Silicon carbide-based integrated Schottky power device and preparation method thereof

By designing a polysilicon gate with contact and separation structure between the Schottky metal layer and the n-type drift layer in a silicon carbide-based integrated Schottky power device, the gate oxide layer reliability problem of the silicon carbide-based MOSFET device is solved, and the conduction is reduced. The on-voltage and high-frequency power consumption improve the performance of the device.

CN118943193APending Publication Date: 2024-11-12HATCHIP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410997348.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The gate oxide layer reliability issues of silicon carbide-based MOSFET devices, especially the time-dependent dielectric breakdown and bias temperature instability effects, lead to degradation of device performance, limiting its application in high-temperature and high-pressure environments.

Method used

A silicon carbide-based integrated Schottky power device is designed. By forming Schottky contact between Schottky metal layer and n-type drift layer, and using a separate structure of polysilicon gate, the gate capacitance is reduced and high-frequency power consumption is reduced. . The method of preparing the device includes epitaxially growing an n-type drift layer on an n+ type silicon carbide substrate, forming a p-type base region and a source region, growing the first and second oxide layers, forming a Schottky metal layer, and setting it on top Passivation layer ensures the structural stability of the device.

Benefits of technology

Through the contact between the Schottky metal layer and the n-type drift layer, the on-voltage is reduced and the gate oxide layer is avoided. The polysilicon gate of the separated structure reduces the gate capacitance, reduces the high-frequency power consumption of the device, and improves the overall performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943193A_ABST
    Figure CN118943193A_ABST
Patent Text Reader

Abstract

The invention relates to the field of semiconductor devices, and discloses a silicon carbide-based integrated Schottky power device and a preparation method thereof. The device comprises a back drain metal layer, an n + type silicon carbide substrate and an n type drift layer which are sequentially stacked from bottom to top, two sides of the top of the n-type drift layer are respectively provided with a p-type base region; a p +-type source region and an n +-type source region are wrapped in the p-type base region; a first source metal layer, a first oxide layer, a Schottky metal layer, a second oxide layer and a second source metal layer are sequentially arranged above the n-type drift layer from left to right, Schottky contact is formed between the Schottky metal layer and the n-type drift layer, and polysilicon gates are wrapped in the first oxide layer and the second oxide layer; and gate oxide layers adjacent to the polysilicon gate are correspondingly arranged below the first oxide layer and the second oxide layer. In this way, the gate oxide layer can be prevented from being degraded, and the performance of the device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a silicon carbide-based integrated Schottky power device and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC) is a typical representative of the third generation of semiconductors. Silicon carbide materials have a wide bandgap, high breakdown voltage, high thermal conductivity, high electron saturation rate and other advantages. Therefore, power electronic devices made of silicon carbide materials have higher voltage resistance, current confidentiality and operating frequency. They can work in high frequency and high temperature environments, have high reliability, and are suitable for harsh working environments. Therefore, silicon carbide materials as third generation power electronic devices have become the most important development direction of power electronic technology, and have important application prospects in military and civil fields.

[0003] Metal Oxide Semiconductor Field Effect Transistor (MOSFET) is a voltage-controlled device with the advantages of fast switching speed, good high-frequency performance, low noise, and low driving power. It is a commonly used power switching device. Compared with silicon-based MOSFETs of the same level, silicon carbide-based MOSFETs have the advantages of higher voltage resistance and higher operating temperature due to their material properties. Without the need to introduce complex structural design, they can achieve lower specific on-resistance than silicon-based materials under the same voltage conditions. It is expected to become the most suitable power switching device working under high temperature and high pressure conditions. However, the reliability issues of silicon carbide-based MOSFET devices have also restricted their commercial development and widespread application.

[0004] However, the reliability of silicon carbide-based MOSFET devices, especially the reliability of the gate oxide layer, including the TDDB (Time Dependent Dielectric Breakdown) effect and BTI (Bias Temperature Instability) effect of the gate oxide layer, has restricted the further application and development of the device. Because silicon carbide has a large number of interface state defects in Si / SiO2, under high voltage stress, electrons in SiC can easily pass through the barrier and enter the gate oxide, resulting in severe degradation of the gate oxide layer, affecting the performance of power devices. Summary of the invention

[0005] The present invention provides a silicon carbide-based integrated Schottky power device and a preparation method thereof, which can avoid the degradation of a gate oxide layer and improve the performance of the device.

