Photovoltaic tile preparation method based on ultraviolet curing technology
Through ultraviolet curing technology and self-cleaning coatings, the high energy consumption, easy damage and dust impact problems in photovoltaic shingles are solved, and efficient and low-cost photovoltaic shingles are achieved and power generation efficiency is improved.
Patent Information
- Application Number
- CN202411007965.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing photovoltaic shingles preparation methods have problems such as high energy consumption, high lamination equipment requirements, easy damage to flexible battery cells, difficulty in preparing corrugated photovoltaic shingles, and dust and dirt affecting power generation efficiency.
Photovoltaic tile is prepared by ultraviolet curing technology. By preparing tempered glass with curved structures, laminated components and using ultraviolet curing glue layer for light curing, plasticizer, stabilizer and coupling agent are added to improve the stability and power generation efficiency of glue layer. , and spray the self-cleaning functional coating on the tempered glass to prevent dust from adhesion.
The preparation of photovoltaic shingles with low energy consumption and high stability is achieved, which avoids damage to flexible cell cells, reduces the difficulty of preparing waveform photovoltaic shingles, and improves the power generation efficiency and artistry of photovoltaic modules, and reduces the impact of dust.
Smart Images

Figure CN118943218A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic tile preparation, and in particular to a method for preparing photovoltaic tiles based on ultraviolet light curing technology. Background Art
[0002] Photovoltaic building integration refers to the technology of combining photovoltaic power generation devices with building materials so that the building itself can generate electricity. Photovoltaic tiles are the basic components. Generally speaking, photovoltaic tiles are composed of glass, film cells and back panels.
[0003] In the prior art, the main packaging method for glass photovoltaic modules is to completely bond the cover glass and the back glass through PVB film or EVA film under high temperature and high pressure. The production conditions for preparing photovoltaic tiles are relatively harsh, the requirements for laminating equipment are high, and the energy consumption is high.
[0004] The defects of the existing photovoltaic tile preparation method are:
[0005] 1. Application document WO2019196332A1 proposes a curved photovoltaic tile and a method for preparing the same. However, the photovoltaic tile is prepared by using a general hot melt adhesive film to completely bond the panel and the back panel, which has high requirements for the lamination equipment and consumes a lot of energy. It does not consider the use of ultraviolet light curing technology to prepare the photovoltaic tile;
[0006] 2. Application document CN116638833A discloses a photovoltaic tile preparation method and a photovoltaic tile and roof installation system. However, the photovoltaic tile preparation process does not take into account that if the edge of the flexible cell is too close to the edge of the tempered glass during preparation, the flexible cell may be damaged when the photovoltaic tile is laminated;
[0007] 3. Application document CN111200033A proposes a photovoltaic tile preparation process and a photovoltaic tile preparation production line. However, the photovoltaic tile preparation in the patent document is to lay out and combine the photovoltaic modules and then bend them. It is difficult to bend the assembled photovoltaic tile paving parts, and it is difficult to prepare corrugated photovoltaic tiles.
[0008] 4. Application document CN116914007A discloses a new type of photovoltaic tile. During the use of the photovoltaic tile prepared in this application document, dust and dirt in the air are easily attached to the surface of the photovoltaic tile, resulting in a reduction in the photovoltaic tile's absorption area for sunlight, thereby reducing the power generation efficiency of the photovoltaic module. Summary of the invention
[0009] The purpose of the present invention is to provide a method for preparing photovoltaic tiles based on ultraviolet light curing technology to solve the problems raised in the above background technology.
[0010] To achieve the above object, the present invention provides the following technical solution: a method for preparing photovoltaic tiles based on ultraviolet curing technology, comprising the following steps:
[0011] Step S1, preparing tempered glass with a curved surface structure;
[0012] Step S2, sequentially arranging and stacking the panel tempered glass, the UV-curing adhesive layer, the flexible battery sheet, the UV-curing adhesive layer and the back panel tempered glass;
[0013] Step S3, pre-pressing the photovoltaic tile paving pieces stacked in the above step S2 using a laminator to obtain photovoltaic tile laminates;
[0014] Step S4, using ultraviolet curing equipment to irradiate the ultraviolet curing adhesive layer on the photovoltaic tile paving member to achieve curing and shaping of the photovoltaic tile laminate;
[0015] Step S5, laser cutting and trimming the photovoltaic tile laminate after the processing in step S4 to obtain a photovoltaic tile assembly;
[0016] Step S6, edge sealing and wiring of the photovoltaic tile assembly processed in step S5.
[0017] Preferably, the UV-curable adhesive layer is an adhesive layer for solar module encapsulation to which a photoinitiator is added, and the adhesive layer for solar module encapsulation is an EVA hot-melt adhesive layer.
