Silicon carbide-based integrated polycrystalline heterojunction power device and preparation method thereof

By using polycrystalline heterojunction structures of polysilicon layer and n-type drift layer in silicon carbide-based MOSFET devices and separating polysilicon gates, the problem of gate oxide layer degradation is solved, and the performance and reliability of the device under high temperature and high pressure conditions are improved.

CN118943192APending Publication Date: 2024-11-12HATCHIP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410997295.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The gate oxide layer reliability issues of silicon carbide-based MOSFET devices, especially the time-dependent dielectric breakdown and bias temperature instability effects, lead to a degradation of device performance, limiting its application under high temperature and high pressure conditions.

Method used

Using silicon carbide-based integrated polycrystalline heterojunction structure, the polycrystalline heterojunction between the polycrystalline silicon layer and the gate oxide layer is formed on the n-type drift layer, and a polycrystalline silicon gate and oxide layer with separate structures are arranged on the top to reduce the The on-voltage and protect the gate oxide from drain-mass pulse breakdown.

Benefits of technology

It effectively reduces the on-voltage, protects the gate oxide layer, reduces the gate capacitance, improves the overall performance of the device, and improves its reliability under high temperature and high voltage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943192A_ABST
    Figure CN118943192A_ABST
Patent Text Reader

Abstract

The invention relates to the field of semiconductor devices, and discloses a silicon carbide-based integrated polycrystalline heterojunction power device and a preparation method thereof. The device comprises a back drain metal layer, an n + type silicon carbide substrate and an n type drift layer which are sequentially stacked from bottom to top, two sides of the top of the n-type drift layer are respectively provided with a p-type base region; a p +-type source region and an n +-type source region are wrapped in the p-type base region; a first source electrode metal layer and a second source electrode metal layer are arranged on the two sides of the upper portion of the n-type drift layer respectively, a first gate oxide layer, a polycrystalline silicon layer and a second gate oxide layer are arranged between the first source electrode metal layer and the second source electrode metal layer side by side, the polycrystalline silicon layer is located above the n-type drift layer, and a polycrystalline heterojunction is formed between the polycrystalline silicon layer and the n-type drift layer. A third source electrode metal layer is arranged above the polycrystalline silicon layer; an oxide layer is arranged above the gate oxide layer, and a polysilicon gate is wrapped in the oxide layer. Through the mode, the gate oxide layer can be prevented from being degraded, and the performance of the device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a silicon carbide-based integrated polycrystalline heterojunction power device and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC) is a typical representative of the third generation of semiconductors. Silicon carbide materials have a wide bandgap, high breakdown voltage, high thermal conductivity, high electron saturation rate and other advantages. Therefore, power electronic devices made of silicon carbide materials have higher voltage resistance, current confidentiality and operating frequency. They can work in high frequency and high temperature environments, have high reliability, and are suitable for harsh working environments. Therefore, silicon carbide materials as third generation power electronic devices have become the most important development direction of power electronic technology, and have important application prospects in military and civil fields.

[0003] Metal Oxide Semiconductor Field Effect Transistor (MOSFET) is a voltage-controlled device with the advantages of fast switching speed, good high-frequency performance, low noise, and low driving power. It is a commonly used power switching device. Compared with silicon-based MOSFETs of the same level, silicon carbide-based MOSFETs have the advantages of higher voltage resistance and higher operating temperature due to their material properties. Without the need to introduce complex structural design, they can achieve lower specific on-resistance than silicon-based materials under the same voltage conditions. It is expected to become the most suitable power switching device working under high temperature and high pressure conditions. However, the reliability issues of silicon carbide-based MOSFET devices have also restricted their commercial development and widespread application.

