groove; wherein the third groove is in a circular ring shape;
[0028] Sequentially stacking a channel layer and a barrier layer on the regulating layer;
[0029] Etching the barrier layer to form a first trench, and depositing a dielectric layer on the bottom and sidewalls of the first trench; wherein the first trench sequentially penetrates the barrier layer, the channel layer and the regulating layer from top to bottom along the vertical direction of the device, and is embedded in the drift layer;
[0030] Preparing a metal layer on the barrier layer; etching the metal layer to simultaneously form a gate layer located in the first trench and a Schottky metal layer located on both sides of the third trench;
[0031] Etching the barrier layer to form a second trench; wherein the second trench sequentially penetrates the barrier layer and the channel layer from top to bottom along the vertical direction of the device and is embedded in the first semiconductor layer;
[0032] Preparing a source electrode layer in the second trench; wherein the source electrode layer fills the second trench and covers the Schottky metal layer and the barrier layer;
[0033] The substrate is peeled off, and a drain metal layer is prepared on a side of the auxiliary layer away from the drift layer.
[0034] In one embodiment, the step of providing a substrate and forming an auxiliary layer on the substrate comprises:
[0035] A nucleation layer, a first buffer layer, a second buffer layer, a planarization layer, a third buffer layer and a fourth buffer layer are sequentially stacked on the substrate; wherein
[0036] Depositing aluminum nitride with a thickness of 10 nm to 30 nm on the substrate as the nucleation layer;
[0037] Depositing aluminum gallium nitride with a thickness of 0.1 μm to 0.2 μm on the nucleation layer as the first buffer layer;
[0038] Alternately depositing several layers of aluminum nitride and gallium nitride with a thickness of 1 nm to 3 nm on the first buffer layer to form the planar layer;
[0039] Depositing 150nm-300nm thick gallium nitride formed at low temperature on the flat layer as the third buffer layer;
[0040] A 500nm-1000nm thick gallium nitride formed at high temperature is deposited on the third buffer layer as the fourth buffer layer.
[0041] In one embodiment, the step of preparing a drift layer on the auxiliary layer includes at least one of the following:
[0042] Depositing undoped gallium nitride with a thickness of 1 μm to 20 μm on the auxiliary layer to form the drift layer;
[0043] Depositing 1 μm to 20 μm thick doped gallium nitride on the auxiliary layer to form the drift layer; wherein the doping concentration ranges from 1×10 15 cm -3 ~1×10 16 cm -3 .
[0044] In one embodiment, the specific steps of preparing the regulating layer on the drift layer include:
[0045] Depositing 50nm to 500nm thick doped gallium nitride on the drift layer to form the regulating layer; wherein the doping concentration range is 1×10 16 cm -3 ~1×10 17 cm -3 .
[0046] In one embodiment, the specific steps of etching the regulating layer to form a third groove and depositing the first semiconductor layer in the third groove include:
[0047] Etching the regulating layer until it extends into the drift layer to form the third trench; wherein the total height of the third trench in the vertical direction of the device is 150nm to 500nm, and the photolithographic pattern formed by etching is in a circular ring shape;
[0048] A P-type doped gallium nitride having a thickness of 150 nm to 500 nm is deposited in the third trench to form the first semiconductor layer.
[0049] In one embodiment, the specific steps of sequentially stacking a channel layer and a barrier layer on the regulating layer include:
[0050] Depositing undoped gallium nitride with a thickness of 0.3 μm to 1 μm on the regulating layer to form the channel layer;
[0051] Aluminum gallium nitride with a thickness of 20nm to 30nm is deposited on the channel layer to form the barrier layer.
[0052] In one embodiment, the specific steps of etching the barrier layer to form a first trench and depositing a dielectric layer on the bottom and sidewalls of the first trench include:
[0053] Etching the barrier layer inside the inner ring of the third trench until it extends into the drift layer to form the first trench, wherein the depth of the first trench in the drift layer is less than the depth of the third trench in the drift layer, and the formed photolithography pattern is in the shape of a long strip;
[0054] Aluminum nitride with a thickness of 20 nm to 30 nm is deposited on the bottom and sidewalls of the first trench to form the dielectric layer.
[0055] In one embodiment, the second semiconductor layer is prepared in the first trench, and the specific steps include:
[0056] P-type doped gallium nitride is deposited on the dielectric layer to form the second semiconductor layer; wherein the thickness of the second semiconductor is smaller than the height of the first trench, and the height difference between the upper surface of the second semiconductor layer and the top surface of the first trench is in the range of 20nm to 30nm.
[0057] In one embodiment, a metal layer is prepared on the barrier layer, and the specific steps of etching the metal layer include:
[0058] Depositing a metal with a thickness of 20 nm to 30 nm on the barrier layer to form a metal layer; during the deposition process, part of the metal is directly deposited in the first groove;
[0059] The metal layer in the first trench and the metal layer around the third trench are etched away to form a gate layer in the first trench and a Schottky metal layer outside the third trench.
[0060] In one of the embodiments, 0.5 μm to 1.5 μm is deposited on the barrier layer, the gate layer, and the Schottky metal layer;
[0061] The passivation layer on the Schottky metal layer is etched.