[0018] Preferably, a plasticizer, a stabilizer and a coupling agent are added to the UV-curable adhesive layer, the stabilizer includes p-methoxyphenol or hydroquinone, and the coupling agent is an inorganic coupling agent, which includes one of a metal oxide coupling agent and a metal acid salt coupling agent.
[0019] Preferably, the pre-pressing temperature of the laminator is between 90-165° C., the pressure is between 0.4-1.2 atm, and the time is 2-5 min.
[0020] Preferably, the process of preparing the tempered glass with a curved surface structure in step S1 is as follows:
[0021] a. Preheating and forming: Put the glass plate into a high-temperature oven for preheating to soften it, then quickly place the hot glass plate on the mold, and use the pressing plate to apply uniform pressure to the hot glass to form the tempered glass.
[0022] b. After the glass is formed, it is subjected to rapid cooling, the quality of the tempered glass after rapid cooling is inspected, and the edge of the smooth glass is polished;
[0023] c. Spray the self-cleaning coating evenly on the top of the panel glass and the bottom of the back glass with a thickness of 42um, and dry the sprayed surface of the tempered glass.
[0024] Preferably, the coating with self-cleaning function is composed of 12-18 parts of hydrophobic silica nanoparticles with active groups, 115-146 parts of alcohol solvents and 1-2 parts of additives in parts by weight, and the coating with self-cleaning function is highly transparent.
[0025] Preferably, the tempered glass is a wave-shaped structure, the wave shape of the tempered glass is a sine curve, and the amplitude of the wave shape of the tempered glass is 10-15 mm.
[0026] Preferably, in step S2, the flexible solar cell is a solar cell made of amorphous silicon encapsulated with resin as the main photovoltaic element layer laid flat on a flexible material.
[0027] Preferably, in step S2, the gap distance between the outer edge of the flexible battery sheet and the long side of the tempered glass is not less than 12 mm, the gap distance between the outer edge of the flexible battery sheet and the wide side of the tempered glass is not less than 15 mm, and the gap distance between the edge of the UV-cured adhesive layer and the edge of the tempered glass is not less than 5 mm.
[0028] Preferably, in step S4, the UV curing equipment is a UV curing box with a built-in UV lamp, the main wavelength range is 300-400nm, and the irradiation intensity is not less than 450MW / cm 2 The total irradiation reaches 4800MJ / cm 2 above.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The present invention uses a UV-curing adhesive layer, which can trigger the photoinitiator in the resin to produce active free radicals or ion radicals under the irradiation of ultraviolet light, thereby initiating polymerization, cross-linking and grafting reactions, so that the photovoltaic module is stably bonded internally, and the curing is fast and energy-saving. At the same time, a plasticizer, a stabilizer and a coupling agent are added to the UV-curing adhesive layer. The stabilizer can improve the stability of the UV-curing adhesive layer, the plasticizer reduces the softening temperature and the glass transition temperature of the adhesive film, thereby improving the low-temperature resistance of the UV-curing adhesive layer, and the coupling agent can enhance the interfacial bonding force of the material and the charge transfer efficiency, thereby improving the power generation efficiency of the photovoltaic adhesive film.
[0031] 2. The present invention determines the gap distance between the outer edge of the flexible battery cell and the edge of the tempered glass when stacking the layers of photovoltaic tile paving components, thereby ensuring that the tempered glass can completely cover the flexible battery cell. At the same time, it can also avoid cracks when the stacked photovoltaic tile paving components are pre-pressed, which may damage the flexible battery cell. In addition, there are certain requirements for the distance between the UV-curing layer used and the edge of the tempered glass to ensure that there will be no lack of glue.
[0032] 3. The present invention prepares curved glass by preheating and compression molding flat glass to form tempered glass, and quenching and polishing the formed glass. The prepared corrugated curved glass is used as a panel and a backplane to directly prepare corrugated photovoltaic tiles, which reduces the difficulty of preparing corrugated photovoltaic modules. The curved photovoltaic tiles can extend the sunlight time and increase the light absorption area, thereby improving the power generation efficiency. The use of curved tempered glass to prepare curved photovoltaic tiles increases the practicality and artistry of the product.
