Graphite negative electrode particle, preparation method thereof, battery and energy storage device

By designing graphite negative electrode particles with specific pore structures and preparation methods, the problem of difficulty in both expansion rate and compaction density in lithium-ion batteries in the prior art is solved, and the improvement of high energy density and cycling performance is achieved.

CN118943365AActive Publication Date: 2024-11-12XIAMEN HITHIUM ENERGY STORAGE TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410977475.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Existing graphite materials are difficult to have low expansion rates and high compaction density in lithium-ion batteries, which affects the energy efficiency performance of the battery.

Method used

A graphite negative electrode particle is designed, which has multiple long pores, and the angle between the maximum length direction of the pore and the maximum length direction of the graphite particles is 0°≤α≤30°, and is subject to a specific preparation method. Includes carbon source pretreatment and graphitization, the porosity and pore shape are controlled for high compaction density and low expansion rates.

Benefits of technology

The low expansion rate and high compaction density of graphite negative electrode particles during lithium embedding are achieved, which improves the energy density and cycling performance of the battery and reduces the risk of rupture of the solid electrolyte interface film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943365A_ABST
    Figure CN118943365A_ABST
Patent Text Reader

Abstract

The invention provides graphite negative electrode particles, a preparation method thereof, a battery and an energy storage device. The graphite negative electrode particle provided by the embodiment of the invention is provided with a plurality of pores, the plurality of pores are strip-shaped, the maximum length direction of the pores is a first long diameter direction, and the maximum length direction of the graphite negative electrode particle is a second long diameter direction. An included angle alpha between the first long diameter direction and the second long diameter direction is larger than or equal to 0 degree and smaller than or equal to 30 degrees, and the porosity P1 of particles with the diameter larger than 10 microns in the graphite negative electrode particles is larger than or equal to 10% and smaller than or equal to 60%. The graphite negative electrode particle provided by the invention has relatively high compaction density and relatively low expansion rate in a lithium intercalation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage, and specifically to a graphite negative electrode particle, a preparation method thereof, a battery and an energy storage device. Background Art

[0002] Energy storage lithium-ion batteries have increasingly higher requirements for energy efficiency performance. Improving energy efficiency performance mainly depends on improving the kinetics of the electrochemical system. Graphite is often used as the negative electrode material of lithium-ion batteries, but existing graphite materials are difficult to have both a low expansion rate and a high compaction density. Summary of the invention

[0003] The embodiment of the present application provides a graphite negative electrode particle, which has a higher compaction density and a lower expansion rate during the lithium insertion process.

[0004] In a first aspect, an embodiment of the present application provides a graphite negative electrode particle, wherein the graphite negative electrode particle has a plurality of pores, wherein the plurality of pores are in the shape of long strips, wherein the maximum length direction of the pores is a first major axis direction, wherein the maximum length direction of the graphite negative electrode particle is a second major axis direction, wherein the angle α between the first major axis direction and the second major axis direction is in the range of 0°≤α≤30°, and wherein the porosity P1 of particles with a diameter greater than 10 μm in the graphite negative electrode particles is in the range of 10%≤P1≤60%.

[0005] Furthermore, in the same graphite negative electrode particle, the range of the angle β between any two pores in the first major axis direction is: 0°≤β≤20°.

[0006] Furthermore, in the same graphite negative electrode particle, the distance d between two adjacent pores is in the range of 0.5 μm≤d≤5 μm.

[0007] Furthermore, the minimum length direction of the pore is the short diameter direction, the size of the pore along the first long diameter direction is smaller than the size of the pore along the short diameter direction, the size w1 of the pore along the short diameter direction is in the range of 0.5μm≤w1≤1μm; the size w2 of the pore along the first long diameter direction is in the range of 3μm≤w1≤20μm.

[0008] Furthermore, the porosity P2 of the graphite negative electrode particles with a diameter greater than or equal to 6 μm and less than or equal to 10 μm is in the range of 5%≤P2≤20%; the porosity P3 of the graphite negative electrode particles with a diameter greater than or equal to 1 μm and less than 6 μm is in the range of 3%≤P2≤5%.

[0009] Furthermore, the graphite negative electrode particles include multiple layers stacked in sequence, and the first major axis direction of the pores is parallel to the layers.

[0010] In a second aspect, the present application also provides a method for preparing graphite negative electrode particles, the preparation method comprising:

[0011] Providing a carbon source, wherein the mass fraction of volatile matter in the carbon source ranges from 3% to 15%;

[0012] pre-treating the carbon source at a first temperature to obtain intermediate particles; and

[0013] The intermediate particles are graphitized at a second temperature to obtain the graphite negative electrode particles, wherein the first temperature is lower than the second temperature, wherein the graphite negative electrode particles have a plurality of pores, the plurality of pores are in the shape of long strips, the maximum length direction of the pores is the first long diameter direction, the maximum length direction of the graphite negative electrode particles is the second long diameter direction, the angle α between the first long diameter direction and the second long diameter direction is in the range of 0°≤α≤30°, and the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles is in the range of 10%≤P1≤60%.

[0014] Furthermore, when or before the carbon source is pretreated at the first temperature, the method further comprises:

[0015] The carbon source is polished to perform a rounding treatment, wherein the rotation speed during the rounding treatment ranges from 40 r / min to 50 r / min.

[0016] Furthermore, the first temperature T1 is in the range of 500°C≤T1≤800°C; the second temperature T2 is in the range of 2800°C≤T2≤3500°C.

[0017] In a third aspect, an embodiment of the present application further provides a battery, comprising:

[0018] Electrolyte;

[0019] Positive electrode;

[0020] a diaphragm, the diaphragm being located on one side of the positive electrode plate, and

[0021] A negative electrode plate is arranged on a side of the diaphragm away from the positive electrode plate, and the negative electrode plate includes a negative electrode active layer, and the negative electrode active layer includes the graphite negative electrode particles described in the embodiment of the present application.

[0022] In a fourth aspect, an embodiment of the present application further provides an energy storage device, comprising:

[0023] include:

[0024] The housing; and

[0025] A plurality of batteries according to the embodiments of the present application are contained in the box.

[0026] The porosity P1 of the graphite negative electrode particles with a diameter greater than 10 μm in the embodiment of the present application is in the range of 10%≤P1≤60%, so that the graphite negative electrode particles have a lower expansion rate during the lithium insertion process; the graphite negative electrode particles have a plurality of pores, the plurality of pores are long strips, the maximum length direction of the pores is the first long diameter direction, the maximum length direction of the graphite negative electrode particles is the second long diameter direction, and the angle α between the first long diameter direction and the second long diameter direction is in the range of: 0°≤α≤30°, which can make the graphite negative electrode particles have a higher compaction density. By designing the porosity and the angle between the long diameter of the pores and the long diameter of the graphite negative electrode particles, the graphite negative electrode particles have a lower expansion rate and a higher compaction density, so that when applied to batteries, the batteries have a higher energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 It is a schematic diagram of the structure of graphite negative electrode particles according to an embodiment of the present application.