[0062] In one embodiment, the specific step of etching the barrier layer to form the second trench includes:
[0063] Etching a portion of the passivation layer whose projection is located above the third trench between the Schottky metal layer and the first trench until it extends into the first semiconductor layer on the third trench to form a second trench; wherein the photolithography pattern formed by etching is in a circular ring shape;
[0064] A source layer is prepared in the second trench; wherein the source layer fills the second trench and covers the Schottky metal layer and the passivation layer.
[0065] The technical solution provided by the embodiments of the present application may include the following beneficial effects: by designing a gate groove in the device, preparing the gate metal in the gate groove, and then designing a ring-shaped source groove surrounding the gate groove in the device, and preparing the source metal in the source groove. This arrangement can wrap the gate in the source of the ring structure to reduce the electric field strength in the gate area, thereby reducing the risk of gate breakdown. At the same time, the design of the ring-shaped source groove helps to distribute the electric field more evenly, reduce the area where the electric field is concentrated, and further prevent premature breakdown to improve the performance and reliability of the device.
[0066] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0068] Figure 1 It is a schematic structural diagram of a nitride semiconductor device according to an embodiment of the present application at a certain viewing angle.
[0069] Figure 2-Figure 27 It is a structural schematic diagram of a manufacturing process of a nitride semiconductor device according to an embodiment of the present application.
[0070] Description of reference numerals:
[0071] 10. Substrate; 101. First metal layer.
[0072] 20. Auxiliary layer; 201. Nucleation layer; 202. First buffer layer; 203. Planarization layer; 204. Third buffer layer; 205. Fourth buffer layer.
[0073] 30. Drift layer.
[0074] 40. Channel layer.
[0075] 50. Barrier layer.
[0076] 60. Second trench / source trench; 601. Second metal layer / source layer.
[0077] 70, first trench / gate trench; 700, total metal layer; 701, dielectric layer; 702, third metal layer / gate layer; 703, second semiconductor layer; 704, fourth metal layer / Schottky metal layer.
[0078] 80. Regulatory layer.
[0079] 90. A third trench; 901. A first semiconductor layer.
[0080] 100. Passivation layer.
[0081] a, first depth; b, second depth; c, third depth. DETAILED DESCRIPTION
[0082] Compared with the first generation semiconductor material Si (silicon) and the second generation semiconductor material GaAs (gallium arsenide), the third generation wide bandgap semiconductor materials represented by GaN (gallium nitride) materials and SiC (silicon carbide) materials have advantages such as high breakdown electric field strength and higher electron saturation velocity. Compared with SiC materials, GaN materials have the advantages of large bandgap width, high saturated electron drift velocity, small dielectric constant, strong corrosion resistance and relatively easy preparation of high-quality heterojunctions, and are widely used in power semiconductor devices.
[0083] The current GaN power devices can be divided into lateral power devices and vertical power devices according to the conduction direction of the current. Lateral power devices refer to the formation of heterojunction structure by epitaxial barrier layer on the channel layer, and the polarization effect of GaN-based material system is used to generate two-dimensional electron gas (2DEG) on the heterojunction surface as a lateral current path. However, lateral devices have serious current collapse problems. Vertical power devices refer to the use of GaN materials for conduction to form a current that passes up and down. It can effectively solve the problems of lateral power devices.
[0084] Gallium nitride Schottky barrier diodes (SBDs) have broad application prospects in mobile communications, semiconductor lighting, and consumer electronics due to their advantages such as high blocking voltage, high switching speed, and low power consumption. The current gallium nitride Schottky barrier diodes (SBDs) mainly adopt two structural forms: vertical SBDs based on GaN bulk materials and lateral SBDs based on heterojunction two-dimensional electron gas (2DEG) such as barrier layers and channel layers.
[0085] Generally, vertical GaN devices are mostly composed of strip-shaped gates and drains. When forming vertical SBDs, the gate strips usually need to be split for preparation. This method not only leaves a large area of the device empty, resulting in uneven electric field and current distribution in the device, but also because the gate is exposed, the gate is prematurely broken down due to electric field concentration, thereby reducing the performance and reliability of the power device.
[0086] Based on this, the present application provides a nitride semiconductor device that can effectively solve the problems of breakdown and electric field unevenness caused by the structural design of power devices.
[0087] Reference Figure 1 , Fig.18 as well as Fig. 20 The nitride semiconductor provided in the present application includes a first metal layer 101, an auxiliary layer 20, a drift layer 30, a channel layer 40, a barrier layer 50 and a second metal layer 601 arranged in sequence along the vertical direction of the device. It also includes a first trench 70 and a second trench 60, which both penetrate the barrier layer 50 and the channel layer 40 and extend into the drift layer 30.
[0088] The first trench 70 includes a dielectric layer 701 covering the bottom and sidewalls of the trench and a third metal layer 702 filled in the first trench. The second trench is filled with a second metal layer 601. The second trench 60 is arranged around the first trench 70 and is in a circular ring shape.
[0089] It should be noted that, in some embodiments, the first metal layer 101 forms an ohmic contact with the auxiliary layer 20, and the lead-out terminal of the first metal layer 101 is a drain. The lead-out terminal of the second metal layer 601 is a source. The third metal layer 702 forms an ohmic contact with both the drift region and the barrier layer 50, and the lead-out terminal of the third metal layer 702 is a gate.
