Cathode catalyst layer and membrane electrode of proton exchange membrane fuel cell

By combining a platinum-based catalyst with sulfur-doped carbon support in a proton exchange membrane fuel cell, a catalytic layer with high activity and low oxygen transport resistance is formed, and the problems of low cathodic oxygen reduction reaction activity and large oxygen transport resistance are solved. High-efficiency performance and high power density of low-platinum load membrane electrodes are achieved.

CN118943397APending Publication Date: 2024-11-12NORTH CHINA ELECTRIC POWER UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411031214.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In existing proton exchange membrane fuel cells, the cathode oxygen reduction reaction activity and high oxygen transmission resistance lead to high voltage loss and reduced performance, making it difficult to achieve high-efficiency fuel cell performance with low platinum load.

Method used

The platinum-based catalyst is used to combine with sulfur-doped carbon support, and a catalytic layer with high activity and low oxygen transport resistance is formed through sulfur element doping and heat treatment. The electrostatic interaction between thiophene sulfur and ionomers modified on the carbon support is uniformly distributed. Ionomers, reducing oxygen-related mass transport resistance.

Benefits of technology

The performance of low-platinum load membrane electrodes is significantly improved, and high power density below 0.45V is achieved, and the non-pressure oxygen mass transfer resistance is greatly reduced, which improves the overall performance of the fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943397A_ABST
    Figure CN118943397A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fuel cells, in particular to a cathode catalyst layer and a membrane electrode of a proton exchange membrane fuel cell. The cathode catalyst layer of the proton exchange membrane fuel cell provided by the invention comprises a platinum-based catalyst and an ionomer, sulfur-related functional groups, mainly thiophenic sulfur (C-S-C), are modified on a carbon carrier, and then the platinum-based catalyst is prepared based on the modified carrier. The catalyst layer with high activity and low oxygen transfer resistance is created, the distribution uniformity of ionomers in the catalyst layer is ensured by utilizing the electrostatic interaction between thiophene sulfur modified on the carbon carrier and the ionomers, the mass transfer resistance related to local oxygen is greatly reduced, and the inhibition effect of the mass transfer resistance on the performance of a low-platinum membrane electrode is reduced to the minimum; the performance of the low-platinum-load membrane electrode is greatly improved, so that the power density of the fuel cell under the conditions of low platinum load and high current density reaches an unprecedented level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fuel cells, and in particular to a cathode catalyst layer and a membrane electrode of a proton exchange membrane fuel cell. Background Art

[0002] Fuel cells, as an environmentally friendly, efficient and clean energy source, have received widespread attention in recent years. In the process of energy conversion, the slow cathode oxygen reduction reaction requires a large amount of platinum-based catalyst to accelerate the reaction. In order to achieve large-scale commercialization of proton exchange membrane fuel cells, reducing the platinum content in its cathode is an urgent need to reduce costs. However, the researchers' research shows that reducing the total Pt loading in the cathode (<0.1mg Pt cm -2 ), which results in surprisingly high voltage losses, leading to a significant reduction in battery performance. Studies have shown that these voltage losses are mainly caused by the reduction in oxygen reduction reaction (ORR) activity in the cathode catalyst layer in contact with the ionomer and the O 2 The influence of mass transfer resistance through the three-phase interface to the platinum or platinum alloy catalyst interface. Developing a cathode catalyst layer with high activity and low oxygen transport resistance is still a key technical issue that needs to be solved urgently. Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a cathode catalyst layer and membrane electrode of a proton exchange membrane fuel cell. The cathode catalyst layer of a proton exchange membrane fuel cell provided by the present invention can greatly reduce the non-pressure oxygen mass transfer of the membrane electrode, greatly reduce the inhibitory effect of this core factor of the low platinum loading membrane electrode, and improve the performance of the low platinum loading membrane electrode.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a cathode catalyst layer of a proton exchange membrane fuel cell, comprising a platinum-based catalyst and an ionomer. The preparation method of the platinum-based catalyst comprises the following steps:

[0006] Mixing a sulfur-containing precursor, a carbon support and a solvent and evaporating them under reduced pressure to obtain a first precursor mixture;

[0007] Subjecting the first precursor mixture to a first heat treatment in an inert atmosphere to obtain a sulfur-doped carbon support;

[0008] Mixing a cobalt salt, a platinum salt, a solvent and the sulfur-doped carbon support and evaporating the mixture under reduced pressure to obtain a second precursor mixture;

[0009] The second precursor mixture is subjected to a second heat treatment in a reducing atmosphere, and then the obtained material is subjected to an annealing treatment to obtain the platinum-based catalyst.