[0006] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide a silicon carbide-based integrated Schottky power device, comprising: a back drain metal layer, an n+ type silicon carbide substrate, and an n-type drift layer stacked in sequence from bottom to top; p-type base regions are respectively arranged on both sides of the top of the n-type drift layer, and a p+ type source region and an n+ type source region are wrapped in the p-type base region. The p+ type source region and the n+ type source region are arranged side by side and the sides are in contact with each other, and the p+ type source region is arranged close to the side of the n-type drift layer; a first source metal layer, a first oxide layer, a Schottky metal layer, a second oxide layer are arranged in sequence from left to right above the n-type drift layer. A Schottky metal layer and a second source metal layer are provided, a Schottky contact is formed between the Schottky metal layer and the n-type drift layer, a polysilicon gate is wrapped in the first oxide layer and the second oxide layer, a gate oxide layer adjacent to the polysilicon gate is provided below the first oxide layer and the second oxide layer, the gate oxide layer is provided above the n-type drift layer, and the polysilicon gate is provided on a side of the gate oxide layer away from the n-type drift layer; a top metal layer is provided above the first source metal layer, the first oxide layer, the Schottky metal layer, the second oxide layer and the second source metal layer, and a passivation layer is provided above the top metal layer.

[0007] According to one embodiment of the present invention, the depth of the p-type base region is 1.5 μm, and the doping concentration is 1e17 cm -3 ~1e18 cm -3 The depth of the n+ type source region is 0.2 μm, and the doping concentration is greater than 1e19 cm -3 The depth of the p+ source region is 3.0 μm and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

[0008] According to one embodiment of the present invention, the thickness of the Schottky metal layer is 1000 Å.

[0009] According to an embodiment of the present invention, the thickness of the gate oxide layer is 500A; the thickness of the polysilicon gate is 4000A.

[0010] According to an embodiment of the present invention, the thickness of the first oxide layer and the second oxide layer are both 1.0 μm.

[0011] According to one embodiment of the present invention, the passivation layer includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0012] According to an embodiment of the present invention, the thickness of the first source metal layer and the second source metal layer are both 1000 Å.

[0013] According to an embodiment of the present invention, the thickness of the top metal layer is 4 μm.

[0014] According to one embodiment of the present invention, the back drain metal layer includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0015] In order to solve the above technical problems, another technical solution adopted by the present invention is: to provide a method for preparing the silicon carbide-based integrated Schottky power device, comprising:

[0016] Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate;

[0017] Step S2: forming a p-type base region on the n-type drift layer by sequentially growing a first masking layer process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process;

[0018] Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process;

[0019] Step S4: removing the first masking layer by wet method, re-depositing the second masking layers of each layer, and forming a p+ type source region by photolithography, etching and ion implantation;

[0020] Step S5: growing a gate oxide layer through a carbon film growth and high temperature activation process and a nitrogen annealing process;

[0021] Step S6: depositing saturated doped polysilicon on the gate oxide layer, and forming two mutually separated polysilicon gates through photolithography and etching processes;

[0022] Step S7: depositing a layer of borophosphosilicate glass on the polysilicon gate and the gate oxide layer, and forming an oxidation region by photolithography and etching, wherein the oxidation region wraps the two polysilicon gates;

[0023] Step S8: forming a first source metal layer and a second source metal layer on both sides of the oxidation region by a metal deposition process and a rapid annealing process;

[0024] Step S9: forming a first oxide layer and a second oxide layer separated from each other and a Schottky filling region located between the first oxide layer and the second oxide layer in the oxide region by a dry etching process, depositing a layer of metal titanium in the Schottky filling region, and forming a Schottky metal layer by an annealing process;

[0025] Step S10: forming a top metal layer on the first source metal layer, the first oxide layer, the Schottky metal layer, the second oxide layer and the second source metal layer by a sputtering process and an etching process, and depositing a passivation layer on the top metal layer;

[0026] Step S11: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of a silicon carbide-based integrated Schottky power device.