[0033] 4. In the present invention, a highly transparent coating with self-cleaning function composed of hydrophobic silica nanoparticles with active groups, alcohol solvents and additives prepared in a certain weight ratio is evenly coated on the surface of the tempered glass and dried, so that dust particles in the air adhere to the surface of the coating in a suspended state and are not easy to adhere to the surface of the tempered glass, thereby reducing the dust and dirt in the outside air adhering to the surface of the photovoltaic tiles and improving the power generation efficiency of the photovoltaic modules. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of the stacked structure of an embodiment of the present invention. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Embodiment 1
[0037] An embodiment provided by the present invention is a method for preparing photovoltaic tiles based on ultraviolet light curing technology, comprising the following steps:
[0038] Step S1, preparing tempered glass with a curved surface structure, the specific process is as follows:
[0039] a. Preheating and forming: Put the glass plate into a high-temperature oven for preheating to soften it, then quickly place the hot glass plate on the mold, and use a pressing plate to apply uniform pressure to the hot glass to form the tempered glass. The tempered glass has a wavy structure, and the waveform of the tempered glass is a sine curve shape. The amplitude of the waveform of the tempered glass is 12mm;
[0040] b. After the glass is formed, it is subjected to rapid cooling, the quality of the tempered glass after rapid cooling is inspected, and the edge of the smooth glass is polished;
[0041] c. Spray the coating with self-cleaning function evenly on the top of the panel glass and the bottom of the back panel glass with a thickness of 42um, and dry the sprayed surface of the tempered glass;
[0042] The coating with self-cleaning function is composed of 12 parts of hydrophobic silica nanoparticles with active groups, 115 parts of alcohol solvents and 1 part of additives according to weight parts, and the coating with self-cleaning function is highly transparent;
[0043] Step S2, sequentially arranging and laminating the panel tempered glass, the UV-curing adhesive layer, the flexible battery sheet, the UV-curing adhesive layer and the backboard tempered glass, during the arrangement and lamination process, the gap distance between the outer edge of the flexible battery sheet and the long side of the tempered glass is 12 mm, the gap distance between the outer edge of the flexible battery sheet and the wide side of the tempered glass is 15 mm, the gap distance between the edge of the UV-curing adhesive layer and the edge of the tempered glass is 5 mm, the flexible battery sheet is a solar cell sheet made of amorphous silicon encapsulated in resin as the main photoelectric element layer laid flat on a flexible material, the UV-curing adhesive layer is an adhesive layer for encapsulating solar modules with a photoinitiator added, the adhesive layer for encapsulating solar modules is an EVA hot melt adhesive layer, a plasticizer, a stabilizer and a coupling agent are added to the UV-curing adhesive layer, the stabilizer includes p-methoxyphenol, the coupling agent is an inorganic coupling agent, and the inorganic coupling agent includes a metal oxide coupling agent;
[0044] Step S3, pre-pressing the photovoltaic tile paving pieces stacked in the above step S2 using a laminator, with the pre-pressing temperature of the laminator being 100° C., the pressure being 0.8 atm, and the time being 2.5 min;
[0045] Step S4: Use ultraviolet curing equipment to irradiate the ultraviolet curing adhesive layer on the photovoltaic tile paving piece to achieve curing and shaping. The ultraviolet curing equipment is an ultraviolet curing box with a built-in ultraviolet lamp. The irradiation wavelength range is set to 350nm and the irradiation intensity is 450MW / cm 2 The total irradiation reaches 4800MJ / cm 2 above;
[0046] Step S5, laser cutting and trimming the photovoltaic tile laminate after the processing in step S4 to obtain a photovoltaic tile assembly;
[0047] Step S6, edge sealing and wiring of the photovoltaic tile assembly processed in step S5.