[0010] Preferably, the sulfur-containing precursor includes one or more of sulfonated phthalocyanine salts, thiophene, dithiophene, propanethiol, pentamethylenethiol, cyclohexanethiol, thiourea and aminosulfonate; the carbon carrier includes carbon black; and the mass ratio of the sulfur-containing precursor to the carbon carrier is 10:1 to 1:10.

[0011] Preferably, the temperature of the first heat treatment is 900-1000° C., and the time is 1.5-6 hours.

[0012] Preferably, the molar ratio of the Co element in the cobalt salt to the Pt element in the platinum salt is 1:1 to 1:3, and the mass of the Pt element in the platinum salt is 5 to 60% of the mass of the sulfur-doped carbon support.

[0013] Preferably, the mixture of the cobalt salt, the platinum salt, the solvent and the sulfur-doped carbon carrier further comprises the addition of small molecule sulfur, wherein the small molecule sulfur comprises one or more of elemental sulfur, propyl mercaptan, 1,3-propanediol, 11-mercaptohexadecanoic acid, 2-mercaptobenzimidazole, 1-mercaptopropane and sodium thioglycolate; and the molar ratio of the small molecule sulfur to the Pt element in the platinum salt is 3:1 to 1:1.

[0014] Preferably, the reducing atmosphere is a mixed atmosphere of hydrogen and argon, and the temperature of the second heat treatment is 750-950° C., and the time is 1.5-3 hours.

[0015] Preferably, the annealing treatment is performed at a temperature of 400 to 600° C. and for a time of 2 to 5 hours.

[0016] Preferably, the ionomer comprises one or more of perfluorosulfonic acid resin, sulfonated polyarylethersulfone, sulfonated polyarylether(sulfide), sulfonated polyetheretherketone, sulfonated polyimide and polybenzimidazole; and the mass ratio of the ionomer to the sulfur-doped carbon carrier in the platinum-based catalyst is 0.2 to 1:1.

[0017] The present invention provides a proton exchange membrane fuel cell membrane electrode, comprising a proton exchange membrane, a cathode catalyst layer composited on one side surface of the proton exchange membrane, and an anode catalyst layer composited on the other side surface of the proton exchange membrane, wherein the cathode catalyst layer is the cathode catalyst layer of the proton exchange membrane fuel cell described in the above technical solution, and the anode catalyst layer is a Pt / C catalyst layer.

[0018] Preferably, the Pt loading in the cathode catalyst layer is 0.1-0.5 mg / cm 2 The Pt loading in the anode catalyst layer is 0.01 to 0.05 mg / cm 2 .

[0019] The present invention provides a cathode catalyst layer of a proton exchange membrane fuel cell, comprising a platinum-based catalyst and an ionomer. The preparation method of the platinum-based catalyst comprises the following steps: mixing a sulfur-containing precursor, a carbon carrier and a solvent and evaporating under reduced pressure to obtain a first precursor mixture; subjecting the first precursor mixture to a first heat treatment in an inert atmosphere to obtain a sulfur-doped carbon carrier; mixing a cobalt salt, a platinum salt, a solvent and the sulfur-doped carbon carrier and evaporating under reduced pressure to obtain a second precursor mixture; subjecting the second precursor mixture to a second heat treatment in a reducing atmosphere, and then annealing the obtained material to obtain the platinum-based catalyst. The present invention dopes sulfur onto the carbon carrier through the first heat treatment, and a part of it is oxidized to generate SO x The functional groups are modified on the surface of the carbon carrier, and a part of them directly reacts with the carbon on the surface of the carbon carrier to form a CSC (thiophene sulfur) structure; the present invention reduces the platinum salt and the cobalt salt into a platinum-cobalt alloy through a second heat treatment, and loads it onto the sulfur-doped carbon carrier. The present invention creates a catalytic layer with high activity and low oxygen transport resistance, and utilizes the electrostatic interaction between the thiophene sulfur (CSC) modified on the carbon carrier and the ionomer to ensure the uniformity of the distribution of the ionomer in the catalytic layer, greatly reducing the mass transfer resistance related to local oxygen, and minimizing its inhibitory effect on the performance of the low-platinum membrane electrode, thereby achieving a significant improvement in the performance of the low-platinum-loaded membrane electrode, so that the power density of the fuel cell at low platinum load and low voltage (below 0.45V) reaches an unprecedented level, providing a direction for the future development of low-platinum-loaded fuel cells.