[0090] Specifically, the first metal layer 101 can be understood as a drain metal. The first trench 70 can also be understood as a gate trench, and the corresponding third metal layer 702 filled in the first trench 70 can be understood as a gate metal. The second trench 60 can be understood as a source trench, and the corresponding second metal layer 601 filled in the second trench 60 can be understood as a source metal.
[0091] For ease of understanding and readability, the first trench 70 is expressed as gate trench 70. The third metal layer 702 is expressed as gate layer 702. The second trench 60 is expressed as source trench 60, and the second metal layer 601 is expressed as source layer 601.
[0092] In the present application, the annular source groove 60 is designed around the gate groove 70, and then the gate layer 702 is filled in the gate groove 70 accordingly to control the flow of current in the device, and the source layer 601 is filled in the source groove 60 to control the current flowing into or out of the device.
[0093] This structure can not only wrap the gate layer 702 to reduce the electric field strength in the gate area, thereby reducing the risk of gate breakdown. Secondly, the annular source groove 60 makes the filled source layer 601 have the same shape, providing a larger contact area between the source layer 601 and the drift layer 30, which helps to reduce the contact resistance. Finally, the annular source layer 601 helps to distribute the electric field more evenly, reduce the area where the electric field is concentrated, and further prevent the premature breakdown of the device.
[0094] In some embodiments, the drift layer 30 and the channel layer 40 are made of gallium nitride (GaN), the barrier layer 50 is made of aluminum gallium nitride (AlGaN), and the dielectric layer 701 is made of aluminum nitride (AlN).
[0095] Since the gate groove 70 sequentially penetrates the barrier layer 50 and the channel in the vertical direction of the device and then extends to the drift layer 30, the bottom of the gate layer 702 contacts the drift layer 30, and the side wall of the gate layer 702 contacts the channel layer 40. Therefore, when the dielectric layer 701 is prepared in the bottom and the side wall, the dielectric layer 701 forms AlN / GaN heterojunctions with the drift layer 30 and the channel layer 40 respectively.
[0096] The heterostructure formed by AlN / GaN will produce a piezoelectric effect due to the lattice constant mismatch. This effect, combined with the spontaneous polarization effect of AlN, can produce a strong built-in electric field. The built-in electric field can attract electrons in GaN to the vicinity of the AlN / GaN interface to form a high-density 2DEG, thereby reducing channel resistance and improving current driving capability, thereby improving the conductivity and switching speed of the device.
[0097] In some embodiments, continue to refer to Fig.18 The gate groove 70 is also filled with a second semiconductor layer 703. That is, after the dielectric layer 701 is prepared at the bottom and sidewall of the gate groove 70, the second semiconductor layer 703 and the gate layer 702 are filled in sequence.
[0098] Specifically, the material of the second semiconductor layer 703 is selected from gallium nitride (p-GaN) doped with p-type impurities. It still relies on the setting that the gate groove 70 penetrates the barrier layer 50 and the channel layer 40 and penetrates into the drift layer 30. When the p-GaN (second semiconductor layer) is filled in the gate groove 70, the band structure between p-GaN and AlGaN (barrier layer 50) changes, resulting in an increase in the barrier, that is, the barrier height of AlGaN can be increased. The increase in the barrier height can raise the potential energy at the channel under the gate layer 702 to above the Fermi level, and improve the conductivity of the channel by modulating the concentration of carriers in the channel.
[0099] In some embodiments, continue to refer to Figure 1 A regulation layer 80 is disposed between the drift layer 30 and the channel layer 40 .
[0100] Specifically, the material of the control layer 80 is doped gallium nitride. The specific doping concentration depends on the doping distribution requirements in the device manufacturing process, which will not be elaborated here.
[0101] Preparing the regulating layer 80 on the drift layer 30 can effectively adjust the electric field distribution in the drift layer 30 to optimize the breakdown voltage and the current carrying capacity of the device. It is also possible to create a space charge region in the drift layer 30 through complex doping engineering to help smooth the electric field distribution and reduce the local electric field strength, thereby increasing the device breakdown voltage.
[0102] In one embodiment, referring to Figure 1 The gate groove 70 sequentially penetrates the barrier layer 50, the channel layer 40 and the regulating layer 80, and then extends into the drift layer 30. The dielectric layer 701 on the inner sidewall of the gate groove 70 contacts the regulating layer 80, the channel layer 40 and the barrier layer 50 respectively.
[0103] In some embodiments, reference Fig. 9 and Fig.11 The nitride semiconductor device further includes a third trench 90, which penetrates the regulating layer 80 and extends into the drift layer 30. The third trench 90 is filled with a first semiconductor layer 901, and the first semiconductor layer 901 is flush with the upper surface of the regulating layer 80.
[0104] Specifically, the material of the first semiconductor layer 901 is consistent with the material of the second semiconductor layer 703 , and is gallium nitride doped with p-type impurities (p-GaN).
[0105] Adding the first semiconductor layer 901 between the source and the drain can block the charge penetration under high voltage conditions, thereby increasing the breakdown voltage of the device.
[0106] Furthermore, the first semiconductor layer 901 and the regulating layer 80 below the channel layer 40 work together to effectively increase the device saturation output current and reduce turn-off leakage, thereby achieving better reliability and lower power consumption.
[0107] In some embodiments, reference Figure 1 , 14 The third trench 90 is arranged around the gate trench 70 , and the projection of the source trench 60 on the regulating layer 80 is entirely located on the first semiconductor layer 901 . The source trench 60 penetrates the barrier layer 50 and the channel layer 40 and extends into the first semiconductor layer 901 .