[0029] Figure 2 This is a scanning electron microscope image of the graphite negative electrode particles prepared in Example 2 of the present application.

[0030] Figure 3 It is a schematic diagram of a process for preparing graphite negative electrode particles according to an embodiment of the present application.

[0031] Figure 4 It is a schematic diagram of the structure of a battery according to an embodiment of the present application.

[0032] Figure 5 The battery of one embodiment of the present application is Figure 4 Schematic diagram of the cross-sectional structure in the AA direction.

[0033] Figure 6 It is a schematic diagram of the structure of the negative electrode plate of one embodiment of the present application.

[0034] Figure 7 It is a schematic diagram of the structure of the positive electrode plate of one embodiment of the present application.

[0035] Figure 8 It is a schematic structural diagram of an energy storage device according to an embodiment of the present application.

[0036] Description of reference numerals:

[0037] 100-graphite negative electrode particles, 10-pores, 300-battery, 310-positive electrode plate, 311-positive electrode current collector, 312-positive electrode active layer, 320-diaphragm, 330-negative electrode plate, 331-negative electrode current collector, 332-negative electrode active layer, 340-shell, 350-end cover assembly, 400-energy storage device, 410-case. DETAILED DESCRIPTION

[0038] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0039] The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.

[0040] The technical solutions in the embodiments of the present application will be described below in conjunction with the accompanying drawings.

[0041] It should be noted that, for the convenience of explanation, in the embodiments of the present application, the same figure marks represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments.

[0042] Energy storage lithium-ion batteries have increasingly higher requirements for energy efficiency performance. Improving energy efficiency performance mainly depends on improving the kinetics of the electrochemical system. Graphite is often used as the negative electrode material of lithium-ion batteries, but existing graphite materials are difficult to have both a low expansion rate and a high compaction density.

[0043] See also Figure 1 and Figure 2 The present application embodiment provides a graphite negative electrode particle 100, wherein the graphite negative electrode particle 100 has a plurality of pores 10, wherein the plurality of pores 10 are in the shape of long strips, and the maximum length direction of the pores 10 is the first major diameter direction (such as Figure 1The maximum length direction of the graphite negative electrode particles 100 is the second major diameter direction (as shown by the dashed line OO). Figure 1 The angle α between the first major axis direction and the second major axis direction is in the range of 0°≤α≤30°, and the porosity P1 of the graphite negative electrode particles 100 with a diameter greater than 10 μm is in the range of 10%≤P1≤60%.

[0044] The graphite negative electrode particle 100 of the embodiment of the present application can be used as, but not limited to, a negative electrode active material of a lithium ion battery.

[0045] It can be understood that the pore 10 is an elongated structure, that is, the length of the pore 10 is greater than the width of the pore 10 .

[0046] It should be noted that the graphite negative electrode particle 100 of the embodiment of the present application is an elongated structure or a long strip structure; in other words, the length of the graphite negative electrode particle 100 is greater than the width of the graphite particle.

[0047] It should be noted that, unless otherwise specified, the diameter of the graphite negative electrode particle 100 mentioned in the embodiments of the present application refers to the size of the graphite negative electrode particle 100 in the long diameter direction, that is, the maximum length of the graphite negative electrode particle 100 .

[0048] It can be understood that the angle α between the long diameter of the pore 10 and the long diameter of the graphite negative electrode particle 100 is in the range of 0°≤α≤30°.

[0049] Furthermore, the angle α between the first long axis direction and the second long axis direction may be, but is not limited to, less than or equal to 25°, less than or equal to 20°, less than or equal to 15°, less than or equal to 10°, etc.

[0050] Specifically, the angle α between the first long axis direction and the second long axis direction can be but is not limited to 0°, 3°5°, 8°, 10°, 13°, 15°, 18°, 20°, 23°, 25°, 28°, 30°, etc. The larger the angle α between the first long axis direction and the second long axis direction, the lower the powder compaction density of the graphite negative electrode particles 100. This is because when preparing the negative electrode sheet, during the cold pressing process, due to the orientation of the graphite negative electrode particles 100, the second long axis direction of the graphite negative electrode particles 100 tends to be arranged more parallel to the plane direction of the negative electrode collector. The larger the angle α between the first long axis direction and the second long axis direction, the stronger the inhibitory effect on the cold pressing external force, and the smaller the compaction density of the graphite negative electrode particles 100. However, the expansion force of the graphite negative electrode particles 100 during the lithium insertion process is mainly monitored in the thickness direction of the negative electrode sheet (also called the Z direction). The larger the angle α between the first long axis direction and the second long axis direction, the smaller the expansion force of the graphite negative electrode particles 100 during the lithium insertion process. The smaller the angle α between the first long diameter direction and the second long diameter direction, the greater the compaction density of the graphite negative electrode particles 100, and the greater the expansion force of the graphite negative electrode particles 100 during the lithium insertion process. In this embodiment, by making the angle α between the first long diameter direction and the second long diameter direction ≤ 30°, the graphite negative electrode particles 100 can have a higher compaction density and a lower expansion force, thereby reducing the risk of rupture of the solid electrolyte interface film (Solid Electrolyte Interface, referred to as SEI film) caused by the expansion of the graphite negative electrode particles 100 during the lithium insertion process, reducing the repeated consumption of active lithium during the cycle of the graphite negative electrode particles 100, thereby improving the cycle performance of the graphite negative electrode particles 100.

[0051] Furthermore, the angle α between the first long axis direction and the second long axis direction is in the range of 0°≤α≤15°. In this way, the graphite negative electrode particles 100 can have a higher compaction density and a lower expansion force.

[0052] Optionally, among the graphite negative electrode particles 100 , at least 50% or more of the particles having a diameter greater than 10 μm have a porosity ranging from 10% to 60%.

[0053] Specifically, the porosity P1 of the graphite negative electrode particles 100 with a diameter greater than 10 μm may be, but is not limited to, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc. If the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles 100 is too small, the graphite negative electrode particles 100 are prone to expand during the lithium insertion process, increasing the expansion rate of the graphite negative electrode particles 100; if the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles 100 is too large, on the one hand, the grain boundaries of the graphite negative electrode particles 100 will increase, and the compaction density and gram capacity of the graphite negative electrode particles 100 will be significantly reduced. On the other hand, since the grain boundaries of the graphite negative electrode particles 100 increase, the defects will also increase, which will induce more side reaction products, causing the by-products to accumulate on the surface of the graphite negative electrode particles 100, and the size of the graphite negative electrode particles 100 will increase, which will significantly deteriorate the expansion force of the battery using the graphite negative electrode particles 100.