[0027] The beneficial effects of the present invention are as follows: by forming a Schottky contact between the Schottky metal layer and the n-type drift layer, the on-voltage can be reduced when the power device is forward-conducted; in the reverse bias, the degradation of the gate oxide layer can be avoided, and the polysilicon gate with a separated structure can reduce the gate capacitance and reduce the high-frequency power consumption of the device, thereby improving the performance of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic structural diagram of a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention;

[0029] Figure 2 It is a schematic flow chart of a method for preparing a power device of a silicon carbide-based integrated Schottky device according to an embodiment of the present invention;

[0030] Figure 3 Schematic diagram of the structure formed in step S1 of the method for preparing a power device of a silicon carbide-based integrated Schottky device according to an embodiment of the present invention;

[0031] Figure 4 Schematic diagram of the structure formed in step S2 of the method for preparing a power device of a silicon carbide-based integrated Schottky device according to an embodiment of the present invention;

[0032] Figure 5 Schematic diagram of the structure formed in step S3 of the method for preparing a power device of a silicon carbide-based integrated Schottky device according to an embodiment of the present invention;

[0033] Figure 6 is a schematic diagram of a structure formed in step S4 in the method for preparing a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention;

[0034] Figure 7 is a schematic diagram of the structure formed in step S5 in the method for preparing a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention;

[0035] Figure 8 is a schematic diagram of the structure formed in step S5 in the method for preparing a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention;

[0036] Fig. 9 is a schematic diagram of a structure formed in step S6 in the method for preparing a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention;

[0037] Fig.10 is a schematic diagram of the structure formed in step S7 of the method for preparing a power device of a silicon carbide-based integrated Schottky device according to an embodiment of the present invention;

[0038] Fig.11 is a schematic diagram of a structure formed in step S8 in the method for preparing a power device of a silicon carbide-based integrated Schottky device according to an embodiment of the present invention;

[0039] Fig.12 is a schematic diagram of a structure formed in step S9 in the method for preparing a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention;

[0040] Fig.13 is a schematic diagram of a structure formed in step S10 in the method for preparing a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention;

[0041] Fig.14 is a schematic diagram of a structure formed in step S10 in the method for preparing a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention;

[0042] Fig.15 It is a schematic diagram of the structure formed in step S11 of the method for preparing a silicon carbide-based integrated Schottky power device according to an embodiment of the present invention.

[0043] The meanings of the symbols in the accompanying drawings are:

[0044] 1-back drain metal layer; 2-n+ type silicon carbide substrate; 3-n type drift layer; 4-p type base region; 5-p+ type source region; 6-n+ type source region; 7-gate oxide layer; 8-polysilicon gate; 9-Schottky metal layer; 10-first oxide layer; 11-second oxide layer; 12-first source metal layer; 13-second source metal layer; 15-top metal layer; 16-passivation layer; 17-first masking layer; 18-second masking layer; 19-carbon film; 20-oxidation region. DETAILED DESCRIPTION

[0045] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] The terms "first", "second" and "third" in the present invention are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second" and "third" can explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. All directional indications (such as up, down, left, right, front, back...) in the embodiments of the present invention are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.

[0047] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0048] Figure 1 Schematic diagram of the structure of a power device of a silicon carbide-based integrated Schottky device according to an embodiment of the present invention. Figure 1The silicon carbide-based integrated Schottky power device comprises: a back drain metal layer 1, an n+ type silicon carbide substrate 2, and an n-type drift layer 3 are stacked in sequence from bottom to top; p-type base regions 4 are respectively arranged on both sides of the top of the n-type drift layer 3, and a p+ type source region 5 and an n+ type source region 6 are wrapped in the p-type base region 4. The p+ type source region 5 and the n+ type source region 6 are arranged side by side and contact each other on the side, and the p+ type source region 5 is arranged close to the side of the n-type drift layer 3; a first source metal layer 12, a first oxide layer 10, a Schottky metal layer 9, a second oxide layer 11, and a second source metal layer 12 are arranged in sequence from left to right above the n-type drift layer 3. 13, a Schottky contact is formed between the Schottky metal layer 9 and the n-type drift layer 3, the first oxide layer 10 and the second oxide layer 11 are both wrapped with a polysilicon gate 8, a gate oxide layer 7 adjacent to the polysilicon gate 8 is correspondingly provided below the first oxide layer 10 and the second oxide layer 11, the gate oxide layer 7 is provided above the n-type drift layer 3, and the polysilicon gate 8 is provided on a side of the gate oxide layer 7 away from the n-type drift layer 3; a top metal layer 15 is provided above the first source metal layer 12, the first oxide layer 10, the Schottky metal layer 9, the second oxide layer 11 and the second source metal layer 13, and a passivation layer 16 is provided above the top metal layer 15.