[0108] It can be understood that the source groove 60 formed on the barrier layer 50 penetrates the barrier layer 50 and the channel layer 40 and the bottom is located in the third groove 90 , and the lower surface of the source layer 601 filled in the source groove 60 is in contact with the first semiconductor layer 901 .
[0109] In one embodiment, the source layer 601 extends into the first semiconductor layer 901 to a depth less than the thickness of the regulation layer 80 .
[0110] In some embodiments, the third trench 90 is annular, and the width of the third trench 90 is greater than the width of the source trench 60. This configuration can ensure that the source layer 601 can be in full contact with the first semiconductor layer 901.
[0111] The specific values of the ring widths of the third trench 90 and the source trench 60 are determined according to the actual needs of the device production and are not limited here. The ratio relationship between the ring widths of the third trench 90 and the source trench 60 is also determined according to actual needs. As long as the simple size relationship between the two is satisfied, it is within the protection scope of this application.
[0112] In some embodiments, reference Figure 1 The gate groove 70 extends into the drift layer 30 to a first depth a, and the third trench 90 extends into the drift layer 30 to a second depth b. The second depth b is greater than the first depth a.
[0113] It can also be understood that the depth of the second semiconductor layer 703 in the drift layer 30 is less than the depth of the first semiconductor layer 901 in the drift layer 30, which has the following beneficial effects:
[0114] First, the second semiconductor layer 703 is embedded in the drift layer 30 at a shallow depth, which can directly and effectively control the channel, help improve the switching speed of the device and reduce the on-resistance. It can also reduce the charge carrier injection between the gate and the drift layer 30, and reduce the power consumption of the device in the on state.
[0115] The deeper the first semiconductor layer 901 is embedded in the drift layer 30, the better it is at blocking the penetration of charge carriers between the source and the drain to improve the withstand voltage of the device. It also helps to form a more uniform electric field distribution in the drift layer 30, reducing the risk of electric field concentration and breakdown. At the same time, it can also withstand a higher reverse bias without breakdown, thereby improving the breakdown voltage of the device.
[0116] In some embodiments, continue to refer to Figure 1 A fourth metal layer 704 is further disposed on the periphery of the third trench 90, and the fourth metal layer 704 is located between the barrier layer 50 and the second metal layer 601. The fourth metal layer 704 and the drift layer 30 together form a Schottky diode.
[0117] A fourth metal layer 704 is formed on the outer periphery of the third trench 90 and on the barrier layer 50. The fourth metal layer 704 may also be understood and replaced by a Schottky metal layer 704.
[0118] First, setting the Schottky diode on the periphery of the third groove 90 means that the Schottky diode is also located on the periphery of the source groove 60. Under the joint action of the annular source layer 601 and the Schottky diode located at the edge of the source groove 60, the gate can be completely wrapped, further avoiding premature breakdown of the gate area, thereby improving the stability of the device.
[0119] Secondly, the Schottky diode provides a current path when it is reverse biased, which can prevent breakdown caused by reverse voltage and protect the device from damage. At the same time, the Schottky diode has a high voltage resistance characteristic and can operate under high reverse voltage without avalanche breakdown.
[0120] The present application also provides a method for manufacturing a nitride semiconductor device, comprising the following steps. It should be noted that the lithography or etching technology involved in the following steps includes electron beam lithography (EBL) and deep ultraviolet lithography (DUV) technology. And different steps are selected according to actual needs. At the same time, the specific steps of lithography include pretreatment, glue coating, pre-baking, exposure and development. The operations are all routine operations and will not be described in detail here.
[0121] Secondly, the deposition technologies involved in the following steps include metal organic chemical vapor deposition (MOCVD), molecular beam epitaxy (MBE), low pressure chemical vapor deposition (LP-CVD) and plasma enhanced chemical vapor deposition (PECVD). Different steps can be selected according to actual needs, and no further details are given here.
[0122] Step S10 , providing a substrate 10 , and sequentially stacking an auxiliary layer 20 and a drift layer 30 on the substrate 10 .
[0123] In one embodiment, the material of the substrate 10 is single crystal diamond.
[0124] Furthermore, the specific steps of preparing the auxiliary layer 20 on the substrate 10 include:
[0125] S101, reference Figure 2 , aluminum nitride with a thickness of 10 nm to 30 nm is deposited on the substrate 10 as a nucleation layer 201 .
[0126] The nucleation layer 201 can promote crystal growth, reduce lattice defects, and improve crystal quality. Secondly, the material selection of the nucleation layer 201 can affect the electrical, optical and other properties of the device. In practical applications, the performance of the device can be optimized by adjusting the properties of the nucleation layer 201. Finally, the nucleation layer 201 can alleviate the lattice mismatch between the single crystal diamond and the gallium nitride body, reduce the lattice strain, and reduce the generation of lattice defects.
[0127] In some embodiments, the material of the nucleation layer 201 may also be gallium nitride (GaN), indium nitride (InN), etc.
[0128] S102. Reference Figure 3 , aluminum gallium nitride (AlGaN) is deposited on the nucleation layer 201 with a thickness of 0.1 μm to 0.2 μm as the first buffer layer 202 .