[0048] Embodiment 2
[0049] An embodiment provided by the present invention is a method for preparing photovoltaic tiles based on ultraviolet light curing technology, comprising the following steps:
[0050] Step S1, preparing tempered glass with a curved surface structure, the specific process is as follows:
[0051] a. Preheating and forming: Put the glass plate into a high-temperature oven for preheating to soften it, then quickly place the hot glass plate on the mold, and use a pressing plate to apply uniform pressure to the hot glass to form the tempered glass. The tempered glass has a wavy structure, and the waveform of the tempered glass is a sine curve shape, and the amplitude of the waveform of the tempered glass is 10mm;
[0052] b. After the glass is formed, it is subjected to rapid cooling, the quality of the tempered glass after rapid cooling is inspected, and the edge of the smooth glass is polished;
[0053] c. Spray the coating with self-cleaning function evenly on the top of the panel glass and the bottom of the back panel glass with a thickness of 42um, and dry the sprayed surface of the tempered glass;
[0054] Among them, the coating with self-cleaning function is composed of 13 parts of hydrophobic silica nanoparticles with active groups, 118 parts of alcohol solvents and 1.3 parts of additives according to weight parts, and the coating with self-cleaning function is highly transparent;
[0055] Step S2, sequentially arranging and laminating the panel tempered glass, the UV-curing adhesive layer, the flexible battery sheet, the UV-curing adhesive layer and the backboard tempered glass, during the arrangement and lamination process, the gap distance between the outer edge of the flexible battery sheet and the long side of the tempered glass is 13 mm, the gap distance between the outer edge of the flexible battery sheet and the wide side of the tempered glass is 16 mm, the gap distance between the edge of the UV-curing adhesive layer and the edge of the tempered glass is 6 mm, the flexible battery sheet is a solar cell sheet made of amorphous silicon encapsulated in resin as the main photoelectric element layer laid flat on a flexible material, the UV-curing adhesive layer is an adhesive layer for encapsulating solar modules with a photoinitiator added, the adhesive layer for encapsulating solar modules is an EVA hot melt adhesive layer, a plasticizer, a stabilizer and a coupling agent are added to the UV-curing adhesive layer, the stabilizer includes hydroquinone, the coupling agent is an inorganic coupling agent, and the inorganic coupling agent includes a metal oxide coupling agent;
[0056] Step S3, pre-pressing the photovoltaic tile paving pieces stacked in the above step S2 using a laminator, with the pre-pressing temperature of the laminator being 100° C., the pressure being 0.8 atm, and the time being 2.5 min;
[0057] Step S4: Use ultraviolet curing equipment to irradiate the ultraviolet curing adhesive layer on the photovoltaic tile paving piece to achieve curing and shaping. The ultraviolet curing equipment is an ultraviolet curing box with a built-in ultraviolet lamp. The irradiation wavelength range is set to 350nm and the irradiation intensity is 450MW / cm 2 The total irradiation reaches 4800MJ / cm 2 above;
[0058] Step S5, laser cutting and trimming the photovoltaic tile laminate after the processing in step S4 to obtain a photovoltaic tile assembly;
[0059] Step S6, edge sealing and wiring of the photovoltaic tile assembly processed in step S5.
[0060] Embodiment 3
[0061] An embodiment provided by the present invention is a method for preparing photovoltaic tiles based on ultraviolet light curing technology, comprising the following steps:
[0062] Step S1, preparing tempered glass with a curved surface structure, the specific process is as follows:
[0063] a. Preheating and forming: Put the glass plate into a high-temperature oven for preheating to soften it, then quickly place the hot glass plate on the mold, and use a pressing plate to apply uniform pressure to the hot glass to form the tempered glass. The tempered glass has a wavy structure, and the waveform of the tempered glass is a sine curve shape. The amplitude of the waveform of the tempered glass is 13mm;
[0064] b. After the glass is formed, it is subjected to rapid cooling, the quality of the tempered glass after rapid cooling is inspected, and the edge of the smooth glass is polished;
[0065] c. Spray the coating with self-cleaning function evenly on the top of the panel glass and the bottom of the back panel glass with a thickness of 42um, and dry the sprayed surface of the tempered glass;
[0066] The coating with self-cleaning function is composed of 12 parts of hydrophobic silica nanoparticles with active groups, 120 parts of alcohol solvents and 1.3 parts of additives according to weight parts, and the coating with self-cleaning function is highly transparent;
[0067] Step S2, sequentially arranging and laminating the panel tempered glass, the UV-curing adhesive layer, the flexible battery sheet, the UV-curing adhesive layer and the backboard tempered glass, during the arrangement and lamination process, the gap distance between the outer edge of the flexible battery sheet and the long side of the tempered glass is 13 mm, the gap distance between the outer edge of the flexible battery sheet and the wide side of the tempered glass is 16 mm, the gap distance between the edge of the UV-curing adhesive layer and the edge of the tempered glass is 5 mm, the flexible battery sheet is a solar cell sheet made of amorphous silicon encapsulated in resin as the main photoelectric element layer laid flat on a flexible material, the UV-curing adhesive layer is an adhesive layer for encapsulating solar modules with a photoinitiator added, the adhesive layer for encapsulating solar modules is an EVA hot melt adhesive layer, a plasticizer, a stabilizer and a coupling agent are added to the UV-curing adhesive layer, the stabilizer includes p-methoxyphenol and hydroquinone, the coupling agent is an inorganic coupling agent, and the inorganic coupling agent includes a metal oxide coupling agent;
[0068] Step S3, pre-pressing the photovoltaic tile paving pieces stacked in the above step S2 using a laminator, with the pre-pressing temperature of the laminator being 100° C., the pressure being 1 atm, and the time being 2 min;
[0069] Step S4: Use ultraviolet curing equipment to irradiate the ultraviolet curing adhesive layer on the photovoltaic tile paving piece to achieve curing and shaping. The ultraviolet curing equipment is an ultraviolet curing box with a built-in ultraviolet lamp. The irradiation wavelength range is set to 350nm and the irradiation intensity is 450MW / cm 2 The total irradiation reaches 4800MJ / cm 2 above;
[0070] Step S5, laser cutting and trimming the photovoltaic tile laminate after the processing in step S4 to obtain a photovoltaic tile assembly;
[0071] Step S6, edge sealing and wiring of the photovoltaic tile assembly processed in step S5.