[0004] However, the reliability of silicon carbide-based MOSFET devices, especially the reliability of the gate oxide layer, including the TDDB (Time Dependent Dielectric Breakdown) effect and BTI (Bias Temperature Instability) effect of the gate oxide layer, has restricted the further application and development of the device. Because silicon carbide has a large number of interface state defects in Si / SiO2, under high voltage stress, electrons in SiC can easily pass through the barrier and enter the gate oxide, resulting in severe degradation of the gate oxide layer, affecting the performance of power devices. Summary of the invention

[0005] The present invention provides a silicon carbide-based integrated polycrystalline heterojunction power device and a preparation method thereof, which can avoid the degradation of a gate oxide layer and improve the performance of the device.

[0006] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide a silicon carbide-based integrated polycrystalline heterojunction power device, comprising: a back drain metal layer, an n+ type silicon carbide substrate, and an n-type drift layer stacked in sequence from bottom to top; p-type base regions are respectively arranged on both sides of the top of the n-type drift layer, and a p+ type source region and an n+ type source region are wrapped in the p-type base region, the p+ type source region and the n+ type source region are arranged side by side and the sides are in contact with each other, and the p+ type source region is arranged close to the side of the n-type drift layer; a first source metal layer and a second source metal layer are respectively arranged on both sides above the n-type drift layer, and between the first source metal layer and the second source metal layer A first gate oxide layer, a polysilicon layer and a second gate oxide layer are arranged side by side, the polysilicon layer is located above the n-type drift layer and forms a polycrystalline heterojunction with the n-type drift layer, and a third source metal layer is arranged above the polysilicon layer; a first oxide layer is arranged above the first gate oxide layer, a second oxide layer is arranged above the second gate oxide layer, a first polysilicon gate is wrapped in the first oxide layer, and a second polysilicon gate is wrapped in the second oxide layer; a top metal layer is arranged above the first source metal layer, the first oxide layer, the third source metal layer, the second oxide layer and the second source metal layer, and a passivation layer is arranged above the top metal layer.

[0007] According to one embodiment of the present invention, the depth of the p-type base region is 1.5 μm, and the doping concentration is 1e17 cm -3 ~1e18 cm -3 The depth of the n+ type source region is 0.2 μm, and the doping concentration is greater than 1e19 cm -3 The depth of the p+ source region is 3.0 μm and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

[0008] According to an embodiment of the present invention, the thickness of the first gate oxide layer and the second gate oxide layer are both 500 Å.

[0009] According to an embodiment of the present invention, the thickness of the first polysilicon gate, the second polysilicon gate and the polysilicon layer are all 4000 Å.

[0010] According to an embodiment of the present invention, the thickness of the first oxide layer and the second oxide layer are both 1.0 μm.

[0011] According to one embodiment of the present invention, the passivation layer includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0012] According to an embodiment of the present invention, the thickness of the first source metal layer, the second source metal layer and the third source metal layer are all 1000 Å.

[0013] According to an embodiment of the present invention, the thickness of the top metal layer is 4 μm.

[0014] According to one embodiment of the present invention, the back drain metal layer includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0015] In order to solve the above technical problems, another technical solution adopted by the present invention is: to provide a method for preparing the silicon carbide-based integrated polycrystalline heterojunction power device, comprising:

[0016] Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate;

[0017] Step S2: forming a p-type base region on the n-type drift layer by sequentially growing a first masking layer process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process;

[0018] Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process;

[0019] Step S4: removing the first masking layer by wet method, re-depositing the second masking layers of each layer, and forming a p+ type source region by photolithography, etching and ion implantation;

[0020] Step S5: growing a gate oxide region by a carbon film growth and high temperature activation process and a nitrogen annealing process;

[0021] Step S6: depositing saturated doped polysilicon on the gate oxide region, and forming a first polysilicon gate and a second polysilicon gate separated from each other through photolithography and etching processes;