[0054] The porosity P1 of the graphite negative electrode particles 100 with a diameter greater than 10 μm in the embodiment of the present application is in the range of 10%≤P1≤60%, so that the graphite negative electrode particles 100 have a lower expansion rate during the lithium insertion process; the graphite negative electrode particles 100 have a plurality of pores 10, the plurality of pores 10 are long strips, the maximum length direction of the pores 10 is the first long diameter direction, the maximum length direction of the graphite negative electrode particles 100 is the second long diameter direction, and the angle α between the first long diameter direction and the second long diameter direction is in the range of: 0°≤α≤30°, which can make the graphite negative electrode particles 100 have a higher compaction density. By designing the porosity and the angle between the long diameter of the pores 10 and the long diameter of the graphite negative electrode particles 100, the graphite negative electrode particles 100 have a lower expansion rate and a higher compaction density, so that when applied to a battery, the battery has a higher energy density.

[0055] In some embodiments, in the same graphite negative electrode particle 100 , the range of the angle β between any two pores 10 in the first major axis direction is: 0°≤β≤20°.

[0056] It can be understood that in the same graphite negative electrode particle 100, the first major axis directions of the plurality of pores 10 tend to extend in the same direction, that is, the extension directions of the plurality of pores 10 tend to be consistent, and the pores 10 tend to be arranged in parallel.

[0057] Specifically, in the same graphite negative electrode particle 100, the angle β between the first major axis directions of any two pores 10 can be, but is not limited to, 0°, 2°, 4°, 6°, 8°, 10°, 12°, 14°, 16°, 18°, 20°, etc.

[0058] In this embodiment, in the same graphite negative electrode particle 100, the smaller the angle β between the first long axis direction of any two pores 10 is, the more conducive it is to improving the compaction density of the graphite negative electrode particle 100; in the same graphite negative electrode particle 100, if the angle β between the first long axis direction of any two pores 10 is too large, it means that the isotropy of the single crystals in the graphite negative electrode particle 100 is relatively high and the anisotropy is reduced, thereby reducing the compaction density of the graphite negative electrode particle 100 and reducing the energy density of the battery.

[0059] In some embodiments, in the same graphite negative electrode particle 100 , the minimum distance d between two adjacent pores 10 is in the range of 0.5 μm≤d≤5 μm.

[0060] Specifically, within the same graphite negative electrode particle 100 , the minimum spacing d between two adjacent pores 10 may be, but is not limited to, 0.5 μm, 0.8 μm, 1.0 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, etc.

[0061] In this embodiment, in the same graphite negative electrode particle 100, if the minimum spacing d between two adjacent pores 10 is too small, there are too many pores 10 in the graphite negative electrode particle 100, which greatly increases the compaction density of the graphite negative electrode particle 100. In the same graphite negative electrode particle 100, if the minimum spacing d between two adjacent pores 10 is too large, it means that there are too few pores 10 in the graphite negative electrode particle 100, which will reduce the buffering capacity of the graphite negative electrode particle 100 during the lithium insertion process, increase the expansion force of the graphite negative electrode particle 100 during the lithium insertion process, and increase the expansion rate of the graphite negative electrode particle 100.

[0062] In some embodiments, the minimum length direction of the pore 10 is the short diameter direction, the size of the pore 10 along the first long diameter direction is smaller than the size of the pore 10 along the short diameter direction, and the size w1 of the pore 10 along the short diameter direction ranges from 0.5μm≤w1≤1μm.

[0063] It can be understood that the short diameter direction is perpendicular to the first long diameter direction.

[0064] Specifically, the size w1 of the pore 10 along the short diameter direction may be, but is not limited to, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 8 μm, 0.85 μm, 0.9 μm, 0.95 μm, 1 μm, etc. If the size w1 of the pore 10 along the short diameter direction is too small, the porosity of the graphite negative electrode particle 100 is reduced, thereby increasing the expansion force of the graphite negative electrode particle 100 during the lithium insertion process; the larger the size w1 of the pore 10 along the short diameter direction, the larger the space in the thickness direction of the negative electrode sheet when the graphite negative electrode particle 100 is applied to the battery, thereby reducing the compaction density of the graphite negative electrode particle 100, but in the process of lithium insertion of the graphite negative electrode particle 100, the larger the force release space of the lattice expansion is, the more significant the reduction of the expansion force is. When the size w1 of the pore 10 along the short diameter direction is in the range of 0.5 μm≤w1≤1 μm, the graphite negative electrode particle 100 can have a higher compaction density and a higher force release space when the graphite negative electrode particle 100 is embedded with lithium, thereby also making the graphite negative electrode particle 100 have a lower expansion force.

[0065] Optionally, a size w2 of the pore 10 along the first major axis direction is in the range of 3 μm≤w1≤20 μm.

[0066] Specifically, the size w2 of the pore 10 along the first major axis direction may be, but is not limited to, 3 μm, 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, etc.

[0067] In this embodiment, if the dimension w2 of the pore 10 along the first long axis direction is too small, the porosity of the graphite negative electrode particle 100 is reduced, thereby increasing the expansion force of the graphite negative electrode particle 100 during the lithium insertion process; if the dimension w2 of the pore 10 along the first long axis direction is too large, the compaction density and gram capacity of the graphite negative electrode particle 100 are reduced.

[0068] In some embodiments, the porosity P2 of the graphite negative electrode particles 100 with a diameter greater than or equal to 6 μm and less than or equal to 10 μm is in a range of 5%≤P2≤20%; the porosity P3 of the graphite negative electrode particles 100 with a diameter greater than or equal to 1 μm and less than 6 μm is in a range of 3%≤P2≤5%.

[0069] Specifically, the porosity P2 of the particles with a diameter greater than or equal to 6 μm and less than or equal to 10 μm in the graphite negative electrode particles 100 may be, but is not limited to, 5%, 6%, 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, etc. If the porosity P2 of the particles with a diameter greater than or equal to 6 μm and less than or equal to 10 μm in the graphite negative electrode particles 100 is too small, the graphite negative electrode particles 100 are prone to expansion during the lithium insertion process, increasing the expansion rate of the graphite negative electrode particles 100; if the porosity P2 of the particles with a diameter greater than or equal to 6 μm and less than or equal to 10 μm in the graphite negative electrode particles 100 is too large, the gram capacity and compaction density of the graphite negative electrode particles 100 are reduced.