[0072] Embodiment 4
[0073] An embodiment provided by the present invention is a method for preparing photovoltaic tiles based on ultraviolet light curing technology, comprising the following steps:
[0074] Step S1, preparing tempered glass with a curved surface structure, the specific process is as follows:
[0075] a. Preheating and forming: Put the glass plate into a high-temperature oven for preheating to soften it, then quickly place the hot glass plate on the mold, and use a pressing plate to apply uniform pressure to the hot glass to form the tempered glass. The tempered glass has a wavy structure, and the waveform of the tempered glass is a sine curve shape, and the amplitude of the waveform of the tempered glass is 10mm;
[0076] b. After the glass is formed, it is subjected to rapid cooling, the quality of the tempered glass after rapid cooling is inspected, and the edge of the smooth glass is polished;
[0077] c. Spray the coating with self-cleaning function evenly on the top of the panel glass and the bottom of the back panel glass with a thickness of 42um, and dry the sprayed surface of the tempered glass;
[0078] Among them, the coating with self-cleaning function is composed of 13 parts of hydrophobic silica nanoparticles with active groups, 118 parts of alcohol solvents and 1.3 parts of additives according to weight parts, and the coating with self-cleaning function is highly transparent;
[0079] Step S2, sequentially arranging and laminating the panel tempered glass, the UV-curing adhesive layer, the flexible battery sheet, the UV-curing adhesive layer and the backboard tempered glass, during the arrangement and lamination process, the gap distance between the outer edge of the flexible battery sheet and the long side of the tempered glass is 12 mm, the gap distance between the outer edge of the flexible battery sheet and the wide side of the tempered glass is 15 mm, the gap distance between the edge of the UV-curing adhesive layer and the edge of the tempered glass is 6 mm, the flexible battery sheet is a solar cell sheet made of amorphous silicon encapsulated in resin as the main photoelectric element layer laid flat on a flexible material, the UV-curing adhesive layer is an adhesive layer for encapsulating solar modules with a photoinitiator added, the adhesive layer for encapsulating solar modules is an EVA hot melt adhesive layer, a plasticizer, a stabilizer and a coupling agent are added to the UV-curing adhesive layer, the stabilizer includes p-methoxyphenol, the coupling agent is an inorganic coupling agent, and the inorganic coupling agent includes a metal acid salt coupling agent;
[0080] Step S3, pre-pressing the photovoltaic tile paving pieces stacked in the above step S2 using a laminator, with the pre-pressing temperature of the laminator being 120° C., the pressure being 0.8 atm, and the time being 2 min;
[0081] Step S4: Use ultraviolet curing equipment to irradiate the ultraviolet curing adhesive layer on the photovoltaic tile paving piece to achieve curing and shaping. The ultraviolet curing equipment is an ultraviolet curing box with a built-in ultraviolet lamp. The irradiation wavelength range is set to 350nm and the irradiation intensity is 450MW / cm 2 The total irradiation reaches 4800MJ / cm 2 above;
[0082] Step S5, laser cutting and trimming the photovoltaic tile laminate after the processing in step S4 to obtain a photovoltaic tile assembly;
[0083] Step S6, edge sealing and wiring of the photovoltaic tile assembly processed in step S5.