[0022] Step S7: depositing a layer of borophosphosilicate glass on the first polysilicon gate, the second polysilicon gate and the gate oxide region, and forming a mutually separated first oxide region and a mutually separated first gate oxide layer and a mutually separated second gate oxide layer through an etching process, wherein the first oxide region wraps the first polysilicon gate, and the second oxide region wraps the second polysilicon gate; depositing P-type polysilicon between the first gate oxide layer and the second gate oxide layer, forming a polysilicon layer through an etching process, and then forming a polycrystalline heterojunction between the polysilicon layer and the n-type drift layer through a rapid annealing process;

[0023] Step S8: forming a corresponding first oxide layer and a second oxide layer in the first oxide region and the second oxide region by photolithography and etching processes respectively;

[0024] Step S9: forming a first source metal layer located on one side of the first oxide layer, a second source metal layer located on one side of the second oxide layer, and a third source metal layer located above the polysilicon layer by a metal deposition process and a rapid annealing process on one side of the first oxide layer, one side of the second oxide layer, and above the polysilicon layer;

[0025] Step S10: forming a top metal layer through a sputtering process and an etching process, and depositing a passivation layer on the top metal layer;

[0026] Step S11: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of a silicon carbide-based integrated polycrystalline heterojunction power device.

[0027] The beneficial effects of the present invention are as follows: by forming a polycrystalline heterojunction between the polycrystalline silicon layer and the n-type drift layer, the on-voltage can be reduced when the power device is forward-conducted; when reversely cut off, the polycrystalline heterojunction is reverse-biased, and the polycrystalline silicon layer and the top metal layer can better protect the gate oxide layer from being broken down by a large drain pulse, thereby avoiding the degradation of the gate oxide layer, and the polycrystalline silicon gate with a separated structure can reduce the gate capacitance, thereby improving the performance of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic structural diagram of a silicon carbide-based integrated polycrystalline heterojunction power device according to an embodiment of the present invention;

[0029] Figure 2 It is a schematic flow chart of a method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0030] Figure 3 It is a schematic diagram of the structure formed in step S1 of the method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0031] Figure 4 It is a schematic diagram of the structure formed in step S2 of the method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0032] Figure 5 It is a schematic diagram of the structure formed in step S3 of the method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0033] Figure 6It is a schematic diagram of the structure formed in step S4 of the method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0034] Figure 7 is a schematic diagram of a structure formed in step S5 of a method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0035] Figure 8 is a schematic diagram of a structure formed in step S5 of a method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0036] Fig. 9 is a schematic diagram of a structure formed in step S6 of a method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0037] Fig.10 is a schematic diagram of a structure formed in step S7 of a method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0038] Fig.11 It is a schematic diagram of the structure formed in step S8 of the method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0039] Fig.12 is a schematic diagram of a structure formed in step S9 of a method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0040] Fig.13 It is a schematic diagram of the structure formed in step S10 in the method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0041] Fig.14 It is a schematic diagram of the structure formed in step S10 in the method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention;

[0042] Fig.15 It is a schematic diagram of the structure formed in step S11 of the method for preparing a silicon carbide-based integrated polycrystalline heterojunction power device according to an embodiment of the present invention.

[0043] The meanings of the symbols in the accompanying drawings are:

[0044] 1-back drain metal layer; 2-n+ type silicon carbide substrate; 3-n type drift layer; 4-p type base region; 5-p+ type source region; 6-n+ type source region; 71-first gate oxide layer; 72-second gate oxide layer; 81-first polysilicon gate; 82-second polysilicon gate; 9-polysilicon layer; 10-first oxide layer; 11-second oxide layer; 12-first source metal layer; 13-second source metal layer; 14-third source metal layer; 15-top metal layer; 16-passivation layer; 17-first shielding layer; 18-second shielding layer; 19-carbon film; 70-gate oxide region; 21-first oxide region; 22-second oxide region. DETAILED DESCRIPTION

[0045] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] The terms "first", "second" and "third" in the present invention are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second" and "third" can explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. All directional indications (such as up, down, left, right, front, back...) in the embodiments of the present invention are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.

