Preparation method of water-soluble platinum-carbon catalyst

A water-soluble platinum-carbon catalyst was prepared by acidification treatment of hydrophilic carbon black support, ultrasonic dispersion and high-temperature reaction, which solved the corrosion resistance and dispersibility problems of graphitized carbon support, achieved efficient dispersion and stability of catalyst, and improved the catalytic performance of fuel cell.

CN118943390AInactive Publication Date: 2024-11-12JI YONG QING NENG YUAN KE JI (JIANG SU) YOU XIAN GONG SI

Patent Information

Application Number
CN202411141997.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Among existing commercial fuel cell catalysts, graphitized carbon supports have poor corrosion resistance, poor water solubility, uneven platinum particle dispersion, and are difficult to prepare in large quantities.

Method used

A water-soluble platinum-carbon catalyst was prepared by using hydrophilic carbon black as a carrier and through acidification, ultrasonic dispersion, high-temperature reaction and washing processes. This process ensures the hydrophilicity of the carbon black surface and the dispersibility of platinum nanoparticles, avoids agglomeration, and improves the stability and activity of the catalyst.

Benefits of technology

It improves the hydrophilicity and dispersibility of the catalyst, enhances its activity and durability, simplifies the preparation process, and ensures the purity and repeatability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943390A_ABST
    Figure CN118943390A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of noble metal nano catalytic materials, in particular to a preparation method of a water-soluble platinum-carbon catalyst, which comprises a preparation method of a platinum-carbon catalyst, the preparation method of the platinum-carbon catalyst comprises the steps of 1, 2, 3, 4, 5 and 6, the step 1 comprises material preparation of hydrophilic carbon black; weighing a certain amount of ultrapure water, placing the ultrapure water for later use, weighing a proper amount of carbon black on weighing paper, pouring the carbon black into a beaker with the weighed water, and shaking to completely infiltrate the catalyst; according to the preparation method of the water-soluble platinum-carbon catalyst provided by the invention, through acidification treatment and high-temperature reaction, the surface property of carbon black is remarkably improved, and the hydrophilicity of the carbon black is increased, so that the catalyst can be better dispersed and stabilized in a water-phase reaction system, the catalytic efficiency is improved, and the water-soluble platinum-carbon catalyst can be prepared through a strict post-treatment process. And by washing and vacuum drying, the stability and durability of the catalyst are ensured, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of precious metal nanocatalytic materials, and in particular to a method for preparing a water-soluble platinum-carbon catalyst. Background Art

[0002] At present, commercial fuel cell catalysts are still mainly platinum-carbon catalysts. Studies have shown that the corrosion resistance of platinum-carbon catalysts supported by traditional carbon black carriers is poor, while catalysts based on graphitized carbon carriers can effectively improve the durability of the carrier. However, there are very few oxygen-containing functional groups on the surface of graphitized carbon carriers, which leads to very poor compatibility of this type of carbon carrier with aqueous solutions. Especially when preparing catalysts in batches, it is more difficult to disperse graphitized carbon carriers above 100 grams in water. In addition, the adsorption effect between the graphitized carbon surface and platinum particles is small, and the problem of weak interaction between highly graphitized structural carbon and metal ions has emerged. In addition, the batch preparation of catalysts still faces many problems and challenges, including poor dispersion of platinum particles on carbon carriers, easy agglomeration of carbon carrier particles, and difficulty in batch preparation. Summary of the Invention

[0003] In order to solve some problems existing in the above-mentioned prior art, the present invention provides a method for preparing a water-soluble platinum-carbon catalyst to solve the shortcomings existing in the above-mentioned prior art.

[0004] To achieve the above-mentioned purpose, the present invention provides a method for preparing a water-soluble platinum-carbon catalyst, including a method for preparing a platinum-carbon catalyst. The method for preparing the platinum-carbon catalyst includes steps one, two, three, four, five and six. Step one includes preparing the materials of hydrophilic carbon black, weighing a certain amount of ultrapure water and setting it aside for later use, then weighing an appropriate amount of carbon black on weighing paper and pouring it into a beaker filled with water, and shaking it to completely soak the catalyst.

[0005] As a further improvement of the present invention, in order to facilitate the provision of a uniform carbon black suspension for subsequent acid treatment and ensure the consistency of the acid treatment effect, the step 2 includes acidification treatment, wherein appropriate amounts of nitric acid and sulfuric acid are weighed in a certain proportion, respectively measured with a graduated cylinder, and then mixed evenly in another container. The mixed acid solution is slowly and evenly added dropwise to the carbon black suspension, while gently stirring with a glass rod to form a mixed solution.