[0129] The first buffer layer 202 can alleviate the lattice mismatch between the substrate 10 and GaN, reduce the lattice strain, thereby reducing the lattice defect density and improving the performance and reliability of the device.
[0130] Furthermore, the first buffer layer 202 includes a plurality of sub-buffer layers, and in a direction away from the substrate 10 , the AL concentration doped in each sub-buffer layer gradually increases in a gradient state.
[0131] In one embodiment, the first buffer layer 202 includes 10 sub-buffer layers, which are stacked in sequence in a direction away from the substrate 10, and the doping AL concentrations are 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, and 100%, respectively.
[0132] S103. Reference Figure 4 , several layers of AlN and GaN with a thickness of 1 nm to 3 nm are alternately deposited on the first buffer layer 202 to form a planarization layer 203 .
[0133] In the present application, the flat layer 203 reduces the dislocation density through a multi-level alternating stress field, so that the subsequent epitaxial layer is flatter and more uniform.
[0134] In one embodiment, a layer of AlN and a layer of GaN form a pair. The thickness of each pair of AlN / GaN is preferably 2 nm. The total thickness of the planar layer 203 is 40 nm.
[0135] S104. Reference Figure 5 , a 150 nm to 300 nm thick low-temperature formed GaN is deposited on the planar layer 203 as the third buffer layer 204 .
[0136] Low-temperature GaN can reduce stress caused by lattice mismatch or thermal expansion coefficient difference. At the same time, low-temperature GaN can improve the adhesion between the subsequently grown GaN and the substrate 10 and reduce defects. Finally, low-temperature GaN can serve as a template for subsequent growth, which helps to improve the growth rate and uniformity of growth.
[0137] In one embodiment, the thickness of the third buffer layer 204 is preferably 150 nm.
[0138] S105, reference Figure 6, a 500nm-1000nm thick GaN formed at high temperature is deposited on the third buffer layer 204 as the fourth buffer layer 205. Preferably, the thickness of the fourth buffer layer 205 is 1000nm.
[0139] The high temperature GaN buffer layer can provide a high-quality foundation, so that the subsequent drift layer 30 can have better crystal quality and lower defect density.
[0140] S106, reference Figure 7 , a drift layer 30 is formed on the auxiliary layer 20 .
[0141] In one embodiment, undoped GaN with a thickness of 1 μm to 20 μm is deposited on the fourth buffer layer 205 to form the drift layer 30 .
[0142] In one embodiment, a 1 μm-20 μm thick doped GaN is deposited on the fourth buffer layer 205 to form the drift layer 30. The doping concentration range is 1×10 15 cm -3 ~1×10 16 cm -3 This means that every cubic centimeter of semiconductor material contains 10 to the 15th power to 10 to the 16th power of doping atoms.
[0143] The drift layer 30 provides a path for conducting most of the current and withstands the voltage when the device is working. In actual application, the thickness and doping concentration of the drift layer 30 directly affect the breakdown voltage and on-resistance of the device. It can be prepared according to actual needs.
[0144] Step S200, refer to Figure 8 , a regulating layer 80 is prepared on the drift layer 30 .
[0145] Specifically, a 50 nm to 500 nm thick doped gallium nitride is deposited on the drift layer 30 to form the control layer 80. The doping concentration range is 1×10 16 cm -3 ~1×10 17 cm -3 This means that every cubic centimeter of semiconductor material contains 10 to the 16th power to 10 to the 17th power of doping atoms.
[0146] The regulating layer 80 is used to adjust the electric field distribution in the drift layer 30 to optimize the breakdown voltage and the current carrying capacity of the device. Through complex doping engineering, a space charge region can be created in the drift layer 30 to help smooth the electric field distribution and reduce the local electric field strength, thereby increasing the breakdown voltage of the device.
[0147] Step S300, refer to Figure 9-11, the regulating layer 80 is etched to form a third trench 90, and a first semiconductor layer 901 is deposited in the third trench 90. The third trench 90 is in a circular ring shape.
[0148] Reference Fig. 9 , the regulating layer 80 is etched until it extends into the drift layer 30 to form a third trench 90. Preferably, the total height of the third trench 90 in the vertical direction of the device is 150nm to 500nm. It can also be understood as the depth of the third trench 90.
[0149] Reference Fig.10 The photolithography pattern formed by etching is in the shape of a circular ring.
[0150] In one embodiment, P-type doped gallium nitride (P-GaN) is deposited in the third trench 90 to form a first semiconductor layer 901 in a ring shape.
[0151] The first semiconductor layer 901 acts as a current block, that is, as described above, the first semiconductor layer 901 can block the charge penetration between the source and the drain to prevent the device from accidentally conducting electricity under high voltage conditions, thereby improving the voltage resistance and reliability of the device.
[0152] Step S400, refer to Fig.12 and Fig.13 , a channel layer 40 and a barrier layer 50 are sequentially stacked on the regulating layer 80 .
[0153] In one embodiment, undoped GaN with a thickness of 0.3 μm to 1 μm is deposited on the regulating layer 80 to form the channel layer 40. The channel layer 40 provides current flow from the gate to the source.
[0154] In one embodiment, a barrier layer 50 is formed by depositing 20 nm to 30 nm thick AlGaN on the channel layer 40. The channel layer 40 and the barrier layer 50 form an AlGaN / GaN heterojunction to form a high-density 2DEG to reduce channel resistance and improve current driving capability, thereby improving the conductivity and switching speed of the device.