[0047] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0048] Figure 1Schematic diagram of the structure of a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention. Figure 1 The power device of the silicon carbide-based integrated polycrystalline heterojunction comprises: a back drain metal layer 1, an n+ type silicon carbide substrate 2, and an n-type drift layer 3 which are stacked in sequence from bottom to top; a p-type base region 4 is respectively arranged on both sides of the top of the n-type drift layer 3, a p+ type source region 5 and an n+ type source region 6 are wrapped in the p-type base region 4, the p+ type source region 5 and the n+ type source region 6 are arranged side by side and contact each other on the side, and the p+ type source region 5 is arranged close to the side of the n-type drift layer 3; a first source metal layer 12 and a second source metal layer 13 are respectively arranged on both sides above the n-type drift layer 3, a first gate oxide layer 71, a polysilicon layer 9 and a gate oxide layer 10 are arranged side by side between the first source metal layer 12 and the second source metal layer 13 and a second gate oxide layer 72, the polysilicon layer 9 is located above the n-type drift layer 3 and forms a polycrystalline heterojunction with the n-type drift layer 3, and a third source metal layer 14 is provided above the polysilicon layer 9; a first oxide layer 10 is provided above the first gate oxide layer 71, and a second oxide layer 11 is provided above the second gate oxide layer 72, a first polysilicon gate 81 is wrapped in the first oxide layer 10, and a second polysilicon gate 82 is wrapped in the second oxide layer 11; a top metal layer 15 is provided above the first source metal layer 12, the first oxide layer 10, the third source metal layer 14, the second oxide layer 11 and the second source metal layer 13, and a passivation layer 16 is provided above the top metal layer 15.

[0049] The silicon carbide-based integrated polycrystalline heterojunction power device of the embodiment of the present invention forms a polycrystalline heterojunction between the polycrystalline silicon layer 9 and the n-type drift layer 3, which can reduce the on-voltage when the power device is forward-conducted; when reversely cut off, the polycrystalline heterojunction is reverse biased, and the polycrystalline silicon layer and the top metal layer can better protect the gate oxide layer from being broken down by the drain large pulse, avoiding the degradation of the gate oxide layer, and the polycrystalline silicon gate with a separated structure can reduce the gate capacitance, thereby improving the performance of the device.

[0050] As an embodiment, the thickness of the n+ type silicon carbide substrate 2 is 350 μm, and the doping concentration is greater than 1e19 cm -3 .

[0051] As an embodiment, the thickness of the n-type drift layer 3 is 9.5 μm to 10.5 μm, and the doping concentration is 1e15 cm -3 ~1e16 cm -3 .

[0052] As an embodiment, the depth of the p-type base region 4 is 1.5 μm, and the doping concentration is 1e17 cm -3 ~1e18 cm -3 ; The depth of the n+ source region 6 is 0.2 μm, and the doping concentration is greater than 1e19 cm-3 ; The depth of the p+ source region 5 is 3.0 μm, and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

[0053] As an embodiment, the thickness of the first gate oxide layer 71 and the first gate oxide layer 72 is 500 Å.

[0054] As an embodiment, the thickness of the first polysilicon gate 81, the first polysilicon gate 82 and the polysilicon layer 9 are all 4000 Å.

[0055] As an embodiment, the thickness of the first oxide layer 10 and the second oxide layer 11 are both 1.0 μm.

[0056] As an embodiment, the passivation layer 16 includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0057] As an embodiment, the thickness of the first source metal layer 12 , the second source metal layer 13 and the third source metal layer 14 are all 1000 Å.

[0058] As an embodiment, the thickness of the top metal layer 15 is 4 μm.

[0059] As an embodiment, the back drain metal layer 1 includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0060] Figure 2 FIG. 1 is a schematic flow chart of a method for preparing a power device of a silicon carbide-based integrated polycrystalline heterojunction according to an embodiment of the present invention. It should be noted that if substantially the same results are obtained, the method of the present invention is not limited to Figure 2 The process sequence shown is limited. Figure 2 As shown, the method comprises the steps of:

[0061] Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate.