[0006] As a further improvement of the present invention, in order to avoid agglomeration caused by excessive local concentration and ensure the repeatability and stability of catalyst preparation, the step three includes ultrasonic dispersion, placing the carbon black suspension with the mixed acid into an ultrasonic disperser, setting appropriate ultrasonic power and dispersion time, and the dispersion time should be adjusted according to the type, particle size and desired hydrophilicity of the carbon black. It is generally recommended to be between 30 minutes and 180 minutes. During the ultrasonic dispersion process, the state of the suspension should be checked regularly.

[0007] As a further improvement to the present invention, in order to more effectively load platinum nanoparticles and form a highly dispersed platinum-carbon catalyst, step four includes a high-temperature reaction, transferring the dispersed carbon black suspension to a polytetrafluoroethylene reactor, and sealing the reactor lid. The reactor is placed in a heating device, set to a temperature of 150°C, for a high-temperature reaction. The high-temperature reaction can accelerate the chemical reaction between the acid and the carbon black, further increasing the hydrophilicity of the carbon black. The reaction time is generally set to 3 hours to ensure that the reaction proceeds fully. During the reaction process, the pressure and temperature of the reactor should be checked regularly to ensure that they are operating within a safe range.

[0008] As a further improvement of the present invention, in order to resist chemical erosion and physical wear during the reaction process, step five includes washing the hydrophilic catalyst layer, pouring the cooled product after the reaction into a filter press, pouring 1-3 L of deionized water into it, and filtering to a conductivity of 20-40 μS / m.

[0009] As a further improvement of the present invention, in order to conveniently remove impurities and unreacted acid on the surface of the catalyst and ensure the purity of the catalyst, step six includes a drying process, in which the filtered catalyst is placed in a vacuum drying oven for drying at a drying temperature of 60-100°C. After drying for 10-30 hours, the catalyst is taken out for grinding and collection.

[0010] When the present invention is working, first, a certain amount of ultrapure water needs to be prepared and placed in a clean container for standby use; then, an appropriate amount of carbon black is accurately weighed on a weighing paper to avoid contact with impurities in the air; the weighed carbon black is slowly poured into a beaker filled with ultrapure water, and the carbon black particles are completely immersed in the water by gently shaking the beaker; the purpose of this step is to provide a uniform carbon black suspension for subsequent acid treatment to ensure the consistency of the acid treatment effect; a certain proportion of nitric acid and sulfuric acid mixture needs to be prepared; the ratio of nitric acid and sulfuric acid should be adjusted according to the type of carbon black and the required hydrophilicity; the mixed use of nitric acid and sulfuric acid can more effectively introduce hydrophilic groups on the surface of carbon black; when preparing the mixed acid, a glass rod should be used for sufficient stirring to ensure that the two are evenly mixed; then, the mixed acid is slowly added to the carbon black suspension, Stir while adding to avoid local excessive concentration that may cause carbon black particles to aggregate or be damaged; transfer the dispersed carbon black suspension to a polytetrafluoroethylene reactor and seal the lid of the reactor; place the reactor in a heating device and set the temperature to 150°C for high-temperature reaction; high-temperature reaction can accelerate the chemical reaction between the acid and carbon black and further increase the hydrophilicity of carbon black; the reaction time is generally set to 3 hours to ensure that the reaction is fully carried out; during the reaction, the pressure and temperature of the reactor should be checked regularly to ensure that it operates within a safe range; after the reaction is completed, the reaction product should be filtered to remove excess acid and impurities; appropriate filter paper or filter membrane should be selected during filtration to avoid the loss of catalyst particles; the filtered catalyst should be placed in a vacuum drying oven and taken out after drying for 10-30 hours for grinding and collection.

[0011] The beneficial effects of the present invention are as follows: The present invention provides a method for preparing a water-soluble platinum-carbon catalyst, and the beneficial effects of the preparation method are mainly reflected in the following aspects: 1. Improve the hydrophilicity of the catalyst: Through acidification treatment and high-temperature reaction, the surface properties of carbon black are significantly improved, increasing its hydrophilicity, which enables the catalyst to be better dispersed and stabilized in the aqueous reaction system, thereby improving the catalytic efficiency.

[0012] 2. Optimize the catalyst preparation process: This method uses ultrasonic dispersion technology to ensure uniform mixing of carbon black and acid solution, avoiding agglomeration caused by local excessive concentration. At the same time, by precisely controlling the reaction time and temperature, the repeatability and stability of catalyst preparation are guaranteed.