[0020] The results of the embodiment show that the ultra-low film electrode (cathode loading 0.1 mg / cm 2 , anode loading 0.025mg / cm 2 , 80℃, 1.5bar, constant dosage ratio 1.5~2.0, IC ratio 0.5) has excellent performance, and the peak power reaches 1.81W / cm 2 The non-pressure oxygen mass transfer resistance of the membrane electrode is as low as 0.056s / cm, while the peak power of commercial catalyst membrane electrode with the same loading is 0.8-0.9W / cm 2 The non-pressure oxygen mass transfer resistance of the membrane electrode is 0.4 to 0.6 s / cm. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the preparation process of the platinum-based catalyst in the cathode catalyst layer of the proton exchange membrane fuel cell in the embodiment;

[0022] Figure 2 The S2p orbital XPS diagram of the S-modified carrier in Example 1 and the S functional groups on the carrier and their proportions are shown in FIG. Figure 2The middle left picture is the S2p orbital XPS picture, and the right picture is the S functional group on the carrier and its proportion;

[0023] Figure 3 The ultra-low-load full cell (cathode loading 0.1 mg / cm2) prepared by the catalyst after carrier modification in Example 1 2 , anode loading 0.025mg / cm 2 , 80℃, 1.5bar, constant dosage ratio 1.5~2.0, IC ratio 0.5) oxygen mass transfer impedance-pressure diagram and performance diagram, Figure 3 The middle left figure is the oxygen mass transfer impedance-pressure diagram, and the right figure is the performance diagram;

[0024] Figure 4 The distribution of ionomers in the membrane electrode made of the catalyst supported by the carrier after modification in Example 1. Figure 4 (a) is the catalyst morphology of the region, (b) is the F signal distribution of the region, (c) is the Pt signal distribution of the region, and (d) is the superposition distribution of the morphology, F signal and Pt signal of the region;

[0025] Figure 5 TEM-Mapping image of the catalyst layer after focused ion beam (FIB) sample preparation in Example 1;

[0026] Figure 6 The S2p orbital XPS diagram of the S-modified carrier in Example 2 and the S functional groups on the carrier and their proportions are shown in FIG. Figure 6 The middle left picture is the S2p orbital XPS picture, and the right picture is the S functional group on the carrier and its proportion;

[0027] Figure 7 The ultra-low-load full cell (cathode loading 0.1 mg / cm2) prepared by the catalyst after carrier modification in Example 2 2 , anode loading 0.025mg / cm 2 , 80℃, 1.5bar, constant dosage ratio 1.5~2.0, IC ratio 0.5) oxygen mass transfer impedance-pressure diagram and performance diagram, Figure 7 The middle left figure is the oxygen mass transfer impedance-pressure diagram, and the right figure is the performance diagram;

[0028] Figure 8 The S2p orbital XPS diagram of the S-modified carrier in Example 3 and the S functional groups on the carrier and their proportions are shown in FIG. Figure 8 The middle left picture is the S2p orbital XPS picture, and the right picture is the S functional group on the carrier and its proportion;