[0062] In step S1, if Figure 3 As shown, the thickness of the n+ type silicon carbide substrate 2 is 350 μm, and the doping concentration is greater than 1e19 cm -3 The thickness of the n-type drift layer 3 is 9.5 μm to 10.5 μm, and the doping concentration is 1e15 cm -3 ~1e16 cm -3 .

[0063] Step S2: forming a p-type base region on the n-type drift layer by sequentially performing a first masking layer growth process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process.

[0064] In step S2, first, a first masking layer 17 is grown on the cleaned n-type drift layer 3. The first masking layer 17 is a sandwich structure, including a thermal oxide layer with a thickness of 500A, a transition layer with a thickness of 1000A, and a low-pressure tetraethoxy silicate glass layer with a thickness of 2μm, which are arranged in sequence from bottom to top. Among them, the thermal oxide layer is used as a shielding layer during injection, which can effectively avoid injection channel tunneling; the transition layer can connect the thermal oxide layer and the low-pressure tetraethoxy silicate glass layer, and the endpoint detection signal is strong during etching. Then, after high-temperature densification, photolithography patterning, photoresist coating, exposure and development are carried out. The thickness of the photoresist is 2μm, the side wall is smooth, and the side wall angle is greater than 88±2°. Next, the etching process is carried out. The etching is carried out using an ICP (Inductive Coupled Plasma) or TCP (Transformer Coupled Plasma) dry etching machine with better anisotropy. First, the top low-pressure tetraethoxysilicate glass layer is etched for 2μm, and the end point is stopped at the transition layer. After the over-etching is completed, the etching is switched to the transition layer, and the end point is stopped at the thermal oxide layer. Finally, the photoresist is removed and cleaned to prepare for ion implantation. Aluminum is injected at high energy at a high temperature of 500°C. The injection is divided into multiple times. Generally, 3 to 5 injections are required, and the injection angle is 0°. For example, taking 5 injections as an example, the energy of the first injection is 30kev, and the dose is 5e15 cm -2 The second implantation energy is 100keV and the dose is 5e13 cm -2 The third injection energy is 250kev and the dose is 5e13cm -2 The fourth injection energy is 350kev and the dose is 5e14 cm -2 The fifth injection energy is 500kev and the dose is 5e15cm -2 , forming a depth of about 1.5 μm and a doping concentration of 1e17 cm -3 ~1e18cm -3 The p-type base region 4, such as Figure 4 shown.

[0065] Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process.

[0066] In step S3, a low-pressure tetraethoxy silicate glass with a thickness of about 5 kA is grown using the first masking layer 17, and a 0.5 μm conductive channel is formed by plasma dry isotropic etching and self-alignment process. Then, nitrogen is injected at a high temperature of 500°C, and the injection is performed in multiple times, generally 3 to 5 times, with an injection angle of 0°. For example, taking 4 injections as an example, the first injection energy is 20 kev and the dose is 5e14 cm -2 The second implantation energy is 40keV and the dose is 5e14 cm -2 The third injection energy is 60keV and the dose is 5e14 cm -2 The fourth injection energy is 100keV and the dose is 8e13 cm -2 , with a depth of 0.2 μm and a doping concentration greater than 1e19 cm -3 The n+ type source region 6, such as Figure 5 shown.

[0067] Step S4: removing the first masking layer by wet method, re-depositing the second masking layer of each layer, and forming a p+ type source region by photolithography, etching and ion implantation.