[0013] 3. Improve the activity of catalyst: Hydrophilic carbon black, as a carrier, can more effectively load platinum nanoparticles to form a highly dispersed platinum-carbon catalyst. This high dispersion helps increase the active sites of the catalyst, thereby improving the rate and efficiency of the catalytic reaction.

[0014] 4. Simplify the post-processing process of the catalyst: Washing with a filter press can easily remove impurities and unreacted acid from the catalyst surface, while controlling the conductivity of the washing liquid to ensure the purity of the catalyst. In addition, the vacuum drying process further removes moisture and residual solvent from the catalyst, simplifying the post-processing steps.

[0015] 5. Enhance the durability of the catalyst: After high-temperature reaction and washing treatment, the catalyst has a more stable structure and can resist chemical erosion and physical wear during the reaction process, thereby extending the service life of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the accompanying drawings: Figure 1 This is the Tafel plot of the water-soluble platinum-carbon catalyst under different voltage and current conditions. DETAILED DESCRIPTION

[0017] In order to make people in this technical field better understand the technical solution in this application, Figure 1 The present invention is further described. The following examples are only used to more clearly illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention.

[0018] like Figure 1 A method for preparing a water-soluble platinum-carbon catalyst is shown, including a method for preparing a platinum-carbon catalyst. The method for preparing the platinum-carbon catalyst includes steps one, two, three, four, five, and six. Step one includes preparing the hydrophilic carbon black material, weighing a certain amount of ultrapure water and setting it aside, then weighing an appropriate amount of carbon black on weighing paper and pouring it into a beaker filled with water, and shaking to completely soak the catalyst.

[0019] The second step includes acidification treatment, which involves weighing appropriate amounts of nitric acid and sulfuric acid in a certain proportion, measuring them separately with a graduated cylinder, and mixing them evenly in another container. The mixed acid solution is slowly and evenly added dropwise to the carbon black suspension while gently stirring with a glass rod to form a mixed solution.

[0020] The step three includes ultrasonic dispersion, which involves placing the carbon black suspension to which the mixed acid is added into an ultrasonic disperser, setting appropriate ultrasonic power and dispersion time. The dispersion time should be adjusted according to the type, particle size, and desired hydrophilicity of the carbon black, and is generally recommended to be between 30 and 180 minutes. During the ultrasonic dispersion process, the state of the suspension should be checked regularly.

[0021] Step 4 involves a high-temperature reaction. The dispersed carbon black suspension is transferred to a polytetrafluoroethylene reactor and the reactor lid is sealed. The reactor is placed in a heating device set to 150°C for a high-temperature reaction. This high-temperature reaction accelerates the chemical reaction between the acid and the carbon black, further increasing its hydrophilicity. The reaction time is typically set at three hours to ensure sufficient reaction time. During the reaction, the reactor pressure and temperature should be regularly checked to ensure they are operating within safe ranges.

[0022] The step five includes washing the hydrophilic catalyst layer, pouring the cooled product after the reaction into a filter press, pouring 1-3 L of deionized water into the filter, and filtering until the conductivity is 20-40 μS / m.

[0023] The step six includes a drying process, wherein the filtered catalyst is placed in a vacuum drying oven for drying at a temperature of 60-100° C. After drying for 10-30 hours, the catalyst is taken out for grinding and collection.

[0024] When the present invention is working, first, a certain amount of ultrapure water needs to be prepared and placed in a clean container for standby use; then, an appropriate amount of carbon black is accurately weighed on weighing paper to avoid contact with impurities in the air; the weighed carbon black is slowly poured into a beaker filled with ultrapure water, and the carbon black particles are completely immersed in the water by gently shaking the beaker; the purpose of this step is to provide a uniform carbon black suspension for subsequent acid treatment to ensure the consistency of the acid treatment effect; a certain proportion of nitric acid and sulfuric acid mixture needs to be prepared; the ratio of nitric acid and sulfuric acid should be adjusted according to the type of carbon black and the required hydrophilicity; the mixed use of nitric acid and sulfuric acid can more effectively introduce hydrophilic groups on the surface of carbon black; when preparing the mixed acid, a glass rod should be used for sufficient stirring to ensure that the two are evenly mixed; then, the mixed acid is slowly added to the carbon black suspension Add the acid to the suspension while stirring to avoid local excessive concentration that may cause aggregation or damage of carbon black particles; transfer the dispersed carbon black suspension to a polytetrafluoroethylene reactor and seal the lid of the reactor; place the reactor in a heating device, set the temperature to 150°C, and perform a high-temperature reaction; high-temperature reaction can accelerate the chemical reaction between the acid and carbon black, and further increase the hydrophilicity of carbon black; the reaction time is generally set to 3 hours to ensure that the reaction is fully carried out; during the reaction, the pressure and temperature of the reactor should be checked regularly to ensure that it operates within a safe range; after the reaction is completed, the reaction product should be filtered to remove excess acid and impurities; appropriate filter paper or filter membrane should be selected during filtration to avoid loss of catalyst particles; the filtered catalyst should be placed in a vacuum drying oven, dried for 10-30 hours, and then taken out for grinding and collection. Example 1