[0070] Specifically, the porosity P3 of the particles with a diameter greater than or equal to 1 μm and less than 6 μm in the graphite negative electrode particles 100 may be, but is not limited to, 3%, 3.2%, 3.4%, 3.6%, 3.8%, 4%, 4%, 4.2%, 4.4%, 4.6%, 4.8%, 5%, etc. If the porosity P3 of the particles with a diameter greater than or equal to 1 μm and less than 6 μm in the graphite negative electrode particles 100 is too small, the graphite negative electrode particles 100 are prone to expansion during the lithium insertion process, increasing the expansion rate of the graphite negative electrode particles 100; if the porosity P3 of the particles with a diameter greater than or equal to 1 μm and less than 6 μm in the graphite negative electrode particles 100 is too large, the gram capacity and compaction density of the graphite negative electrode particles 100 are reduced.

[0071] In some embodiments, the graphite negative electrode particle 100 includes a plurality of layers stacked in sequence, and the first major axis direction of the pore 10 is parallel to the layers.

[0072] It can be understood that the pores 10 extend in the lamellae of the graphite negative electrode particles 100. The extending direction of the pores 10 is parallel to the extending direction of the lamellae of the graphite negative electrode particles 100.

[0073] In this embodiment, during the lithium insertion process of the graphite negative electrode particles 100, the graphite lattice expands, and the pores 10 extend within the lamellae of the graphite negative electrode particles 100, which can play a certain buffering role, reducing the expansion force of the graphite negative electrode particles 100 during the lithium insertion process, thereby reducing the risk of SEI film rupture caused by the expansion of the graphite negative electrode particles 100 during the lithium insertion process, reducing the repeated consumption of active lithium during the cycle of the graphite negative electrode particles 100, thereby improving the cycle performance of the graphite negative electrode particles 100.

[0074] Optionally, the range of D10 of the graphite negative electrode particles 100 is 2μm≤D10≤9μm, wherein D10 refers to the particle size corresponding to when the cumulative particle size distribution percentage of the graphite negative electrode particles 100 reaches 10%. Specifically, the D10 of the graphite negative electrode particles 100 can be, but is not limited to, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, etc.

[0075] Optionally, the range of D50 of the graphite negative electrode particles 100 is 8μm≤D50≤18μm, wherein D50 refers to the particle size corresponding to when the cumulative particle size distribution percentage of the graphite negative electrode particles 100 reaches 50%. Specifically, the D50 of the graphite negative electrode particles 100 can be, but is not limited to, 8μm, 9μm, 10μm, 12μm, 14μm, 16μm, 17μm, 18μm, etc.

[0076] Optionally, the range of D90 of the graphite negative electrode particles 100 is 20 μm ≤ D90 ≤ 35 μm, wherein D90 refers to the particle size corresponding to when the cumulative particle size distribution percentage of the graphite negative electrode particles 100 reaches 90%. Specifically, the D90 of the graphite negative electrode particles 100 can be, but is not limited to, 20 μm, 22 μm, 24 μm, 26 μm, 28 μm, 30 μm, 32 μm, 34 μm, 35 μm, etc.

[0077] Optionally, the range of D99 of the graphite negative electrode particles 100 is D99≤58μm, wherein D99 refers to the particle size corresponding to when the cumulative particle size distribution percentage of the graphite negative electrode particles 100 reaches 99%. Specifically, the D99 of the graphite negative electrode particles 100 can be, but is not limited to, 36μm, 38μm, 40μm, 42μm, 44μm, 46m, 48μm, 50μm, 52μm, 54μm, 56m, 58μm, etc.

[0078] The graphite negative electrode particles 100 of the embodiments of the present application can be prepared by the methods described in the following embodiments of the present application. In addition, they can also be prepared by other methods. The preparation methods of the embodiments of the present application are only one or more preparation methods of the graphite negative electrode particles 100 of the present application, and should not be understood as limiting the graphite negative electrode particles 100 provided in the embodiments of the present application.

[0079] See also Figure 3 The present application also provides a method for preparing graphite negative electrode particles 100, the preparation method comprising:

[0080] S201, providing a carbon source, wherein the mass fraction of volatile matter in the carbon source ranges from 3% to 15%;

[0081] Optionally, the carbon source may be, but is not limited to, at least one of petroleum coke, asphalt coke, coal coke, metallurgical coke, and the like.

[0082] Specifically, the mass fraction of volatile matter in the carbon source may be, but is not limited to, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc. If the mass fraction of volatile matter in the carbon source is too low, the porosity of the obtained graphite negative electrode particles 100 is too low, the impedance of the graphite negative electrode particles 100 is increased, the dynamic performance of the graphite negative electrode particles 100 is reduced, and the expansion force of the graphite negative electrode particles 100 in the lithium insertion process is increased, and the cycle performance of the graphite negative electrode particles 100 is reduced. If the mass fraction of volatile matter in the carbon source is too high, the compaction density of the obtained graphite negative electrode particles 100 is reduced, and the gram capacity and energy density of the graphite negative electrode particles 100 are reduced.

[0083] S202, pre-treating the carbon source at a first temperature to obtain intermediate particles; and

[0084] S203, graphitizing the intermediate particles at a second temperature to obtain the graphite negative electrode particles 100, wherein the first temperature is lower than the second temperature, wherein the graphite negative electrode particles 100 have a plurality of pores 10, the plurality of pores 10 are in the shape of long strips, the maximum length direction of the pores 10 is the first long axis direction, the maximum length direction of the graphite negative electrode particles 100 is the second long axis direction, the angle α between the first long axis direction and the second long axis direction is in the range of 0°≤α≤30°, and the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles 100 is in the range of 10%≤P1≤60%.

[0085] For a detailed description of other features of the graphite negative electrode particles 100 , please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.

[0086] The porosity P1 of the graphite negative electrode particles 100 with a diameter greater than 10 μm obtained by the preparation method of the graphite negative electrode particles 100 of the embodiment of the present application is in the range of 10%≤P1≤60%, so that the graphite negative electrode particles 100 have a lower expansion rate during the lithium insertion process; the graphite negative electrode particles 100 have a plurality of pores 10, the plurality of pores 10 are long strips, the maximum length direction of the pores 10 is the first long diameter direction, the maximum length direction of the graphite negative electrode particles 100 is the second long diameter direction, and the angle α between the first long diameter direction and the second long diameter direction is in the range of: 0°≤α≤30°, which can make the graphite negative electrode particles 100 have a higher compaction density. By designing the porosity and the angle between the long diameter of the pores 10 and the long diameter of the graphite negative electrode particles 100, the graphite negative electrode particles 100 have a lower expansion rate and a higher compaction density, so that when applied to a battery, the battery has a higher energy density.

[0087] Optionally, in S201, providing a carbon source includes: crushing the carbon source.

[0088] Optionally, the carbon source is coarsely crushed by a jaw crusher and ground into fine powder by a jet mill to obtain aggregate particles of the carbon source with a median particle size Dv50 ranging from 6 μm to 18 μm.