[0049] The silicon carbide-based integrated Schottky power device of the embodiment of the present invention forms a Schottky contact between the Schottky metal layer 9 and the n-type drift layer 3, which can reduce the on-voltage when the power device is forward-biased; reverse bias can avoid degradation of the gate oxide layer 7, and the polysilicon gate 8 with a separated structure can reduce the gate capacitance and reduce the high-frequency power consumption of the device, thereby improving the performance of the device.

[0050] As an embodiment, the thickness of the n+ type silicon carbide substrate 2 is 350 μm, and the doping concentration is greater than 1e19 cm -3 .

[0051] As an embodiment, the thickness of the n-type drift layer 3 is 9.5 μm to 10.5 μm, and the doping concentration is 1e15 cm -3 ~1e16 cm -3 .

[0052] As an embodiment, the depth of the p-type base region 4 is 1.5 μm, and the doping concentration is 1e17 cm -3 ~1e18 cm -3 ; The depth of the n+ source region 6 is 0.2 μm, and the doping concentration is greater than 1e19 cm -3 ; The depth of the p+ source region 5 is 3.0 μm, and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

[0053] As an embodiment, the thickness of the Schottky metal layer is 1000 Å.

[0054] As an embodiment, the thickness of the gate oxide layer 7 is 500 Å.

[0055] As an embodiment, the thickness of the polysilicon gate 8 is 4000 Å.

[0056] As an embodiment, the thickness of the first oxide layer 10 and the second oxide layer 11 are both 1.0 μm.

[0057] As an embodiment, the passivation layer 16 includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0058] As an embodiment, the thickness of the first source metal layer 12 and the second source metal layer 13 are both 1000 Å.

[0059] As an embodiment, the thickness of the top metal layer 15 is 4 μm.

[0060] As an embodiment, the back drain metal layer 1 includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0061] Figure 2 FIG. 1 is a flow chart of a method for preparing a power device of a silicon carbide-based integrated Schottky device according to an embodiment of the present invention. It should be noted that if substantially the same results are obtained, the method of the present invention is not limited to Figure 2 The process sequence shown is limited. Figure 2 As shown, the method comprises the steps of:

[0062] Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate.

[0063] In step S1, if Figure 3 As shown, the thickness of the n+ type silicon carbide substrate 2 is 350 μm, and the doping concentration is greater than 1e19 cm -3 The thickness of the n-type drift layer 3 is 9.5 μm to 10.5 μm, and the doping concentration is 1e15 cm -3 ~1e16 cm -3 .

[0064] Step S2: forming a p-type base region on the n-type drift layer by sequentially performing a first masking layer growth process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process.

[0065] In step S2, first, a first masking layer 17 is grown on the cleaned n-type drift layer 3. The first masking layer 17 is a sandwich structure, including a thermal oxide layer with a thickness of 500A, a transition layer with a thickness of 1000A, and a low-pressure tetraethoxy silicate glass layer with a thickness of 2μm, which are arranged in sequence from bottom to top. Among them, the thermal oxide layer is used as a shielding layer during injection, which can effectively avoid injection channel tunneling; the transition layer can connect the thermal oxide layer and the low-pressure tetraethoxy silicate glass layer, and the endpoint detection signal is strong during etching. Then, after high-temperature densification, photolithography patterning, photoresist coating, exposure and development are carried out. The thickness of the photoresist is 2μm, the side wall is smooth, and the side wall angle is greater than 88±2°. Next, the etching process is carried out. The etching is carried out using an ICP (Inductive Coupled Plasma) or TCP (Transformer Coupled Plasma) dry etching machine with better anisotropy. First, the top low-pressure tetraethoxysilicate glass layer is etched for 2μm, and the end point is stopped at the transition layer. After the over-etching is completed, the etching is switched to the transition layer, and the end point is stopped at the thermal oxide layer. Finally, the photoresist is removed and cleaned to prepare for ion implantation. Aluminum is injected at high energy at a high temperature of 500°C. The injection is divided into multiple times. Generally, 3 to 5 injections are required, and the injection angle is 0°. For example, taking 5 injections as an example, the energy of the first injection is 30kev, and the dose is 5e15 cm -2 The second implantation energy is 100keV and the dose is 5e13 cm -2 The third injection energy is 250kev and the dose is 5e13cm -2 The fourth injection energy is 350kev and the dose is 5e14 cm -2 The fifth injection energy is 500kev and the dose is 5e15cm -2 , forming a depth of about 1.5 μm and a doping concentration of 1e17 cm -3 ~1e18cm -3 The p-type base region 4, such as Figure 4 shown.