[0029] Fig. 9 The ultra-low-load full cell (cathode loading 0.1 mg / cm2) prepared by the catalyst after carrier modification in Example 3 2 , anode loading 0.025mg / cm 2, 80℃, 1.5bar, constant dosage ratio 1.5~2.0, IC ratio 0.5) oxygen mass transfer impedance-pressure diagram and performance diagram, Fig. 9 The middle left figure is the oxygen mass transfer impedance-pressure diagram, and the right figure is the performance diagram;

[0030] Fig.10 The ultra-low-load full cell (cathode loading 0.1 mg / cm2) prepared by the catalyst without modifying the carrier is shown in the comparative example. 2 , anode loading 0.025mg / cm 2 , 80℃, 1.5bar, constant dosage ratio 1.5~2.0, IC ratio 0.5) performance diagram and oxygen mass transfer impedance-pressure diagram, Fig.10 The middle left figure is a performance diagram, and the right figure is an oxygen mass transfer impedance-pressure diagram;

[0031] Fig.11 TEM-Mapping of membrane electrode area 1 prepared for catalyst without carrier modification. Fig.11 (a) is the catalyst morphology of the region, (b) is the F signal distribution of the region, (c) is the Pt signal distribution of the region, and (d) is the superposition distribution of the morphology, F signal and Pt signal of the region;

[0032] Fig.12 TEM-Mapping of membrane electrode area 2 prepared for catalyst without carrier modification. Fig.12 (a) is the catalyst morphology of the region, (b) is the F signal distribution of the region, (c) is the Pt signal distribution of the region, and (d) is the superposition distribution of the morphology, F signal and Pt signal of the region;

[0033] Fig.13 3TEM-Mapping of the membrane electrode area prepared for the catalyst without carrier modification. Fig.13 (a) is the catalyst morphology of the area, (b) is the F signal distribution of the area, (c) is the Pt signal distribution of the area, and (d) is the superimposed distribution of the morphology, F signal and Pt signal of the area. DETAILED DESCRIPTION

[0034] The present invention provides a cathode catalyst layer of a proton exchange membrane fuel cell, comprising a platinum-based catalyst and an ionomer. The preparation method of the platinum-based catalyst comprises the following steps:

[0035] Mixing a sulfur-containing precursor, a carbon support and a solvent and evaporating them under reduced pressure to obtain a first precursor mixture;

[0036] Subjecting the first precursor mixture to a first heat treatment in an inert atmosphere to obtain a sulfur-doped carbon support;

[0037] Mixing a cobalt salt, a platinum salt, a solvent and the sulfur-doped carbon support and evaporating the mixture under reduced pressure to obtain a second precursor mixture;

[0038] The second precursor mixture is subjected to a second heat treatment in a reducing atmosphere, and then the obtained material is subjected to an annealing treatment to obtain the platinum-based catalyst.

[0039] The cathode catalyst layer of the proton exchange membrane fuel cell provided by the present invention comprises a platinum-based catalyst. The preparation of the platinum-based catalyst is described in detail below.

[0040] The present invention mixes a sulfur-containing precursor, a carbon carrier and a solvent and evaporates them under reduced pressure to obtain a first precursor mixture.

[0041] In the present invention, the sulfur-containing precursor preferably includes one or more of sulfonated phthalocyanine salts, thiophene, dithiophene, propanethiol, pentamethylenethiol, cyclohexanethiol, thiourea and aminosulfonate, more preferably sulfonated phthalocyanine salts, and the sulfonated phthalocyanine salts are preferably sulfonated cobalt phthalocyanine. In the present invention, the carbon carrier preferably includes carbon black, and the carbon black is preferably one or more of Ketjen carbon (Ketjen), Vulcan, graphitized carbon black and acetylene black, more preferably Ketjen carbon EC300. In the present invention, the mass ratio of the sulfur-containing precursor and the carbon carrier is preferably 10:1 to 1:10, more preferably 1:1 to 1:3, and further preferably 1:2. In the present invention, the solvent is preferably a mixed solvent of an organic solvent and water, the organic solvent is preferably ethanol, and the volume ratio of the organic solvent to water is preferably 2:1 to 1:2; more preferably 1:1. The present invention has no special requirements for the amount of the solvent, as long as the sulfur-containing precursor and the carbon carrier are fully dissolved or dispersed.