[0068] In step S4, the first masking layer 17 is removed by wet method, and the second masking layer 18 of each layer is re-deposited, and photolithography patterning, photoresist coating, exposure and development are performed in sequence, and the second masking layer is etched, and P-type ion implantation is performed after the photoresist is removed. Aluminum is implanted at high energy at a high temperature of 500°C, and the implantation is performed in multiple times. Generally, 4 to 7 implantations are required, and the implantation angle is 0°. For example, taking 7 implantations as an example, the first implantation energy is 30kev and the dose is 5e15cm -2 The second implantation energy is 100keV and the dose is 5e14 cm -2 The third implantation energy is 250kev and the dose is 5e14 cm -2 The fourth injection energy is 350kev and the dose is 5e14 cm -2 The fifth injection energy is 500kev and the dose is 5e15cm -2 The sixth injection energy is 600kev and the dose is 5e14 cm -2 The seventh injection energy is 700kev and the dose is 5e13 cm -2 , forming a depth of about 3.0 μm and a doping concentration of 1e18 cm -3 ~1e19 cm -3 The p+ type source region 5, such as Figure 6 shown.

[0069] Step S5: growing a gate oxide region through a carbon film growth and high temperature activation process and a nitrogen annealing process.

[0070] In step S5, a carbon film 19 is sputtered in a metal sputtering chamber, and then activated in a high temperature furnace at 1650° C. for 30 min, and finally the carbon film 19 is removed by sulfuric acid. Figure 7 As shown. A nitrogen annealing process is added before growing the gate oxide region 70. During the nitrogen annealing process, a sandwich annealing process with NO / O2 / NO is used. Specifically, before thermal oxidation, the sample surface is treated with a gas with a NO content of 2% for 1 hour, and then thermal oxidation is performed in a gas with an O2 content of 5% to grow a gate oxide region 70 with a thickness of 500A. Finally, the sample is thermally annealed with a gas with a NO content of 2% for 1 hour. The temperature is controlled at 1250°C throughout the process, and the following is obtained. Figure 8 A gate oxide region 70 is shown.

[0071] Step S6: depositing saturated doped polysilicon on the gate oxide region, and forming a first polysilicon gate and a second polysilicon gate separated from each other through photolithography and etching processes.

[0072] In step S6, first, saturated doped polysilicon with a thickness of about 4000A is deposited in a low-temperature furnace tube, and the polysilicon is photoetched to form a first polysilicon gate 81 and a second polysilicon gate 82 separated from each other. Fig. 9 shown.

[0073] Step S7: depositing a layer of borophosphosilicate glass on the first polysilicon gate, the second polysilicon gate and the gate oxide region, and forming mutually separated first oxide region and second oxide region and mutually separated first gate oxide layer and second gate oxide layer through an etching process, wherein the first oxide region wraps the first polysilicon gate, and the second oxide region wraps the second polysilicon gate; depositing P-type polysilicon between the first gate oxide layer and the second gate oxide layer, forming a polysilicon layer through an etching process, and then forming a polycrystalline heterojunction between the polysilicon layer and the n-type drift layer through a rapid annealing process.

[0074] In step S7, a layer of borophosphosilicate glass with a thickness of 1 μm is first deposited as a dielectric isolation layer, and a first oxide region 21 and a second oxide region 22 separated from each other and a first gate oxide layer 71 and a second gate oxide layer 72 separated from each other are formed by an etching process, the first oxide region 21 wraps the first polysilicon gate 81, and the second oxide region 22 wraps the second polysilicon gate 82. P-type polysilicon is deposited between the first gate oxide layer 71 and the second gate oxide layer 72, and a polysilicon layer 9 is formed by an etching process, and then a polycrystalline heterojunction is formed between the polysilicon layer 9 and the n-type drift layer 3 by a rapid annealing process, such as Fig.10 shown.

[0075] Step S8: forming corresponding first oxide layers and second oxide layers in the first oxide region and the second oxide region through photolithography and etching processes respectively.

[0076] In step S8, the pattern is exposed by using the photomask of the ohmic contact hole, and then the borophosphosilicate glass of the two oxidation regions 20 is dry-etched to serve as the ohmic contact hole, and the first oxide layer 10 and the second oxide layer 11 are formed, as shown in FIG. Fig.11 shown.