[0089] Specifically, the median particle size Dv50 of the aggregate particles of the carbon source may be, but is not limited to, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, etc. The larger the median particle size Dv50 of the aggregate particles of the carbon source, the larger the range of the spacing between two adjacent pores 10 in the multiple pores 10 of the obtained graphite negative electrode particles 100, and the fewer pores 10 in the graphite negative electrode particles 100, which will reduce the buffering capacity of the graphite negative electrode particles 100 during the lithium insertion process, increase the expansion force of the graphite negative electrode particles 100 during the lithium insertion process, and increase the expansion rate of the graphite negative electrode particles 100.

[0090] Furthermore, the median particle size Dv50 of the aggregate particles of the carbon source ranges from 8 μm to 123 μm. This allows the obtained graphite negative electrode particles 100 to have a higher compaction density and better buffering capacity during the lithium insertion process, which can better reduce the expansion rate of the graphite negative electrode particles 100 during the lithium insertion process.

[0091] In some embodiments, when the carbon source is pretreated at the first temperature or before the carbon source is pretreated at the first temperature, the method further includes: polishing the carbon source to perform rounding treatment, wherein the rotation speed during rounding treatment ranges from 40r / min to 50r / min.

[0092] Optionally, the carbon source is subjected to a filleting treatment in a horizontal kettle.

[0093] Specifically, the rotation speed during the rounding treatment may be, but is not limited to, 40 r / min, 42 r / min, 44 r / min, 46 r / min, 48 r / min, 50 r / min, etc. Grinding the carbon source for rounding treatment can make the edge corners of the obtained graphite negative electrode particles 100 better, improve the compaction density of the obtained graphite negative electrode particles 100, and improve the processing performance of the graphite negative electrode particles 100. When the rotation speed during the rounding treatment is too low, the edge corners of the carbon source will not be shaped, and the compaction density will be low during rolling; when the rotation speed during the rounding treatment is too high, the angle α between the first long diameter direction and the second long diameter direction of the obtained graphite negative electrode particles 100 will be too large, which will also reduce the compaction density of the graphite negative electrode particles 100, but will also reduce the expansion force of the graphite negative electrode particles 100 during the lithium insertion process. When the rotation speed during the rounding treatment is in the range of 40 r / min to 50 r / min, the obtained graphite negative electrode particles 100 can have a higher compaction density and a lower expansion force during the lithium insertion process.

[0094] It should be noted that the grinding of the carbon source for rounding can be performed before the carbon source is pretreated at the first temperature, or can be performed simultaneously with the pretreatment step. In other words, the pretreatment process can be carried out in a horizontal kettle, and this application does not make specific limitations.

[0095] Optionally, in S201, the first temperature T1 is in the range of 500°C≤T1≤800°C. That is, the pretreatment temperature T1 is in the range of 500°C≤T1≤800°C.

[0096] Specifically, the first temperature T1 may be, but is not limited to, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, etc. In this embodiment, if the pretreatment temperature is too low, it will not have a significant effect on the volatilization of volatiles, and will not play a role in internal pore formation, thereby reducing the porosity of the obtained graphite negative electrode particles 100, thereby increasing the expansion force of the graphite negative electrode particles 100 during the lithium insertion process; if the pretreatment temperature is too high, the preparation cost of the graphite negative electrode particles 100 will be increased, and in addition, the short diameter size of the pores 10 in the obtained graphite negative electrode particles 100 will be increased, and the compaction density of the graphite negative electrode particles 100 will be reduced.

[0097] Optionally, the pretreatment time ranges from 2 hours to 4 hours. Specifically, the pretreatment time may be, but is not limited to, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, etc. If the pretreatment time is too short, too little volatile matter is removed; if the pretreatment time is too long, the preparation cost of the graphite negative electrode particles 100 is increased.

[0098] Optionally, in S203, the graphitizing the intermediate particles at a second temperature includes: placing the intermediate particles in a graphite crucible, and graphitizing them in a graphitization furnace at a second temperature T2 in the range of 2800°C ≤ T2 ≤ 3500°C, wherein the height of the graphite crucible is in the range of 100 cm to 140 cm, and the filling height of the intermediate particles in the graphite crucible is 70% to 90% of the height of the graphite crucible.

[0099] Optionally, the height of the graphite crucible may be, but is not limited to, 100 cm, 105 cm, 110 cm, 115 cm, 120 cm, 125 cm, 130 cm, 135 cm, 140 cm, etc. Increasing the height of the graphite crucible is beneficial to improving the porosity of the obtained graphite negative electrode particles 100 .

[0100] Optionally, the filling height of the intermediate particles in the graphite crucible is 70%, 75%, 80%, 85%, 90% of the height of the graphite crucible, etc. The smaller the filling height ratio of the intermediate particles in the graphite crucible, the more conducive it is to improve the porosity of the obtained graphite negative electrode particles 100.

[0101] Optionally, in S202, the second temperature T2 is in the range of 2800°C≤T2≤3500°C. That is, the temperature of the graphitization treatment is in the range of 2800°C≤T2≤3500°C. Specifically, the second temperature T2 may be, but is not limited to, 2800°C, 2850°C, 2900°C, 2950°C, 3000°C, 3050°C, 3100°C, 3150°C, 3200°C, 3250°C, 3300°C, 3350°C, 3400°C, 3450°C, 3500°C, etc. If the temperature of the graphitization treatment is too low, the degree of graphitization of the graphite negative electrode particles 100 is reduced, the conductivity of the graphite negative electrode particles 100 is reduced, and thus the dynamic performance of the graphite negative electrode particles 100 is reduced; if the temperature of the graphitization treatment is too high, the preparation cost of the graphite negative electrode particles 100 is increased.

[0102] Optionally, the holding time of the graphitization treatment ranges from 12h to 24h. Specifically, the holding time of the graphitization treatment may be, but is not limited to, 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc. If the holding time of the graphitization treatment is too short, the graphitization degree of the obtained graphite negative electrode particles 100 is too low, which reduces the conductivity of the graphite negative electrode particles 100, thereby reducing the kinetic performance of the graphite negative electrode particles 100; if the holding time of the graphitization treatment is too long, the preparation cost of the graphite negative electrode particles 100 is increased.

[0103] See also Figures 4 to 6The embodiment of the present application also provides a battery 300, which includes an electrolyte, a positive electrode plate 310, a separator 320 and a negative electrode plate 330, wherein the separator 320 is located on one side of the positive electrode plate 310, and the negative electrode plate 330 is arranged on the side of the separator 320 away from the positive electrode plate 310, and the negative electrode plate 330 includes a negative electrode active layer 332, and the negative electrode active layer 332 includes the graphite negative electrode particles 100 described in the embodiment of the present application.