[0084] Embodiment 5
[0085] An embodiment provided by the present invention is a method for preparing photovoltaic tiles based on ultraviolet light curing technology, comprising the following steps:
[0086] Step S1, preparing tempered glass with a curved surface structure, the specific process is as follows:
[0087] a. Preheating and forming: Put the glass plate into a high-temperature oven for preheating to soften it, then quickly place the hot glass plate on the mold, and use a pressing plate to apply uniform pressure to the hot glass to form the tempered glass. The tempered glass has a wavy structure, and the waveform of the tempered glass is a sine curve shape. The amplitude of the waveform of the tempered glass is 15mm;
[0088] b. After the glass is formed, it is subjected to rapid cooling, the quality of the tempered glass after rapid cooling is inspected, and the edge of the smooth glass is polished;
[0089] c. Spray the coating with self-cleaning function evenly on the top of the panel glass and the bottom of the back panel glass with a thickness of 42um, and dry the sprayed surface of the tempered glass;
[0090] The coating with self-cleaning function is composed of 16 parts of hydrophobic silica nanoparticles with active groups, 140 parts of alcohol solvents and 2 parts of additives according to weight parts, and the coating with self-cleaning function is highly transparent;
[0091] Step S2, sequentially arranging and laminating the panel tempered glass, the UV-curing adhesive layer, the flexible battery sheet, the UV-curing adhesive layer and the backboard tempered glass, during the arrangement and lamination process, the gap distance between the outer edge of the flexible battery sheet and the long side of the tempered glass is 12 mm, the gap distance between the outer edge of the flexible battery sheet and the wide side of the tempered glass is 15 mm, the gap distance between the edge of the UV-curing adhesive layer and the edge of the tempered glass is 6 mm, the flexible battery sheet is a solar cell sheet made of amorphous silicon encapsulated in resin as the main photoelectric element layer laid flat on a flexible material, the UV-curing adhesive layer is an adhesive layer for encapsulating solar modules with a photoinitiator added, the adhesive layer for encapsulating solar modules is an EVA hot melt adhesive layer, a plasticizer, a stabilizer and a coupling agent are added to the UV-curing adhesive layer, the stabilizer includes p-methoxyphenol and hydroquinone, the coupling agent is an inorganic coupling agent, and the inorganic coupling agent includes a metal acid salt coupling agent;
[0092] Step S3, pre-pressing the photovoltaic tile paving pieces stacked in the above step S2 using a laminator, with the pre-pressing temperature of the laminator being 160° C., the pressure being 1.2 atm, and the time being 1.2 min;
[0093] Step S4: Use ultraviolet curing equipment to irradiate the ultraviolet curing adhesive layer on the photovoltaic tile paving piece to achieve curing and shaping. The ultraviolet curing equipment is an ultraviolet curing box with a built-in ultraviolet lamp. The irradiation wavelength range is set to 350nm and the irradiation intensity is 450MW / cm 2 The total irradiation reaches 4800MJ / cm 2 above;
[0094] Step S5, laser cutting and trimming the photovoltaic tile laminate after the processing in step S4 to obtain a photovoltaic tile assembly;
[0095] Step S6, edge sealing and wiring of the photovoltaic tile assembly processed in step S5.
[0096] Embodiment 6
[0097] An embodiment provided by the present invention is a method for preparing photovoltaic tiles based on ultraviolet light curing technology, comprising the following steps:
[0098] Step S1, preparing tempered glass with a curved surface structure, the specific process is as follows:
[0099] a. Preheating and forming: Put the glass plate into a high-temperature oven for preheating to soften it, then quickly place the hot glass plate on the mold, and use a pressing plate to apply uniform pressure to the hot glass to form the tempered glass. The tempered glass has a wavy structure, and the waveform of the tempered glass is a sine curve shape. The amplitude of the waveform of the tempered glass is 15mm;
[0100] b. After the glass is formed, it is subjected to rapid cooling, the quality of the tempered glass after rapid cooling is inspected, and the edge of the smooth glass is polished;
[0101] c. Spray the coating with self-cleaning function evenly on the top of the panel glass and the bottom of the back panel glass with a thickness of 42um, and dry the sprayed surface of the tempered glass;
[0102] The coating with self-cleaning function is composed of 16 parts of hydrophobic silica nanoparticles with active groups, 140 parts of alcohol solvents and 2 parts of additives according to weight parts, and the coating with self-cleaning function is highly transparent;
[0103] Step S2, sequentially stacking the panel tempered glass, the UV-curing adhesive layer, the flexible battery sheet, the UV-curing adhesive layer and the backboard tempered glass, during the layout and stacking process, the gap distance between the outer edge of the flexible battery sheet and the long side of the tempered glass is 12 mm, the gap distance between the outer edge of the flexible battery sheet and the wide side of the tempered glass is 15 mm, the gap distance between the edge of the UV-curing adhesive layer and the edge of the tempered glass is 5 mm, the flexible battery sheet is a solar cell sheet made of amorphous silicon encapsulated in resin as the main photovoltaic element layer laid flat on a flexible material, the UV-curing adhesive layer is an adhesive layer for encapsulating solar modules with a photoinitiator added, the adhesive layer for encapsulating solar modules is an EVA hot melt adhesive layer, a plasticizer, a stabilizer and a coupling agent are added to the UV-curing adhesive layer, the stabilizer includes hydroquinone, the coupling agent is an inorganic coupling agent, and the inorganic coupling agent includes a metal acid salt coupling agent;
[0104] Step S3, pre-pressing the photovoltaic tile paving pieces stacked in the above step S2 using a laminator, with the pre-pressing temperature of the laminator being 120° C., the pressure being 0.8 atm, and the time being 2 min;
[0105] Step S4: Use ultraviolet curing equipment to irradiate the ultraviolet curing adhesive layer on the photovoltaic tile paving piece to achieve curing and shaping. The ultraviolet curing equipment is an ultraviolet curing box with a built-in ultraviolet lamp. The irradiation wavelength range is set to 350nm and the irradiation intensity is 450MW / cm 2 The total irradiation reaches 4800MJ / cm 2 above;
[0106] Step S5, laser cutting and trimming the photovoltaic tile laminate after the processing in step S4 to obtain a photovoltaic tile assembly;
[0107] Step S6, edge sealing and wiring of the photovoltaic tile assembly processed in step S5.