[0042] In the present invention, the method for mixing the sulfur-containing precursor, the carbon carrier and the solvent is preferably: adding the sulfur-containing precursor and the carbon carrier to the solvent and ultrasonically dispersing them. The present invention has no special requirements for the conditions of the ultrasonic dispersion, as long as the mixing is uniform.

[0043] In the present invention, the reduced pressure evaporation is preferably carried out in a rotary evaporator, and the reduced pressure evaporation is based on evaporation to dryness, that is, a solid first precursor mixture is obtained. The present invention fully mixes the sulfur-containing precursor with the carbon carrier through the mixing and reduced pressure evaporation.

[0044] After obtaining the first precursor mixture, the present invention performs a first heat treatment on the first precursor mixture in an inert atmosphere to obtain a sulfur-doped carbon carrier.

[0045] In the present invention, the inert atmosphere is preferably nitrogen, argon, helium or neon, more preferably nitrogen or argon. In the present invention, the temperature of the first heat treatment is preferably 900-1000°C, more preferably 900-950°C, the time is preferably 1.5-6h, more preferably 2-3h, and the heating rate from room temperature to the temperature of the first heat treatment is preferably 5°C / min; the first heat treatment is preferably carried out in a tube furnace. During the first heat treatment, the S element in the sulfur-containing precursor is doped onto the carbon carrier, and a part of it is oxidized to generate SO x The functional groups are modified on the surface of the carbon support (although it is an inert gas atmosphere, the presence of a small amount of air cannot be avoided during the process), and a part of them directly reacts with the C on the surface of the carbon support to form a CSC (thiophene sulfur) structure.

[0046] After the first heat treatment is completed, the temperature is naturally lowered to obtain a sulfur-doped carbon carrier. After the natural cooling, the present invention also preferably performs pickling on the obtained material, the pickling solution used for pickling is preferably 0.5 mol / L sulfuric acid, the pickling temperature is preferably 80°C, and the time is preferably 8 to 9 hours.

[0047] After obtaining the sulfur-doped carbon carrier, the present invention mixes the cobalt salt, the platinum salt, the solvent and the sulfur-doped carbon carrier and evaporates them under reduced pressure to obtain a second precursor mixture.

[0048] In the present invention, the cobalt salt is preferably cobalt acetate, and the platinum salt is preferably chloroplatinic acid. In the present invention, the solvent is preferably an organic solvent, and the organic solvent is preferably ethanol and / or ethylene glycol. In the present invention, the molar ratio of the Co element in the cobalt salt to the Pt element in the platinum salt is preferably 1:1 to 1:3, more preferably 1:1 to 1:2; the mass of the Pt element in the platinum salt is preferably 5 to 60% of the mass of the sulfur-doped carbon carrier, more preferably 20 to 45%. The present invention has no special requirements for the amount of the solvent, as long as the cobalt salt and the platinum salt can be fully dispersed.

[0049] In the present invention, the method for mixing the cobalt salt, platinum salt, solvent and sulfur-doped carbon carrier is preferably: mixing the platinum salt with an organic solvent to obtain a platinum salt organic solution; mixing the platinum salt organic solution and the cobalt salt, ultrasonically dispersing them, stirring the obtained mixed solution to be uniform, and then adding the sulfur-doped carbon carrier.

[0050] In the present invention, small molecule sulfur is preferably added to the mixed solution, and the small molecule sulfur preferably includes one or more of elemental sulfur, propyl mercaptan, 1,3-propanedithiol, 11-mercaptohexadecanoic acid, 2-mercaptobenzimidazole, 1-mercaptopropane and sodium thioglycolate, and more preferably propyl mercaptan; the molar ratio of the small molecule sulfur to the Pt element in the platinum salt is preferably 3:1 to 1:1, and more preferably 2:1 to 1:1. In the present invention, the role of the small molecule sulfur is to control the particle size of the catalyst platinum-cobalt alloy particles finally synthesized.