[0104] It can be understood that the positive electrode plate 310 , the separator 320 , and the negative electrode plate 330 are at least partially immersed in the electrolyte.

[0105] It can be understood that the positive electrode sheet 310, the separator 320 and the negative electrode sheet 330 are stacked in sequence to form an electrode assembly. The electrode assembly can be, but is not limited to, a winding structure, a laminated structure, etc., which is not specifically limited in the present application.

[0106] Optionally, the negative electrode sheet 330 further includes a negative electrode current collector 331 , and the negative electrode active layer 332 is disposed on the surface of the negative electrode current collector 331 . It can be understood that the negative electrode active layer 332 can cover one surface or two opposite surfaces of the negative electrode current collector 331 .

[0107] Optionally, the negative electrode current collector 331 may be, but is not limited to, a copper sheet.

[0108] Optionally, the negative electrode active layer 332 further includes a negative electrode conductor, a negative electrode binder and a negative electrode thickener.

[0109] See also Figure 7 Optionally, the positive electrode sheet 310 includes a positive current collector 311 and a positive active layer 312, and the positive active layer 312 is disposed on the surface of the positive current collector 311. It can be understood that the positive active layer 312 can cover one surface or two opposite surfaces of the positive current collector 311.

[0110] Optionally, the positive electrode current collector 311 may be, but is not limited to, an aluminum sheet.

[0111] Optionally, the positive electrode active layer 312 includes a positive electrode active material, a positive electrode conductor, a positive electrode binder and a positive electrode thickener.

[0112] Optionally, the positive electrode active material may be, but is not limited to, lithium iron phosphate.

[0113] Optionally, the diaphragm 320 may be, but is not limited to, at least one of a polypropylene film (PP film for short), a polyethylene film (PE film for short), a ceramic diaphragm 320 , and the like.

[0114] Optionally, the battery 300 further includes a shell 340 and an end cap assembly 350, wherein the shell 340 and the end cap assembly 350 enclose a closed receiving chamber for receiving the electrolyte, the positive electrode sheet 310, the diaphragm 320 and the negative electrode sheet 330. It can be understood that the end cap assembly 350 is electrically connected to the positive electrode sheet 310 and the negative electrode sheet 330, respectively, and the positive electrode sheet 310 and the negative electrode sheet 330 are led out to be electrically connected to an external device or other battery 300.

[0115] The graphite negative electrode particles 100 and the battery 300 of the embodiment of the present application are further described below through specific examples.

[0116] Example 1

[0117] The graphite negative electrode particles 100 of this embodiment are prepared by the following steps:

[0118] (1) providing petroleum coke having a mass fraction of volatile matter of 5%, crushing the petroleum coke by a jaw crusher, and grinding the petroleum coke into fine powder by a jet mill to obtain a carbon source aggregate, wherein the Dv50 of the carbon source aggregate is 8 um;

[0119] (2) placing the aggregate of the carbon source in a horizontal kettle and pre-treating it at 600° C. to obtain intermediate particles, wherein the rotation speed of the horizontal kettle is 40 r / min; and

[0120] (3) The intermediate particles are placed in a graphite crucible with a height of 100 cm, and the filling height of the intermediate particles is 90% of the height of the graphite crucible. A graphitization process is performed in a graphite furnace at 3100° C. to obtain graphite negative electrode particles 100.

[0121] Example 2

[0122] The difference between this embodiment and embodiment 1 is that the mass fraction of the volatile matter of the tar oil is 10%.

[0123] During the graphitization process, the height of the graphite crucible is 120 cm, and the intermediate particle filling height is 80% of the height of the graphite crucible.

[0124] Example 3

[0125] The difference between this embodiment and embodiment 1 is that the mass fraction of the volatile matter in the petroleum tar is 15%.

[0126] During the graphitization process, the height of the graphite crucible is 140 cm, and the intermediate particle filling height is 70% of the height of the graphite crucible.

[0127] Example 4

[0128] The difference between this embodiment and embodiment 1 is that the rotation speed of the horizontal kettle is 0.

[0129] During the graphitization process, the height of the graphite crucible is 120 cm, and the filling height of the intermediate particles is 80% of the graphite crucible.

[0130] Example 5

[0131] The difference between this embodiment and embodiment 1 is that the rotation speed of the horizontal kettle is 45 r / min.

[0132] During the graphitization process, the height of the graphite crucible is 120 cm, and the filling height of the intermediate particles is 80% of the graphite crucible.

[0133] Example 6

[0134] The difference between this embodiment and embodiment 1 is that the pretreatment temperature is 700°C.

[0135] During the graphitization process, the height of the graphite crucible is 120 cm, and the filling height of the intermediate particles is 80% of the graphite crucible.

[0136] Example 7

[0137] The difference between this embodiment and embodiment 1 is that the pretreatment temperature is 800°C.

[0138] During the graphitization process, the height of the graphite crucible is 120 cm, and the filling height of the intermediate particles is 80% of the graphite crucible.

[0139] Example 8

[0140] The difference between this embodiment and embodiment 1 is that the Dv50 of the carbon source aggregate is 10 um.

[0141] During the graphitization process, the height of the graphite crucible is 120 cm, and the filling height of the intermediate particles is 80% of the graphite crucible.

[0142] Example 9

[0143] The difference between this embodiment and embodiment 1 is that the Dv50 of the carbon source aggregate is 15 um.

[0144] During the graphitization process, the height of the graphite crucible is 120 cm, and the filling height of the intermediate particles is 80% of the graphite crucible.

[0145] Comparative Example 1

[0146] The difference between this comparative example and Example 1 is that the mass fraction of the volatile matter of the petroleum tar is 18%, and the Dv50 of the carbon source aggregate is 18 um.

[0147] During the graphitization process, the height of the graphite crucible is 150 cm, and the intermediate particle filling height is 65% of the graphite crucible.

[0148] Comparative Example 2

[0149] The difference between this comparative example and Example 1 is that the rotation speed of the horizontal kettle is 55 r / min.

[0150] During the graphitization process, the height of the graphite crucible is 120 cm, and the filling height of the intermediate particles is 80% of the graphite crucible.

[0151] The graphite negative electrode particles 100 of each embodiment and comparative example are assembled into a square shell battery 300: the negative electrode sheets 330 are respectively made using the graphite negative electrode particles 100 prepared in each embodiment and comparative example, and the negative electrode sheets 330, the polypropylene separator 320, the lithium iron phosphate positive electrode sheet 310 and the lithium hexafluorophosphate electrolyte with a concentration of 1 mol / L are assembled into a soft-pack battery 300.

[0152] Various performance tests were performed on the graphite negative electrode particles 100 of various embodiments and comparative examples and the batteries 300 assembled therefrom. The test results are shown in Table 1 below.