[0155] Step S500, etching the barrier layer 50 to form a first trench 70. As can be seen from the above content, the first trench in this step is the gate trench 70, and is also replaced by the gate trench 70 in this embodiment.
[0156] Specifically, refer to Fig.14 The projection of the region where the gate groove 70 is provided on the control layer 80 is located in the inner ring region of the third trench 90 mentioned above. The barrier layer 50 , the channel layer 40 , the control layer 80 and even the drift layer 30 are etched.
[0157] In one embodiment, the photolithography pattern on the gate groove 70 is designed to be a long strip. Further, the gate groove 70 is rectangular in shape. Preferably, the gate groove 70 is a combination of a rectangular and a circular structure, and the rectangular and circular structures have an overlapping area. Preferably, referring to Fig.15 The gate groove 70 is a combination of a rectangular and a circular structure, and the center of the circular structure coincides with the midpoint of the rectangular structure. Further, the diameter of the circular structure is greater than the width of the rectangle.
[0158] In one embodiment, the distances from both sides of the gate trench 70 to the third trench 90 are equal.
[0159] In some embodiments, continue to refer to Fig.14 , the depth of the gate groove 70 in the drift layer 30 is less than the depth of the third trench 90 in the drift layer 30 .
[0160] S501 , depositing a dielectric layer 701 on the bottom and sidewalls of the gate trench 70 .
[0161] Reference Fig.16 and Fig.17 , AlN with a thickness of 20 nm to 30 nm is deposited on the bottom and sidewall of the gate groove 70 to form a dielectric layer 701. The relevant contents and effects of the dielectric layer 701 are consistent with the description of the dielectric layer 701 in the above content, and will not be repeated here.
[0162] S502 , preparing a second semiconductor layer 703 in the gate groove 70 .
[0163] Specifically, refer to Fig.18 , P-GaN is deposited on the dielectric layer 701 to form a second semiconductor layer 703. The relevant contents and effects of the second semiconductor layer 703 are consistent with the description of the dielectric layer 701 in the above content, and will not be repeated here.
[0164] In some embodiments, the thickness of the second semiconductor layer 703 is smaller than the height of the gate trench 70 , and the height difference between the upper surface of the second semiconductor layer 703 and the top surface of the first trench is in the range of 20 nm to 30 nm.
[0165] When preparing the gate layer 702, this arrangement can ensure that the gate metal above the gate groove 70 is completely deposited in the gate groove 70. Preferably, the upper surface of the gate layer 702 is flush with the top of the gate groove 70 and the upper surface of the barrier layer 50.
[0166] Step S600, refer to Fig.19 , a total metal layer 700 is prepared on the barrier layer 50 .
[0167] Specifically, a metal with a thickness of 20 nm to 30 nm is deposited on the barrier layer 50 to form a total metal layer 700. The metal layer is made of at least one of metal materials such as Ni (Nickel), Pt (Platinum), Mo (Molybdenum), Cr (Chromium), Al (Aluminum), and Au (Gold).
[0168] During the deposition process, continue to refer to Fig.19 , the metal located above the gate groove 70 is directly deposited in the gate groove 70 . Another part of the metal is deposited on the barrier layer 50 .
[0169] S601, reference Fig. 20 , the metal layer in the gate groove 70 and the total metal layer 700 around the third trench 90 are etched away to form a gate layer 702 located in the gate groove 70 and a Schottky metal layer 704 located outside the third trench 90 .
[0170] During this process, continue to refer to Fig. 20 , the metal in the gate groove 70 is retained to form a gate layer 702. The total metal layer 700 of the outer ring of the projection of the third trench 90 above the barrier layer 50 is retained to form a Schottky metal layer 704. The Schottky metal layer 704, the barrier layer 50, the drift layer 30, etc. constitute a Schottky barrier diode structure.
[0171] S602, depositing a passivation layer 100 on the device surface. Fig.21 A passivation layer 100 with a thickness of 0.5 μm to 1.5 μm is deposited on the upper surface of the barrier layer 50 , the gate layer 702 , the Schottky metal layer 704 and the dielectric layer 701 .
[0172] S603, reference Fig. 22 , the passivation layer 100 on the Schottky metal layer 704 and the passivation layer 100 between the Schottky metal layer 704 and the gate layer 702 and on the barrier layer 50 in the projection of the third trench 90 on the barrier layer 50 are etched. It can also be understood that the passivation layer 100 above the gate layer 702 is retained and not etched.
[0173] Reference Fig. 22 and Fig.23 The region on the barrier layer 50 where the passivation layer 100 is not provided is the region of the source groove 60. The rounded region is in a circular ring shape.
[0174] Step S700, etching the barrier layer 50 to form a second trench 60. As can be seen from the above, the second trench 60 in this step is the source trench 60, which is also replaced by the source trench 60 in this embodiment. Therefore, this step can be understood as etching in the source trench 60 region to form the source trench 60.
[0175] Reference Fig.24 and Fig.25 The source groove 60 penetrates the barrier layer 50 and the channel layer 40 from top to bottom along the vertical direction of the device, and is embedded in the first semiconductor layer 901. The source groove 60 is also arranged in a circular ring shape around the gate groove 70.
[0176] In some embodiments, the source trench 60 is embedded into the first semiconductor layer 901 to a depth less than the thickness of the regulation layer 80 .