[0108] Comparative Example 1
[0109] The photovoltaic tile preparation method of this comparative example is different from that of Example 1 in that in step S1, the coating with cleaning function is not sprayed on the top of the panel glass and the bottom of the back panel glass, and the rest is the same as that of Example 1.
[0110] Comparative Example 2
[0111] The photovoltaic tile preparation method of this comparative example is different from that of Example 1 in that there is no need to prepare curved tempered glass, flat tempered glass is used in step S2, and the rest is the same as that of Example 1.
[0112] Comparative Example 3
[0113] The photovoltaic tile preparation method of this comparative example is different from that of Example 1 in that a UV-curable adhesive layer without adding a plasticizer, a stabilizer and a coupling agent is used in step S2, and the rest is the same as that in Example 1.
[0114] Power generation efficiency inspection test
[0115] The photovoltaic tile samples prepared in Examples 1-6 and the samples prepared in the comparative example were taken, and the power generation efficiency of the photovoltaic tiles was tested according to the external quantum effect measurement method; the samples prepared in Examples 1-6 and the comparative example were respectively used and tested on the 1st day and the 50th day; this experiment mainly focuses on the power generation efficiency of the photovoltaic tiles.
[0116] The power generation efficiency test results of the photovoltaic tiles of Examples 1-6 and Comparative Examples 1-3 are as follows
[0117] Serial number Day 1 (Power generation efficiency %) Day 50 (Power generation efficiency%) Embodiment 1 22.65 21.45 Embodiment 2 22.90 21.89 Embodiment 3 21.89 20.60 Embodiment 4 22.73 21.45 Embodiment 5 22.75 21.56 Embodiment 6 22.80 21.85 Comparative Example 1 22.30 18.50 Comparative Example 2 19.05 16.50 Comparative Example 3 21.60 20.70
[0118] In UV-curing adhesives, stabilizers can improve the storage stability of resins. Coupling agents are substances that can improve the interfacial compatibility of materials; in the preparation process of photovoltaic adhesive films, coupling agents can be used to enhance the interfacial bonding force and charge transfer efficiency of materials, thereby improving the photoelectric conversion efficiency of photovoltaic adhesive films, thereby improving the power generation efficiency of photovoltaic tiles. Inorganic coupling agents are a class of substances based on inorganic compounds. Common inorganic coupling agents include metal oxides, metal acid salts, etc.; metal oxide coupling agents have high thermal stability and chemical stability, which can effectively enhance the thermal stability and chemical stability of photovoltaic adhesive films; metal acid salt coupling agents have high electrical conductivity and light absorption performance, which can improve the photoelectric conversion efficiency of photovoltaic adhesive films, thereby improving the power generation efficiency of prepared photovoltaic tiles. Plasticizers can weaken the forces between polymer molecules, reduce the softening temperature and glass transition temperature of the film, and improve low temperature resistance.
[0119] Combined with Examples 1-6 and Comparative Examples 1-3, and combined with the test results, analysis was performed:
[0120] By comparing Examples 1-6 with Comparative Example 1, since a certain thickness of coating with a self-cleaning function is sprayed on the surface of the tempered glass, dust impurities in the air are not easy to adhere to the surface of the tempered glass. Therefore, after using the photovoltaic tiles for a long time, the power generation efficiency of the photovoltaic tiles is not easy to change greatly due to dust adhesion affecting the light absorption area;
[0121] By comparing Examples 1-6 with Comparative Example 2, it can be seen that the photovoltaic tiles made of flat glass often lose light energy due to reflection, while the photovoltaic tiles with curved surface design can reduce reflection, increase the absorption of light energy, and extend the illumination time of the photovoltaic panels, thereby improving the power generation efficiency.