[0153] (1) Porosity test: After disassembling the battery 300, select the outermost fold, middle fold, and innermost fold of the negative electrode sheet 330, and further select the negative electrode sheet 330 on the tab side, the middle position, and the opposite side of the tab of each fold of the negative electrode sheet 330 for ion milling-scanning electron microscope test (CP+SEM test for short). Select 5 pictures at different field of view positions at 1KX magnification, use NanoMeasurer software to measure the size of the porosity of each picture, and finally calculate the internal porosity of the graphite negative electrode particle 100. The diameter of the graphite negative electrode particle 100 is measured by the longest diameter (i.e., the maximum length) of the particle using the same software.

[0154] (2) The angle α between the first long axis and the second long axis, the dimension w1 of the short axis, the distance d between two adjacent pores 10, etc. are measured by using a scanning electron microscope (SEM). Figure 2As shown. In each embodiment and comparative example, when measuring the angle α between the first long axis direction and the second long axis direction, 100 graphite negative electrode particles 100 are taken, and the average values ​​of the first long axis direction and the second long axis direction on each graphite negative electrode particle 100 are calculated respectively, and the average value of the angle α between the first long axis direction and the second long axis direction in the 100 particles is obtained as the angle α between the first long axis direction and the second long axis direction of the graphite negative electrode particles 100 of the embodiment or comparative example. When measuring the size w1 in the short axis direction, 100 pores 10 are taken, and the size in the short axis direction of each pore 10 is averaged as the w1 of the graphite negative electrode particles 100 of the embodiment or comparative example. When measuring the distance d between two adjacent pores 10, 100 pores 10 are taken, and the average value of the distance between any two adjacent pores 10 is obtained as the d of the graphite negative electrode particles 100 of the embodiment or comparative example.

[0155] (3) Powder compaction density test: 2 to 3 g of graphite negative electrode particles 100 are added to a mold with a diameter of 13 mm. After pressurizing to 5 tons, the pressure is maintained for 10 seconds and then released. The mass and volume of the pressed cylinder are measured, and the powder compaction density is calculated.

[0156] (4) Expansion force test after 500 cycles: During the cycle, the battery 300 is mounted with a fixture, which is set to a three-layer structure, wherein a stress sensor is installed between the upper two layers, and the lower two layers of plates fix the lithium-ion battery 300. During the cycle, when the lithium-ion battery 300 expands due to thickness changes, the pressure sensor on the upper layer converts the position signal into a mechanical signal to obtain the expansion force at this time, and measures the expansion force of the battery 300 after 500 cycles.

[0157] Table 1 Performance parameters of each embodiment and comparative example

[0158]

[0159] From the test results of Example 1 to Example 3, it can be seen that the higher the mass fraction of the volatile matter of the carbon source, the higher the height of the graphite crucible, the smaller the proportion of the height filled by the intermediate particles, and the greater the porosity of the obtained graphite negative electrode particles 100. In addition, as the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles 100 increases, the powder compaction density of the graphite negative electrode particles 100 gradually decreases. This is because the porosity occupies a certain volume space. Although the graphite negative electrode particles 100 are soft, during the cold pressing process, the graphite negative electrode particles 100 will have a certain compression along the thickness direction (also known as the Z direction) of the negative electrode sheet 330, but the greater the porosity of the graphite negative electrode particles 100, the larger the space occupied by the pores 10, and the smaller the mass under the same volume, which in turn affects the use of the graphite negative electrode particles 100 in a high volume energy density system. However, since the porosity has a certain stress release effect, during the cyclic lithium insertion process of the graphite negative electrode particles 100, the lattice expansion caused by the lithium insertion will be partially released due to the existence of the pores 10 inside the graphite negative electrode particles 100, thereby showing a trend that the expansion force of the graphite negative electrode particles 100 decreases significantly with the increase of the pores 10.

[0160] From the test results of Example 2, Example 4, Example 5 and Comparative Example 2, it can be seen that when the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles 100 remains unchanged, as the angle α between the first long diameter direction and the second long diameter direction increases, the powder compaction density of the graphite negative electrode particles 100 gradually decreases. This is because during the cold pressing process, due to the orientation of the graphite negative electrode particles 100, the direction of the maximum length of the graphite negative electrode particles 100 tends to be arranged more parallel to the negative electrode collector 331. If the angle α between the first long diameter direction and the second long diameter direction is larger, the suppression effect on the cold pressing external force is stronger, and the powder compaction density will be smaller. At the same time, the larger the angle α between the first long diameter direction and the second long diameter direction, the smaller the force exhibited in the Z direction, so that the expansion force of the battery 300 using the graphite negative electrode particles 100 will also be smaller. When the angle α between the first long axis direction and the second long axis direction is too large, the powder compaction density of the prepared graphite negative electrode particles 100 will be too low, which is not conducive to improving the energy density of the battery 300 .

[0161] It can be seen from the test results of Example 1, Example 6 and Example 7 that with the increase of the pretreatment temperature, the porosity of the obtained graphite negative electrode particles 100 gradually increases, the size w1 of the short diameter direction of the pores 10 also gradually increases, the compaction density of the graphite negative electrode particles 100 gradually decreases, and the expansion force generated by the battery 300 using the graphite negative electrode particles 100 during the cycle process also gradually decreases; however, it has little effect on the spacing between adjacent pores 10.

[0162] It can be seen from the test results of Example 2, Example 6 and Example 7 that when the angle α between the first long axis direction and the second long axis direction of the graphite negative electrode particle 100 remains unchanged, as the size w1 of the pore 10 inside the graphite negative electrode particle 100 along the short axis direction increases, the powder compaction density of the graphite negative electrode particle 100 gradually decreases. This is because the size w1 of the pore 10 along the short axis direction increases, which means that the larger the space in the Z direction, the smaller the powder compaction density; and because the space in the Z direction is large, the force release space for the lattice expansion caused by lithium insertion is larger, and the reduction of the expansion force is more significant.

[0163] It can be seen from the test results of Example 2, Example 8 and Example 9 that when the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles 100, the angle α between the first major axis direction and the second major axis direction, and the size w1 of the pore 10 along the minor axis direction remain unchanged, as the distance d between two adjacent pores 10 in the same graphite negative electrode particle 100 increases, the powder compaction density of the graphite negative electrode particle 100 gradually increases, which is mainly reflected in the decrease in the number of pores 10 in the Z direction; and the decrease in the number of pores 10 will affect the release of the lattice expansion force, resulting in an increase in the expansion force.