[0077] Step S9: On one side of the first oxide layer, on one side of the second oxide layer and above the polysilicon layer, a first source metal layer located on one side of the first oxide layer, a second source metal layer located on one side of the second oxide layer, and a third source metal layer located above the polysilicon layer are formed by a metal deposition process and a rapid annealing process.

[0078] In step S9, a nickel metal layer with a thickness of 1000 Å is deposited on the side of the first oxide layer 10 away from the polysilicon layer 9 and on the side of the second oxide layer 11 away from the polysilicon layer 9, and a nickel metal layer is deposited on the polysilicon layer 9, and a rapid annealing is performed at 500° C. to 700° C. for 60 seconds to form a layer of Ni x Si y The nickel without alloy layer on the dielectric SiO2 is removed by etching solution, and finally rapid annealing is performed at 980℃ for 60 seconds to make Ni x Si y The alloy layer becomes a high temperature alloy to form a good ohmic contact, that is, the first source metal layer 12, the second source metal layer 13 and the third source metal layer 14, such as Fig.12 shown.

[0079] Step S10: forming a top metal layer through a sputtering process and an etching process, and depositing a passivation layer on the top metal layer.

[0080] In step S10, a layer of titanium aluminum metal with a thickness of 4 μm is sputtered on the first source metal layer 12, the first oxide layer 10, the third source metal layer 13, the second oxide layer 11 and the second source metal layer 13, and the gate and the source are isolated by metal etching to form a top metal layer 15, such as Fig.13 A passivation layer 16 is deposited on the top metal layer 15, as shown. Fig.14 The passivation layer 16 includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0081] Step S11: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of a silicon carbide-based integrated polycrystalline heterojunction power device.

[0082] In step S11, a blue film is attached to the front side of the n+ type silicon carbide substrate 2, and the back side is thinned to 100 μm. Then, the blue film is removed, cleaned, titanium is evaporated on the back side, and an ohmic contact is made by laser annealing to form a back drain metal layer 1, thereby completing the preparation of a silicon carbide-based integrated polycrystalline heterojunction power device. Fig.15 As shown, the back drain metal layer 1 includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0083] The method for preparing a power device with a silicon carbide-based integrated polycrystalline heterojunction in an embodiment of the present invention forms a polycrystalline heterojunction between the polycrystalline silicon layer 9 and the n-type drift layer 3, which can reduce the on-voltage when the power device is forward-conducted; when reversely cut off, the polycrystalline heterojunction is reverse-biased, and the polycrystalline silicon layer and the top metal layer can better protect the gate oxide layer from being broken down by a large drain pulse, thereby avoiding the degradation of the gate oxide layer, and the polycrystalline silicon gate with a separated structure can reduce the gate capacitance, thereby improving the performance of the device.

[0084] The above are only implementation modes of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A silicon carbide-based integrated polycrystalline heterojunction power device, It is characterized in that The invention comprises a back drain metal layer, an n+ type silicon carbide substrate, and an n-type drift layer which are stacked in sequence from bottom to top; a p-type base region is respectively arranged on both sides of the top of the n-type drift layer, a p+ type source region and an n+ type source region are wrapped in the p-type base region, the p+ type source region and the n+ type source region are arranged side by side and the sides are in contact with each other, and the p+ type source region is arranged close to the side of the n-type drift layer; a first source metal layer and a second source metal layer are respectively arranged on both sides above the n-type drift layer, and a first gate oxide layer, a polysilicon layer, and a second gate oxide layer are arranged side by side between the first source metal layer and the second source metal layer The polysilicon layer is located above the n-type drift layer and forms a polycrystalline heterojunction with the n-type drift layer. A third source metal layer is provided above the polysilicon layer; a first oxide layer is provided above the first gate oxide layer, and a second oxide layer is provided above the second gate oxide layer. A first polysilicon gate is wrapped in the first oxide layer, and a second polysilicon gate is wrapped in the second oxide layer; a top metal layer is provided above the first source metal layer, the first oxide layer, the third source metal layer, the second oxide layer, and the second source metal layer, and a passivation layer is provided above the top metal layer.