[0051] In the present invention, the reduced pressure evaporation is preferably carried out in a rotary evaporator, and the reduced pressure evaporation is based on evaporation to dryness.

[0052] After obtaining the second precursor mixture, the present invention performs a second heat treatment on the second precursor mixture in a reducing atmosphere, and then performs an annealing treatment on the obtained material to obtain the platinum-based catalyst.

[0053] In the present invention, the reducing atmosphere is a mixed atmosphere of hydrogen and argon, and the volume of the hydrogen is preferably 5% of the volume of the argon. In the present invention, the temperature of the second heat treatment is preferably 750-950°C, more preferably 800-900°C, the time is preferably 1.5-3h, more preferably 2h, and the second heat treatment is preferably performed in a tube furnace. During the second heat treatment, platinum salt and cobalt salt are reduced to form platinum-cobalt alloy, which is loaded onto the carbon carrier, and small molecular sulfur interacts with the alloy to limit the agglomeration and growth of alloy particles.

[0054] In the present invention, the temperature of the annealing treatment is preferably 400-600°C, more preferably 500-600°C, and the time is preferably 2-5h, more preferably 3-4h. In the present invention, the annealing treatment is preferably carried out in a reducing atmosphere, and the reducing atmosphere is preferably the same as the reducing atmosphere of the second heat treatment, which will not be repeated here. The present invention uses the annealing treatment to produce an ordered phase in the alloy, that is, to transform the disordered alloy structure into an ordered structure, thereby improving the order of the catalyst.

[0055] After the annealing treatment is completed, the present invention preferably performs pickling on the obtained catalyst material. In the present invention, the pickling solution used for pickling is preferably a 0.5-3 mol / L sulfuric acid aqueous solution, the pickling temperature is preferably 80°C, and the time is preferably 8 hours. Through the pickling, the present invention corrodes the excess metal element on the catalyst surface into metal ions, which are dissolved in water together with other impurity ions and washed away.

[0056] The cathode catalyst layer of the proton exchange membrane fuel cell provided by the present invention comprises an ionomer.

[0057] In the present invention, the ionomer preferably includes one or more of perfluorosulfonic acid resin (PFSA), sulfonated polyarylethersulfone (SPSF), sulfonated polyarylether (sulfide) ether (SPAE), sulfonated polyetheretherketone (SPEEK), sulfonated polyimide (SPI) and polybenzimidazole (PBI), and more preferably perfluorosulfonic acid resin, such as one or more of nafion, 3M resin and Aquivion; the mass ratio of the ionomer to the sulfur-doped carbon carrier in the platinum-based catalyst (i.e., IC ratio) is preferably 0.2 to 1:1, and more preferably 0.3 to 0.5:1.

[0058] The exploration of regulating the distribution of ionomers in the catalyst layer of the membrane electrode has been ongoing. This invention first proposed and successfully modified sulfur-related functional groups on carbon carriers, mainly thiophene sulfur (CSC) modification, and then prepared a platinum-based catalyst based on the modified carrier. Through the Coulomb interaction between thiophene sulfur and ionomers on the carrier, the ionomers in the catalyst layer are uniformly distributed on the catalyst surface, creating an optimal three-phase interface of the catalyst layer, which can greatly reduce the non-pressure oxygen mass transfer of the membrane electrode, greatly reduce the inhibitory effect of this core factor of low platinum loading membrane electrode, and improve the overall performance of the membrane electrode. The present invention creates a catalyst layer with high activity and low oxygen transmission resistance through a new platinum alloy catalyst / carrier design.

[0059] The present invention provides a proton exchange membrane fuel cell membrane electrode, comprising a proton exchange membrane, a cathode catalyst layer composited on one side surface of the proton exchange membrane, and an anode catalyst layer composited on the other side surface of the proton exchange membrane, wherein the cathode catalyst layer is the cathode catalyst layer of the proton exchange membrane fuel cell described in the above technical solution, and the cathode catalyst layer is a Pt / C catalyst layer.