[0025] Step 1: Prepare the hydrophilic carbon black material. Weigh 500 mL of ultrapure water and set aside. Weigh 20 g of carbon black on a weighing paper, pour it into a beaker filled with ultrapure water, and shake to completely soak the carbon black.

[0026] Step 2: Acidification Weigh 10 mL of concentrated nitric acid and 20 mL of concentrated sulfuric acid, measure them separately with a measuring cylinder, and mix them evenly in a glass beaker. Slowly and evenly add the mixed acid solution dropwise to the carbon black suspension, stirring gently with a glass rod while adding to form a mixed solution.

[0027] Step 3: Ultrasonic dispersion The carbon black suspension with mixed acid added was placed in an ultrasonic disperser, the ultrasonic power was set to 200 W, and the dispersion time was set to 90 minutes. During the ultrasonic dispersion process, the state of the suspension was checked regularly to ensure that there was no agglomeration.

[0028] Step 4: High temperature reaction Transfer the dispersed carbon black suspension into a polytetrafluoroethylene reactor and seal the reactor lid; place the reactor in a heating device, set the temperature to 150°C, and conduct a high-temperature reaction for 3 hours; during the reaction, regularly check the pressure and temperature of the reactor to ensure that it operates within a safe range.

[0029] Step 5: Washing of the hydrophilic catalyst layer The cooled product after the reaction was poured into a filter press, and 2 L of deionized water was poured into the filter press for filtration. The filtration was stopped when the conductivity reached 30 μS / m.

[0030] Step 6: Drying process The filtered catalyst was placed in a vacuum drying oven, the drying temperature was set to 80°C, and dried for 24 hours; after drying, the catalyst was taken out and ground and collected. Example 2

[0031] Step 1: Prepare the hydrophilic carbon black material. Weigh 500 mL of ultrapure water and set aside. Weigh 20 g of carbon black on a weighing paper, pour it into a beaker filled with ultrapure water, and shake to completely soak the carbon black.

[0032] Step 2: Acidification Weigh 10 mL of concentrated nitric acid and 20 mL of concentrated sulfuric acid, measure them separately with a measuring cylinder, and mix them evenly in a glass beaker. Slowly and evenly add the mixed acid solution dropwise to the carbon black suspension, stirring gently with a glass rod while adding to form a mixed solution.

[0033] Step 3: Ultrasonic dispersion The carbon black suspension with mixed acid added was placed in an ultrasonic disperser, the ultrasonic power was set to 200 W, and the dispersion time was set to 90 minutes. During the ultrasonic dispersion process, the state of the suspension was checked regularly to ensure that there was no agglomeration.

[0034] Step 4: High temperature reaction Transfer the dispersed carbon black suspension into a polytetrafluoroethylene reactor and seal the reactor lid; place the reactor in a heating device, set the temperature to 150°C, and conduct a high-temperature reaction for 3 hours; during the reaction, regularly check the pressure and temperature of the reactor to ensure that it operates within a safe range.

[0035] Step 5: Washing of the hydrophilic catalyst layer The cooled product after the reaction was poured into a filter press, and 1.5 L of deionized water was poured into the filter press for filtration. The filtration was stopped when the conductivity reached 25 μS / m.

[0036] Step 6: Drying process The filtered catalyst was placed in a vacuum drying oven, the drying temperature was set to 90°C, and dried for 18 hours; after drying, the catalyst was taken out and ground and collected. Example 3

[0037] Step 1: Prepare the hydrophilic carbon black material. Weigh 500 mL of ultrapure water and set aside. Weigh 20 g of carbon black on a weighing paper, pour it into a beaker filled with ultrapure water, and shake to completely soak the carbon black.