[0066] Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process.

[0067] In step S3, a low-pressure tetraethoxy silicate glass with a thickness of about 5 kA is grown using the first masking layer 17, and a 0.5 μm conductive channel is formed by plasma dry isotropic etching and self-alignment process. Then, nitrogen is injected at a high temperature of 500°C, and the injection is performed in multiple times, generally 3 to 5 times, with an injection angle of 0°. For example, taking 4 injections as an example, the first injection energy is 20 kev and the dose is 5e14 cm -2 The second implantation energy is 40keV and the dose is 5e14 cm -2 The third injection energy is 60keV and the dose is 5e14 cm -2 The fourth injection energy is 100keV and the dose is 8e13 cm -2 , with a depth of 0.2 μm and a doping concentration greater than 1e19 cm -3 The n+ type source region 6, such as Figure 5 shown.

[0068] Step S4: removing the first masking layer by wet method, re-depositing the second masking layer of each layer, and forming a p+ type source region by photolithography, etching and ion implantation.

[0069] In step S4, the first masking layer 17 is removed by wet method, and the second masking layer 18 of each layer is re-deposited, and photolithography patterning, photoresist coating, exposure and development are performed in sequence, and the second masking layer is etched, and P-type ion implantation is performed after the photoresist is removed. Aluminum is implanted at high energy at a high temperature of 500°C, and the implantation is performed in multiple times. Generally, 4 to 7 implantations are required, and the implantation angle is 0°. For example, taking 7 implantations as an example, the first implantation energy is 30kev and the dose is 5e15cm -2 The second implantation energy is 100keV and the dose is 5e14 cm -2 The third implantation energy is 250kev and the dose is 5e14 cm -2 The fourth injection energy is 350kev and the dose is 5e14 cm -2 The fifth injection energy is 500kev and the dose is 5e15cm -2 The sixth injection energy is 600kev and the dose is 5e14 cm -2 The seventh injection energy is 700kev and the dose is 5e13 cm -2 , forming a depth of about 3.0 μm and a doping concentration of 1e18 cm -3 ~1e19 cm -3 The p+ type source region 5, such as Figure 6 shown.

[0070] Step S5: growing a gate oxide layer through a carbon film growth and high temperature activation process and a nitrogen annealing process.

[0071] In step S5, a carbon film 19 is sputtered in a metal sputtering chamber, and then activated in a high temperature furnace at 1650° C. for 30 min, and finally the carbon film 19 is removed by sulfuric acid. Figure 7 As shown. A nitrogen annealing process is added before growing the gate oxide layer 7. During the nitrogen annealing process, a sandwich annealing process with NO / O2 / NO is used. Specifically, before thermal oxidation, the sample surface is treated with a gas with a NO content of 2% for 1 hour, and then thermal oxidation is performed in a gas with an O2 content of 5% to grow a gate oxide layer 7 with a thickness of 500A. Finally, the sample is thermally annealed with a gas with a NO content of 2% for 1 hour. The temperature is controlled at 1250°C throughout the process, and the following is obtained. Figure 8 The gate oxide layer 7 is shown.

[0072] Step S6: depositing saturated doped polysilicon on the gate oxide layer, and forming two mutually separated polysilicon gates through photolithography and etching processes.

[0073] In step S6, firstly, saturated doped polysilicon with a thickness of about 4000A is deposited in a low temperature furnace tube, and then the polysilicon is photoetched to form two mutually separated polysilicon gates 8, such as Fig. 9 shown.

[0074] Step S7: depositing a layer of borophosphosilicate glass on the polysilicon gate and the gate oxide layer, and forming an oxidation region through photolithography and etching processes, wherein the oxidation region wraps the two polysilicon gates.