[0060] The present invention has no special requirements for the proton exchange membrane, and a proton exchange membrane well known to those skilled in the art can be used, such as a perfluorosulfonic acid proton exchange membrane. The present invention has no special requirements for the Pt / C catalyst in the Pt / C catalyst layer, and a commercially available Pt / C catalyst well known to those skilled in the art can be used. In the present invention, the Pt loading in the cathode catalyst layer is preferably 0.1 to 0.5 mg / cm -2 The Pt loading in the anode catalyst layer is 0.01 to 0.05 mg / cm -2 The power density of the proton exchange membrane fuel cell membrane electrode provided by the present invention reaches an unprecedented level under low platinum loading and high current density, providing a direction for the future development of low platinum loading fuel cells.

[0061] In the present invention, the method for preparing the proton exchange membrane fuel cell membrane electrode preferably comprises the following steps:

[0062] mixing the platinum-based catalyst, ionomer, organic solvent and water to obtain a slurry;

[0063] The slurry is sprayed onto one side of the proton exchange membrane, and the slurry prepared by the Pt / C catalyst is sprayed onto the other side of the proton exchange membrane;

[0064] The sprayed proton exchange membrane is hot pressed to obtain the proton exchange membrane fuel cell membrane electrode.

[0065] In the present invention, the organic solvent is preferably isopropyl alcohol (IPA); the mass ratio of the organic solvent to water is preferably 1:0.07-0.2; the present invention has no special requirements on the amount of the organic solvent and water, as long as the platinum-based catalyst and the ionomer can be fully dispersed or dissolved. In the present invention, the spraying method is preferably ultrasonic spraying. In the present invention, the temperature of the hot pressing is preferably 120-140°C.

[0066] In order to further illustrate the present invention, the cathode catalyst layer and membrane electrode of the proton exchange membrane fuel cell provided by the present invention are described in detail below in conjunction with examples, but they should not be construed as limiting the protection scope of the present invention.

[0067] Example 1

[0068] Preparation of platinum-based catalysts in the cathode catalyst layer of proton exchange membrane fuel cells, the process is as follows Figure 1 As shown, the specific steps are as follows:

[0069] (1) Modification of carbon carrier: First, the sulfur-containing precursor (sulfonated cobalt phthalocyanine) and the carbon carrier (EC300) were added to a mixed solvent of ethanol and water (ethanol and water volume ratio 1:1) in a certain ratio (S-containing precursor: carbon carrier (mass ratio) = 1:2), and then transferred to a rotary evaporator for uniform ultrasonic dispersion. The precursor mixture (solid) was evaporated under reduced pressure and then sent to a tubular furnace and heated to 900°C at 5°C / min. The temperature was maintained (nitrogen atmosphere) for heat treatment for 2 h and then naturally cooled. Then, the sulfur-doped carbon carrier was pickled in 0.5 mol / L sulfuric acid at 80°C for 8 h to obtain the sulfur-doped carbon carrier.

[0070] (2) Loading Pt and Co onto a carbon support and forming an alloy: 58 mg of cobalt acetate tetrahydrate and chloroplatinic acid ethanol solution (prepared from 120.7 mg of chloroplatinic acid hexahydrate and 80 mL of ethanol) were mixed, and after ultrasonic dispersion, 22 μL of small molecule sulfur (propyl mercaptan) was added. After stirring evenly, 100 mg of the sulfur-doped carbon support obtained in (1) was added, and the mixture was evaporated under reduced pressure by a rotary evaporator to obtain a precursor mixture, which was then heated in a tube furnace for 1 0.5 hours. 2 and Ar(H 2Under the condition of a mixed atmosphere of Ar (5% by volume), the catalyst was heat treated at 900°C for 2h to reduce and form a platinum-cobalt alloy, then the temperature was reduced to 600°C for another 4h, and finally, it was pickled in 1mol / L sulfuric acid at 80°C for 8h to obtain a platinum-based catalyst.