[0038] Step 2: Acidification Weigh 10 mL of concentrated nitric acid and 20 mL of concentrated sulfuric acid, measure them separately with a measuring cylinder, and mix them evenly in a glass beaker. Slowly and evenly add the mixed acid solution dropwise to the carbon black suspension, stirring gently with a glass rod while adding to form a mixed solution.

[0039] Step 3: Ultrasonic dispersion The carbon black suspension with mixed acid added was placed in an ultrasonic disperser, the ultrasonic power was set to 200 W, and the dispersion time was set to 90 minutes. During the ultrasonic dispersion process, the state of the suspension was checked regularly to ensure that there was no agglomeration.

[0040] Step 4: High temperature reaction Transfer the dispersed carbon black suspension into a polytetrafluoroethylene reactor and seal the reactor lid; place the reactor in a heating device, set the temperature to 150°C, and conduct a high-temperature reaction for 3 hours; during the reaction, regularly check the pressure and temperature of the reactor to ensure that it operates within a safe range.

[0041] Step 5: Washing of the hydrophilic catalyst layer The cooled product after the reaction was poured into a filter press, and 3 L of deionized water was poured into the filter to filter. The filtration was stopped when the conductivity reached 40 μS / m.

[0042] Step 6: Drying process The filtered catalyst was placed in a vacuum drying oven, the drying temperature was set to 70°C, and dried for 30 hours; after drying, the catalyst was taken out and ground and collected.

[0043] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solutions disclosed in the present invention, those skilled in the art can make some substitutions and modifications to some of the technical features therein according to the disclosed technical content without creative labor, and these substitutions and modifications are all within the protection scope of the present invention.

Claims

1. A method for preparing a water-soluble platinum-carbon catalyst, comprising a method for preparing a platinum-carbon catalyst, characterized in that: The method for preparing the platinum-carbon catalyst includes steps one, two, three, four, five and six. The step one includes preparing the hydrophilic carbon black material, weighing a certain amount of ultrapure water and setting it aside for later use, weighing an appropriate amount of carbon black on weighing paper and pouring it into a beaker filled with water, and shaking to completely soak the catalyst.

2. The method for preparing a water-soluble platinum-carbon catalyst according to claim 1, characterized in that: The step 2 includes an acidification treatment, wherein appropriate amounts of nitric acid and sulfuric acid are weighed in a certain ratio, respectively measured with a measuring cylinder, and mixed evenly in another container, and the mixed acid solution is slowly and evenly added dropwise to the carbon black suspension while gently stirring with a glass rod to form a mixed solution.

3. The method for preparing a water-soluble platinum-carbon catalyst according to claim 1, characterized in that: The step three includes ultrasonic dispersion, which is to put the carbon black suspension with the mixed acid into an ultrasonic disperser, set the appropriate ultrasonic power and dispersion time, and the dispersion time should be adjusted according to the type, particle size and required hydrophilicity of the carbon black. It is generally recommended to be between 30 minutes and 180 minutes. During the ultrasonic dispersion process, the state of the suspension should be checked regularly.

4. The method for preparing a water-soluble platinum-carbon catalyst according to claim 1, characterized in that: The step 4 includes a high temperature reaction, transferring the dispersed carbon black suspension to a polytetrafluoroethylene reactor and sealing the lid of the reactor. The reactor is placed in a heating device and the temperature is set to 150°C for a high temperature reaction. The high temperature reaction can accelerate the chemical reaction between the acid and the carbon black and further increase the hydrophilicity of the carbon black. The reaction time is generally set to 3 hours to ensure that the reaction is fully carried out. During the reaction process, the pressure and temperature of the reactor should be checked regularly to ensure that it operates within a safe range.

5. The method for preparing a water-soluble platinum-carbon catalyst according to claim 1, characterized in that: The step five includes washing the hydrophilic catalyst layer, pouring the cooled product after the reaction into a filter press, pouring 1-3L of deionized water into the filter, and filtering until the conductivity is 20-40us / m.

6. The method for preparing a water-soluble platinum-carbon catalyst according to claim 1, characterized in that: The step six includes a drying process, wherein the filtered catalyst is placed in a vacuum drying oven for drying at a temperature of 60-100° C. After drying for 10-30 hours, the catalyst is taken out for grinding and collection.

Citation Information

Patent Citations

  • Hydrogen fuel cell alloy catalyst and preparation method thereof

    CN116387537A

  • Hydrophilic modification method of platinum-based catalyst for fuel cell

    CN116632259A

  • Carbon carrier applied to fuel cell catalyst and preparation method of carbon carrier

    CN118005001A

Cited By

  • Production method of battery foil and battery foil

    CN120905664A