[0075] In step S7, a layer of borophosphosilicate glass with a thickness of 1 μm is first deposited as a dielectric isolation layer, a pattern is exposed using a photomask of an ohmic contact hole, and then the borophosphosilicate glass is dry-etched as an ohmic contact hole to form an oxidation region 20, such as Fig.10 shown.

[0076] Step S8: forming a first source metal layer and a second source metal layer on both sides of the oxidation region by a metal deposition process and a rapid annealing process.

[0077] In step S8, a nickel metal layer with a thickness of 1000A is deposited on both sides of the oxidation region 20, and a rapid annealing is performed at 500°C to 700°C for 60 seconds to form a layer of Ni x Si y The nickel without alloy layer on the dielectric SiO2 is removed by etching solution, and finally rapid annealing is performed at 980℃ for 60 seconds to make Ni x Si y The alloy layer becomes a high temperature alloy to form a good ohmic contact, that is, the first source metal layer 12 and the second source metal layer 13, such as Fig.11 shown.

[0078] Step S9: forming a first oxide layer and a second oxide layer separated from each other and a Schottky filling area between the first oxide layer and the second oxide layer in the oxide area by a dry etching process, depositing a layer of metal titanium in the Schottky filling area, and forming a Schottky metal layer by an annealing process.

[0079] In step S9, the annealing temperature is 500°C, the annealing time is 1 minute, and the thickness of the Schottky metal layer is 1000 Å. Fig.12 shown.

[0080] Step S10: forming a top metal layer on the first source metal layer, the first oxide layer, the Schottky metal layer, the second oxide layer and the second source metal layer by sputtering and etching processes, and depositing a passivation layer on the top metal layer.

[0081] In step S10, a layer of titanium aluminum metal with a thickness of 4 μm is sputtered on the first source metal layer 12, the first oxide layer 10, the Schottky metal layer 9, the second oxide layer 11 and the second source metal layer 13, and the gate and the source are isolated by metal etching to form a top metal layer 15, such as Fig.13 A passivation layer 16 is deposited on the top metal layer 15, as shown. Fig.14 The passivation layer 16 includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

[0082] Step S11: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of a silicon carbide-based integrated Schottky power device.

[0083] In step S11, a blue film is attached to the front side of the n+ type silicon carbide substrate 2, and the back side is thinned to 100 μm. Then, the blue film is removed, cleaned, titanium is evaporated on the back side, and an ohmic contact is made by laser annealing to form a back drain metal layer 1, thereby completing the preparation of a silicon carbide-based integrated Schottky power device. Fig.15 As shown, the back drain metal layer 1 includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

[0084] The method for preparing a silicon carbide-based integrated Schottky power device in an embodiment of the present invention forms a Schottky contact between the Schottky metal layer 9 and the n-type drift layer 3, which can reduce the on-voltage when the power device is forward-biased; reverse bias can avoid degradation of the gate oxide layer 7, and the polysilicon gate 8 with a separated structure can reduce the gate capacitance and reduce the high-frequency power consumption of the device, thereby improving the performance of the device.

[0085] The above are only implementation modes of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A silicon carbide-based integrated Schottky power device, characterized in that: The invention comprises a back drain metal layer, an n+ type silicon carbide substrate, and an n-type drift layer which are stacked in sequence from bottom to top; p-type base regions are respectively arranged on both sides of the top of the n-type drift layer, a p+ type source region and an n+ type source region are wrapped in the p-type base region, the p+ type source region and the n+ type source region are arranged side by side and the sides are in contact with each other, and the p+ type source region is arranged close to the side of the n-type drift layer; a first source metal layer, a first oxide layer, a Schottky metal layer, a second oxide layer, and a second source metal layer are sequentially arranged above the n-type drift layer from left to right, and the Schottky metal layer is in contact with the A Schottky contact is formed between the n-type drift layers, a polysilicon gate is wrapped in the first oxide layer and the second oxide layer, a gate oxide layer adjacent to the polysilicon gate is correspondingly arranged below the first oxide layer and the second oxide layer, the gate oxide layer is arranged above the n-type drift layer, and the polysilicon gate is arranged on a side of the gate oxide layer away from the n-type drift layer; a top metal layer is arranged above the first source metal layer, the first oxide layer, the Schottky metal layer, the second oxide layer and the second source metal layer, and a passivation layer is arranged above the top metal layer.