[0177] In some embodiments, the ring width of the third trench 90 is greater than the ring width of the source trench 60 .
[0178] Step S800 , preparing a source layer 601 in the source trench 60 .
[0179] The source metal is one of Pt (Platinum, platinum), Mo (Molybdenum, molybdenum), silver (Silver, Ag), aluminum (Aluminum, Al), and copper (Copper, Cu).
[0180] In some embodiments, reference Fig.26 , the source layer 601 fills the source groove 60 and covers the Schottky metal layer 704 and the barrier layer 50 .
[0181] Step S900, refer to Fig. 27 , the substrate 10 is peeled off, and a drain layer 101 is formed on a side of the auxiliary layer 20 away from the drift layer 30 .
[0182] Specifically, the substrate 10 is peeled off using a laser lift-off technique, CMP (chemical mechanical polishing) or a shearing technique.
[0183] The drain layer 101 is made of one of Pt (Platinum), Mo (Molybdenum), silver (Ag), aluminum (Al), and copper (Cu).
[0184] The words "first", "second" and similar terms used in the specification and claims of this application do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, "multiple" or "several" means two or more. Unless otherwise indicated, the words "top" and / or "bottom" and similar terms are only for convenience of description and are not limited to one position or one spatial orientation.
Claims
1. A nitride semiconductor device, comprising a first metal layer, an auxiliary layer, a drift layer, a channel layer, a barrier layer and a second metal layer arranged in sequence along the vertical direction of the device, It is characterized in that The nitride semiconductor device further includes a first trench and a second trench, wherein the first trench and the second trench both penetrate the barrier layer and the channel layer and extend into the drift layer; A dielectric layer covering the bottom and sidewalls of the groove and a third metal layer filled in the first groove are arranged in the first groove; The second groove is filled with the second metal layer; The second groove is arranged around the first groove, and the second groove is in a circular ring shape.
2. The nitride semiconductor device according to claim 1, It is characterized in that A regulating layer is provided between the drift layer and the channel layer; The first trench sequentially penetrates the barrier layer, the channel layer, and the regulating layer and then extends into the drift layer.
3. The nitride semiconductor device according to claim 2, It is characterized in that The nitride semiconductor device further includes a third trench, wherein the third trench penetrates the regulating layer and extends into the drift layer; The third trench is filled with a first semiconductor layer, and the first semiconductor layer is flush with the upper surface of the regulating layer.
4. The nitride semiconductor device according to claim 3, It is characterized in that The third groove is arranged around the first groove, The projections of the second grooves on the regulating layer are all located on the first semiconductor layer, and the second grooves penetrate the barrier layer and the channel layer and then extend into the first semiconductor layer.
5. The nitride semiconductor device according to claim 4, It is characterized in that The third groove is in a circular ring shape, and the ring width of the third groove is greater than the ring width of the second groove.
6. The nitride semiconductor device according to claim 4, It is characterized in that The first trench extends into the drift layer to a first depth, and the third trench extends into the drift layer to a second depth, wherein the second depth is greater than the first depth.
7. The nitride semiconductor device according to claim 6, It is characterized in that The second trench extends into the first semiconductor layer to a third depth, and the third depth is less than the thickness of the regulating layer.
8. The nitride semiconductor device according to claim 3, It is characterized in that The first trench is also filled with a second semiconductor layer; The first dielectric layer, the second semiconductor layer and the third metal layer are sequentially formed in the first trench along the vertical direction of the device.
9. The nitride semiconductor device according to claim 8, It is characterized in that The first semiconductor layer and the second semiconductor layer are made of the same material.
10. The nitride semiconductor device according to any one of claims 3 to 9, It is characterized in that A fourth metal layer is further disposed at the periphery of the third trench, and the fourth metal layer is located between the barrier layer and the second metal layer; The fourth metal layer and the drift layer together form a Schottky diode.
11. The nitride semiconductor device according to claim 10, It is characterized in that The third metal layer and the fourth metal layer are made of the same material.
12. A method for manufacturing a nitride semiconductor device, It is characterized in that The following steps are involved: Providing a substrate, and sequentially stacking an auxiliary layer and a drift layer on the substrate; preparing a regulating layer on the drift layer; Etching the regulating layer to form a third groove, and depositing the first semiconductor layer in the third groove; wherein the third groove is in a circular ring shape; Sequentially stacking a channel layer and a barrier layer on the regulating layer; Etching the barrier layer to form a first trench, and depositing a dielectric layer on the bottom and sidewalls of the first trench; wherein the first trench sequentially penetrates the barrier layer, the channel layer and the regulating layer from top to bottom along the vertical direction of the device, and is embedded in the drift layer; preparing a metal layer on the barrier layer; Etching the metal layer to simultaneously form a gate layer located in the first trench and a Schottky metal layer located on both sides of the third trench; Etching the barrier layer to form a second trench; wherein the second trench sequentially penetrates the barrier layer and the channel layer from top to bottom along the vertical direction of the device and is embedded in the first semiconductor layer; Preparing a source electrode layer in the second trench; wherein the source electrode layer fills the second trench and covers the Schottky metal and the barrier layer; The substrate is peeled off, and a drain metal layer is prepared on a side of the auxiliary layer away from the drift layer.