[0122] By comparing Examples 1-6 with Comparative Example 3, it can be seen that because additives such as stabilizers, plasticizers and coupling agents are added to the UV-cured corneal layer used to prepare photovoltaic tiles, the performance of the photovoltaic tiles can be effectively improved, thereby affecting the power generation efficiency of the photovoltaic tiles.
[0123] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing photovoltaic tiles based on ultraviolet light curing technology, It is characterized in that The steps include: Step S1, preparing tempered glass with a curved surface structure; Step S2, sequentially arranging and stacking the panel tempered glass, the UV-curing adhesive layer, the flexible battery sheet, the UV-curing adhesive layer and the back panel tempered glass; Step S3, pre-pressing the photovoltaic tile paving pieces stacked in the above step S2 using a laminator to obtain photovoltaic tile laminates; Step S4, using ultraviolet curing equipment to irradiate the ultraviolet curing adhesive layer on the photovoltaic tile paving member to achieve curing and shaping of the photovoltaic tile laminate; Step S5, laser cutting and trimming the photovoltaic tile laminate after the processing in step S4 to obtain a photovoltaic tile assembly; Step S6, edge sealing and wiring of the photovoltaic tile assembly processed in step S5.
2. A method for preparing photovoltaic tiles based on ultraviolet curing technology according to claim 1, Features: The UV-curable adhesive layer is an adhesive layer for solar module encapsulation to which a photoinitiator is added, and the adhesive layer for solar module encapsulation is an EVA hot-melt adhesive layer.
3. A method for preparing photovoltaic tiles based on ultraviolet curing technology according to claim 2, Features: Plasticizer, stabilizer and coupling agent are added to the UV-curable adhesive layer. The stabilizer includes p-methoxyphenol or hydroquinone. The coupling agent is an inorganic coupling agent. The inorganic coupling agent includes one of a metal oxide coupling agent and a metal acid salt coupling agent.
4. The method for preparing photovoltaic tiles based on ultraviolet curing technology according to claim 1, Features: The pre-pressing temperature of the laminator is between 90-165°C, the pressure is between 0.4-1.2atm, and the time is 2-5min.
5. The method for preparing photovoltaic tiles based on ultraviolet curing technology according to claim 1, Features: The process of preparing the tempered glass with a curved surface structure in step S1 is as follows: a. Preheating and forming: Put the glass plate into a high-temperature oven for preheating to soften it, then quickly place the hot glass plate on the mold, and use the pressing plate to apply uniform pressure to the hot glass to form the tempered glass. b. After the glass is formed, it is subjected to rapid cooling, the quality of the tempered glass after rapid cooling is inspected, and the edge of the smooth glass is polished; c. Spray the self-cleaning coating evenly on the top of the panel glass and the bottom of the back glass with a thickness of 42um, and dry the sprayed surface of the tempered glass.
6. A method for preparing photovoltaic tiles based on ultraviolet curing technology according to claim 5, Features: The coating with self-cleaning function is composed of 12-18 parts of hydrophobic silicon dioxide nanoparticles with active groups, 115-146 parts of alcohol solvents and 1-2 parts of auxiliary agents in parts by weight, and the coating with self-cleaning function is highly transparent.
7. A method for preparing photovoltaic tiles based on ultraviolet light curing technology according to claim 5, Features: The tempered glass is of a wave structure, the wave shape of the tempered glass is a sine curve, and the amplitude of the wave shape of the tempered glass is 10-15mm.
8. The method for preparing photovoltaic tiles based on ultraviolet curing technology according to claim 1, Features: In step S2, the flexible solar cell is a solar cell made of amorphous silicon encapsulated with resin as the main photovoltaic element layer laid flat on a flexible material.
9. The method for preparing photovoltaic tiles based on ultraviolet curing technology according to claim 1, Features: In step S2, the gap distance between the outer edge of the flexible battery sheet and the long side of the tempered glass is not less than 12 mm, the gap distance between the outer edge of the flexible battery sheet and the wide side of the tempered glass is not less than 15 mm, and the gap distance between the edge of the UV-cured adhesive layer and the edge of the tempered glass is not less than 5 mm.
10. The method for preparing photovoltaic tiles based on ultraviolet curing technology according to claim 1, Features: In step S4, the UV curing equipment is a UV curing box with a built-in UV lamp, the main wavelength range is 300-400nm, and the irradiation intensity is not less than 450MW / cm 2 The total irradiation reaches 4800MJ / cm 2 above.
Citation Information
Patent Citations
Lamination preparation process of curved-surface double-glass photovoltaic module
CN102983213A
Transparent super-hydrophobic self-cleaning coating
CN105086537A
Photovoltaic module packaging technology based on ultraviolet light curing technology
CN106935672A
Water-soluble ultraviolet curing adhesive
JP2002332457A