2. The silicon carbide-based integrated Schottky power device according to claim 1, characterized in that: The depth of the p-type base region is 1.5 μm and the doping concentration is 1e17 cm -3 ~1e18 cm -3 The depth of the n+ type source region is 0.2 μm, and the doping concentration is greater than 1e19 cm -3 The depth of the p+ source region is 3.0 μm and the doping concentration is 1e18 cm -3 ~1e19 cm -3 .

3. The silicon carbide-based integrated Schottky power device according to claim 1, characterized in that: The thickness of the Schottky metal layer is 1000 Å.

4. The silicon carbide-based integrated Schottky power device according to claim 1, characterized in that: The thickness of the gate oxide layer is 500A; the thickness of the polysilicon gate is 4000A.

5. The silicon carbide-based integrated Schottky power device according to claim 1, characterized in that: The thickness of the first oxide layer and the second oxide layer are both 1.0 μm.

6. The silicon carbide-based integrated Schottky power device according to claim 1, characterized in that: The passivation layer includes a plasma enhanced tetraethyl orthosilicate layer with a thickness of 6000 Å, a plasma enhanced silicon nitride layer with a thickness of 300 Å, and a polyimide film layer with a thickness of 7 μm.

7. The silicon carbide-based integrated Schottky power device according to claim 1, characterized in that: The thickness of the first source metal layer and the second source metal layer are both 1000 Å.

8. The silicon carbide-based integrated Schottky power device according to claim 1, characterized in that: The thickness of the top metal layer is 4 μm.

9. The silicon carbide-based integrated Schottky power device according to claim 1, characterized in that: The back drain metal layer includes a metal titanium layer with a thickness of 1000A, a metal nickel layer with a thickness of 2000A, and a metal silver layer with a thickness of 10kA.

10. A method for preparing a silicon carbide-based integrated Schottky power device according to any one of claims 1 to 9, comprising: Step S1: epitaxially growing an n-type drift layer on an n+ silicon carbide substrate; Step S2: forming a p-type base region on the n-type drift layer by sequentially growing a first masking layer process, a high temperature oxidation process, a photolithography process, an etching process, and an ion implantation process; Step S3: using the first masking layer to grow a layer of low-pressure tetraethoxy silicate glass, and forming an n+ type source region through a plasma dry isotropic etching process, a self-alignment process and an ion implantation process; Step S4: removing the first masking layer by wet method, re-depositing the second masking layers of each layer, and forming a p+ type source region by photolithography, etching and ion implantation; Step S5: growing a gate oxide layer through a carbon film growth and high temperature activation process and a nitrogen annealing process; Step S6: depositing saturated doped polysilicon on the gate oxide layer, and forming two mutually separated polysilicon gates through photolithography and etching processes; Step S7: depositing a layer of borophosphosilicate glass on the polysilicon gate and the gate oxide layer, and forming an oxidation region by photolithography and etching, wherein the oxidation region wraps the two polysilicon gates; Step S8: forming a first source metal layer and a second source metal layer on both sides of the oxidation region by a metal deposition process and a rapid annealing process; Step S9: forming a first oxide layer and a second oxide layer separated from each other and a Schottky filling region located between the first oxide layer and the second oxide layer in the oxide region by a dry etching process, depositing a layer of metal titanium in the Schottky filling region, and forming a Schottky metal layer by an annealing process; Step S10: forming a top metal layer on the first source metal layer, the first oxide layer, the Schottky metal layer, the second oxide layer and the second source metal layer by a sputtering process and an etching process, and depositing a passivation layer on the top metal layer; Step S11: forming a back drain metal layer on the back of the n+ type silicon carbide substrate by a metal deposition process and a laser annealing process, thereby completing the preparation of a silicon carbide-based integrated Schottky power device.

Citation Information

Patent Citations

  • Silicon carbide power device, preparation method thereof and chip

    CN116994956A

  • JBS-integrated boss split-gate silicon carbide MOSFET and preparation process

    CN117253923A

  • Asymmetric groove type terminal of anti-radiation MOS (Metal Oxide Semiconductor) field effect transistor and preparation method

    CN117976713A

  • Metal-oxide semiconductor field effect transistor device and manufacturing method therefor

    US20230060069A1