2. The silicon carbide-based integrated polycrystalline heterojunction power device according to claim 1, It is characterized in that The depth of the p-type base region is 1.5 μm and the doping concentration is 1e17 cm -3 ~1e18 cm -3 The depth of the n+ source region is 0.2 μm, and the doping concentration is greater than 1e19 cm -3 The depth of the p+ source region is 3.0 μm and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

3. The silicon carbide-based integrated polycrystalline heterojunction power device according to claim 1, It is characterized in that The thickness of the first gate oxide layer and the second gate oxide layer are both 500 Å.

4. The silicon carbide-based integrated polycrystalline heterojunction power device according to claim 1, It is characterized in that The thickness of the first polysilicon gate, the second polysilicon gate and the polysilicon layer are all 4000 Å.

5. The silicon carbide-based integrated polycrystalline heterojunction power device according to claim 1, It is characterized in that The thickness of the first oxide layer and the second oxide layer are both 1.0 μm.

6. The silicon carbide-based integrated polycrystalline heterojunction power device according to claim 1, It is characterized in that The passivation layer includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

7. The silicon carbide-based integrated polycrystalline heterojunction power device according to claim 1, It is characterized in that The thickness of the first source metal layer, the second source metal layer and the third source metal layer are all 1000 Å.

8. The silicon carbide-based integrated polycrystalline heterojunction power device according to claim 1, It is characterized in that The thickness of the top metal layer is 4 μm.

9. The silicon carbide-based integrated polycrystalline heterojunction power device according to claim 1, It is characterized in that The back drain metal layer includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

10. A method for preparing a silicon carbide-based integrated polycrystalline heterojunction power device according to any one of claims 1 to 9, include: Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate; Step S2: forming a p-type base region on the n-type drift layer by sequentially growing a first masking layer process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process; Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process; Step S4: removing the first masking layer by wet method, re-depositing the second masking layers of each layer, and forming a p+ type source region by photolithography, etching and ion implantation; Step S5: growing a gate oxide region by a carbon film growth and high temperature activation process and a nitrogen annealing process; Step S6: depositing saturated doped polysilicon on the gate oxide region, and forming two first polysilicon gates and a second polysilicon gate separated from each other through photolithography and etching processes; Step S7: depositing a layer of borophosphosilicate glass on the first polysilicon gate, the second polysilicon gate and the gate oxide region, and forming a mutually separated first oxide region and a mutually separated first gate oxide layer and a mutually separated second gate oxide layer through an etching process, wherein the first oxide region wraps the first polysilicon gate, and the second oxide region wraps the second polysilicon gate; depositing P-type polysilicon between the first gate oxide layer and the second gate oxide layer, forming a polysilicon layer through an etching process, and then forming a polycrystalline heterojunction between the polysilicon layer and the n-type drift layer through a rapid annealing process; Step S8: forming a corresponding first oxide layer and a second oxide layer in the first oxide region and the second oxide region by photolithography and etching processes respectively; Step S9: forming a first source metal layer located on one side of the first oxide layer, a second source metal layer located on one side of the second oxide layer, and a third source metal layer located above the polysilicon layer by a metal deposition process and a rapid annealing process on one side of the first oxide layer, one side of the second oxide layer, and above the polysilicon layer; Step S10: forming a top metal layer through a sputtering process and an etching process, and depositing a passivation layer on the top metal layer; Step S11: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of a silicon carbide-based integrated polycrystalline heterojunction power device.

Citation Information

Patent Citations

  • Silicon carbide power device, preparation method thereof and chip

    CN116994956A

  • Silicon carbide power device and manufacturing method thereof

    CN117690969A

  • Upper and lower split-gate silicon carbide field effect transistor structure and manufacturing method thereof

    CN118198134A

  • Metal-oxide semiconductor field effect transistor device and manufacturing method therefor