13. The method for manufacturing a nitride semiconductor device according to claim 12, It is characterized in that The step of providing a substrate and forming an auxiliary layer on the substrate comprises: A nucleation layer, a first buffer layer, a second buffer layer, a planarization layer, a third buffer layer and a fourth buffer layer are sequentially stacked on the substrate; wherein Depositing aluminum nitride with a thickness of 10 nm to 30 nm on the substrate as the nucleation layer; Depositing aluminum gallium nitride with a thickness of 0.1 μm to 0.2 μm on the nucleation layer as the first buffer layer; Alternately depositing several layers of aluminum nitride and gallium nitride with a thickness of 1 nm to 3 nm on the first buffer layer to form the planar layer; Depositing 150nm-300nm thick gallium nitride formed at low temperature on the flat layer as the third buffer layer; A 500nm-1000nm thick gallium nitride formed at high temperature is deposited on the third buffer layer as the fourth buffer layer.
14. The method for manufacturing a nitride semiconductor device according to claim 13, It is characterized in that The step of preparing a drift layer on the auxiliary layer comprises at least one of the following: Depositing undoped gallium nitride with a thickness of 1 μm to 20 μm on the auxiliary layer to form the drift layer; Depositing 1 μm to 20 μm thick doped gallium nitride on the auxiliary layer to form the drift layer; wherein the doping concentration ranges from 1×10 15 cm -3 ~1×10 16 cm -3 .
15. The method for manufacturing a nitride semiconductor device according to claim 14, It is characterized in that The specific steps of preparing the regulating layer on the drift layer include: Depositing 50nm to 500nm thick doped gallium nitride on the drift layer to form the regulating layer; wherein the doping concentration range is 1×10 16 cm -3 ~1×10 17 cm -3 .
16. The method for manufacturing a nitride semiconductor device according to claim 15, It is characterized in that The specific steps of etching the regulating layer to form a third groove and depositing the first semiconductor layer in the third groove include: Etching the regulating layer until it extends into the drift layer to form the third trench; wherein the total height of the third trench in the vertical direction of the device is 150nm to 500nm, and the photolithographic pattern formed by etching is in a circular ring shape; A P-type doped gallium nitride having a thickness of 150 nm to 500 nm is deposited in the third trench to form the first semiconductor layer.
17. The method for manufacturing a nitride semiconductor device according to claim 16, It is characterized in that The specific steps of sequentially stacking a channel layer and a barrier layer on the regulating layer include: Depositing undoped gallium nitride with a thickness of 0.3 μm to 1 μm on the regulating layer to form the channel layer; Aluminum gallium nitride with a thickness of 20nm to 30nm is deposited on the channel layer to form the barrier layer.
18. The method for manufacturing a nitride semiconductor device according to claim 17, It is characterized in that The specific steps of etching the barrier layer to form a first trench and depositing a dielectric layer on the bottom and sidewalls of the first trench include: Etching the barrier layer inside the inner ring of the third trench until it extends into the drift layer to form the first trench, wherein the depth of the first trench in the drift layer is less than the depth of the third trench in the drift layer, and the formed photolithography pattern is in the shape of a long strip; Aluminum nitride with a thickness of 20 nm to 30 nm is deposited on the bottom and sidewalls of the first trench to form the dielectric layer.
19. The method for manufacturing a nitride semiconductor device according to claim 18, It is characterized in that The second semiconductor layer is prepared in the first trench, and the specific steps include: P-type doped gallium nitride is deposited on the dielectric layer to form the second semiconductor layer; wherein the thickness of the second semiconductor is smaller than the height of the first trench, and the height difference between the upper surface of the second semiconductor layer and the top surface of the first trench is in the range of 20nm to 30nm.
20. The method for manufacturing a nitride semiconductor device according to claim 19, It is characterized in that The specific steps of preparing a metal layer on the barrier layer and etching the metal layer include: Depositing a metal with a thickness of 20 nm to 30 nm on the barrier layer to form a metal layer; during the deposition process, part of the metal is directly deposited in the first groove; The metal layer in the first trench and the metal layer around the third trench are etched away to form a gate layer in the first trench and a Schottky metal layer outside the third trench.
21. The method for manufacturing a nitride semiconductor device according to claim 20, It is characterized in that Depositing a passivation layer with a thickness of 0.5 μm to 1.5 μm on the barrier layer, the gate layer, and the Schottky metal layer; The passivation layer on the Schottky metal layer is etched.
22. The method for manufacturing a nitride semiconductor device according to claim 21, It is characterized in that The specific steps of etching the barrier layer to form the second trench include: Etching a portion of the passivation layer whose projection is located above the third trench between the Schottky metal layer and the first trench until it extends into the first semiconductor layer on the third trench to form a second trench; wherein the photolithography pattern formed by etching is in a circular ring shape; A source layer is prepared in the second trench; wherein the source layer fills the second trench and covers the Schottky metal layer and the passivation layer.
Citation Information
Patent Citations
Semiconductor device
CN102044565A
High-performance MIS gate enhanced GaN-based high-electron-mobility transistor and preparation method thereof
CN111682064A
Vertical field effect transistor and method for constructing vertical field effect transistor
CN114375499A
Double-groove SiC MOSFET device
CN115528090A
GaN Lateral Vertical HJFET with Source-P Block Contact
US20180219071A1
Cited By
Zinc gallate film prepared by two-step method, and preparation method and application thereof
CN119615360A