[0164] It can be seen from the test results of Example 1 and Comparative Example 1 that when the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles 100 is too large, this will increase the number of grain boundaries of the graphite negative electrode particles 100, and the compaction density of the graphite negative electrode particles 100 will be significantly reduced. In addition, since the number of grain boundaries of the graphite negative electrode particles 100 increases, the number of defects will also increase, which will induce more side reaction products, causing the by-products to accumulate on the surface of the graphite negative electrode particles 100, and the size of the graphite negative electrode particles 100 will increase, which will significantly deteriorate the expansion force of the battery 300 using the graphite negative electrode particles 100.

[0165] See also Figure 8 The embodiment of the present application further provides an energy storage device 400 , which includes a box body 410 and the battery 300 described in the embodiment of the present application, and the multiple batteries 300 are accommodated in the box body 410 .

[0166] The energy storage device 400 of the present application can be applied to, but is not limited to, energy storage on the power generation side, energy storage on the power grid side, and energy storage on the power consumption side.

[0167] The term "plurality" means greater than or equal to two.

[0168] It can be understood that the multiple batteries 300 of the energy storage device 400 can be connected in parallel with each other; or in series with each other; or partially in parallel and partially in series (in other words, mixed connection). This application does not make any specific restrictions on the connection method of the multiple batteries 300 of the same energy storage device 400.

[0169] It can be understood that the box body 410 has a receiving cavity, and multiple batteries 300 are received in the receiving cavity. In some embodiments, each receiving cavity receives one battery 300. In other embodiments, each receiving cavity receives multiple batteries 300.

[0170] Optionally, the energy storage device 400 may include but is not limited to a battery 300 module, a battery 300 pack, a battery 300 system, etc. The actual application form of the energy storage device 400 provided in the embodiment of the present application may be but is not limited to the listed products, and may also be other application forms. The embodiment of the present application does not strictly limit the application form of the energy storage device 400. The embodiment of the present application only takes the energy storage device 400 as a multi-core battery 300 as an example for explanation. When the energy storage device 400 is a single battery 300, the energy storage device 400 may be at least one of a cylindrical battery 300, a square battery 300, etc.

[0171] Mentioning "embodiment" and "implementation method" in this application means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrases in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should also be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, provided that there is no contradiction between them.

[0172] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the above preferred implementation modes, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.

Claims

1. A graphite negative electrode particle, characterized in that: The graphite negative electrode particles have a plurality of pores, the plurality of pores are in the shape of long strips, the maximum length direction of the pores is the first long diameter direction, the maximum length direction of the graphite negative electrode particles is the second long diameter direction, the range of the angle α between the first long diameter direction and the second long diameter direction is: 0°≤α≤30°, and the range of the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles is 10%≤P1≤60%.

2. The graphite negative electrode particle according to claim 1, characterized in that: In the same graphite negative electrode particle, the range of the angle β between any two pores in the first major axis direction is: 0°≤β≤20°.

3. The graphite negative electrode particle according to claim 1, characterized in that: In the same graphite negative electrode particle, the distance d between two adjacent pores is in the range of 0.5 μm≤d≤5 μm.

4. The graphite negative electrode particle according to claim 1, characterized in that: The minimum length direction of the pore is the short diameter direction, the size of the pore along the first long diameter direction is smaller than the size of the pore along the short diameter direction, the size w1 of the pore along the short diameter direction is in the range of 0.5μm≤w1≤1μm; the size w2 of the pore along the first long diameter direction is in the range of 3μm≤w1≤20μm.

5. The graphite negative electrode particle according to claim 1, characterized in that: The porosity P2 of the graphite negative electrode particles with a diameter greater than or equal to 6 μm and less than or equal to 10 μm is in the range of 5%≤P2≤20%; the porosity P3 of the graphite negative electrode particles with a diameter greater than or equal to 1 μm and less than 6 μm is in the range of 3%≤P2≤5%.

6. The graphite negative electrode particle according to any one of claims 1 to 5, characterized in that: The graphite negative electrode particles include multiple layers stacked in sequence, and the first major axis direction of the pores is parallel to the layers.

7. A method for preparing graphite negative electrode particles, characterized in that: The preparation method comprises: Providing a carbon source, wherein the mass fraction of volatile matter in the carbon source ranges from 3% to 15%; pre-treating the carbon source at a first temperature to obtain intermediate particles; and The intermediate particles are graphitized at a second temperature to obtain the graphite negative electrode particles, wherein the first temperature is lower than the second temperature, wherein the graphite negative electrode particles have a plurality of pores, the plurality of pores are in the shape of long strips, the maximum length direction of the pores is the first long diameter direction, the maximum length direction of the graphite negative electrode particles is the second long diameter direction, the angle α between the first long diameter direction and the second long diameter direction is in the range of 0°≤α≤30°, and the porosity P1 of the particles with a diameter greater than 10 μm in the graphite negative electrode particles is in the range of 10%≤P1≤60%.

8. The method for preparing graphite negative electrode particles according to claim 7, characterized in that: When the carbon source is pretreated at the first temperature or before the carbon source is pretreated at the first temperature, the method further comprises: The carbon source is polished to perform a rounding treatment, wherein the rotation speed during the rounding treatment ranges from 40 r / min to 50 r / min.

9. The method for preparing graphite negative electrode particles according to claim 7, characterized in that: The first temperature T1 is in the range of 500°C≤T1≤800°C; The graphitizing the intermediate particles at a second temperature comprises: placing the intermediate particles in a graphite crucible, and graphitizing them in a graphitization furnace at a second temperature T2 in the range of 2800°C≤T2≤3500°C, wherein the height of the graphite crucible is in the range of 100cm to 140cm, and the filling height of the intermediate particles in the graphite crucible is 70% to 90% of the height of the graphite crucible.

10. A battery, characterized in that: include: Electrolyte; Positive electrode; a diaphragm, the diaphragm being located on one side of the positive electrode plate, and A negative electrode plate, wherein the negative electrode plate is arranged on a side of the separator away from the positive electrode plate, the negative electrode plate comprises a negative electrode active layer, and the negative electrode active layer comprises the graphite negative electrode particles according to any one of claims 1 to 6.

11. An energy storage device, characterized in that: include: include: The housing; and A plurality of batteries according to claim 10, wherein the plurality of batteries are housed in the casing.

Citation Information

Patent Citations

  • Graphite material, method for producing same, carbon material for battery electrodes, and battery

    CN103328378A

  • Preparation method of porous nano metal with controllable porosity

    CN108326306A

  • Artificial graphite, secondary battery, preparation method, and device

    CN113207316A

  • Negative electrode particle and preparation method thereof, negative electrode plate and energy storage device

    CN116314729A

  • Negative active particle and preparation method thereof, negative pole piece and battery

    CN117673355A

Cited By

  • Graphite negative electrode particles, preparation method therefor, battery, and energy storage apparatus

    WO2026016850A1