[0071] The preparation steps of proton exchange membrane fuel cell membrane electrode are as follows:

[0072] The above-mentioned 100 mg platinum-based catalyst was mixed with 800 mg ionomer (nafion) solution (ionomer mass fraction 5%, water and other volatile organic solvents accounted for 95%), 15287.7 mg organic solvent (IPA) and 1452.3 mg water to prepare a slurry, which was sprayed onto a proton exchange membrane by ultrasonic spraying, the above-mentioned catalyst was sprayed on the cathode, and the commercial Pt / C catalyst was sprayed on the anode, and then hot-pressed to form a membrane electrode.

[0073] Figure 2 The XPS graph of the S2p orbital after the carrier modification in Example 1 and the graph of the S functional groups and their proportions on the carrier are shown in Figure 2. Figure 2 The middle left picture is the S2p orbital XPS graph (light gray curve: actual test data; red curve: fitting data; green curve: two peaks correspond to the position of S-Ox, indicating the presence of S-Ox on the catalyst surface; blue curve: two peaks correspond to the position of CSC, indicating the presence of CSC on the catalyst surface), and the right picture is the S functional group on the carrier and its proportion.

[0074] Figure 2 The S2p orbital XPS image of the modified carbon support in the middle left shows that the C support is successfully doped with S element, and the main form is oxidized S (SO X ) and thiophene S (CSC) are modified on the surface of the carbon support. Figure 2 The middle right figure shows that the proportion of thiophene S (CSC) (relative element content ratio) is as high as 69.81%, which is the most important functional group on the S-modified carbon carrier.

[0075] Figure 3 Ultra-low-load full cell prepared by catalyst after carrier modification (cathode Pt loading 0.1 mg / cm 2 , anode Pt loading 0.025mg / cm 2 , 80℃, 1.5bar, constant stoichiometry 1.5-2.0, IC ratio 0.5, where the constant stoichiometry is the ratio of the actual flow rate of the reactants at the cell inlet to the consumption of the reactants) oxygen mass transfer impedance-pressure diagram and performance diagram are compared with the performance of commercial Pt / C catalysts. Figure 3 It can be seen that the ultra-low film electrode prepared by carbon carrier modified with thiophene S (CSC) has a significant improvement in performance compared with commercial Pt / C catalyst, with a peak power of 1.81 W / cm2 , excellent performance ( Figure 3 In comparison, the peak power of commercial catalyst membrane electrode with the same loading is 0.8-0.9W / cm 2 . Figure 3 The middle left figure shows the oxygen mass transfer impedance-pressure diagram of the membrane electrode, from which the main influencing factor of the low platinum loading membrane electrode - non-pressure oxygen mass transfer resistance is obtained. The results show that the non-pressure oxygen mass transfer of the membrane electrode prepared after thiophene S modification is as low as 0.056s / cm. In contrast, the membrane electrode prepared by commercial catalysts (both cathode catalyst and anode catalyst are Pt / C) generally has a value of 0.4-0.6s / cm.

[0076] The non-pressure oxygen mass transfer resistance is the gas phase Knudsen diffusion in the catalyst layer and microporous layer in the membrane electrode and the O in the ionomer covered on the catalyst / support. 2 The cumulative effect of transfer / transmission. For ultra-low film loading electrodes, it mainly reflects the distribution of ionomers on the catalyst / support. Figure 4 The distribution of ionomers in the membrane electrode made of the catalyst supported by the carrier is shown in Figure 2. Figure 4 (a) is the catalyst morphology of the area, (b) is the F signal distribution of the area, (c) is the Pt signal distribution of the area, and (d) is the superimposed distribution of the morphology, F signal and Pt signal of the area. Figure 4 The ionomer (nafion) represented by the F element and the catalyst particles represented by the Pt element are evenly distributed and have a high overlap rate, indicating that the ionomer is evenly distributed in the catalytic layer. Figure 5 TEM-Mapping of the cathode side of the membrane electrode catalyst layer by FIB (focused ion beam) cutting and sample preparation also shows that the ionomers are evenly distributed near the catalyst particles on the carbon support.

[0077] Example 2

[0078] The feed ratio of the S-containing precursor (sulfonated cobalt phthalocyanine) and the carbon carrier (EC300) was changed to S-containing precursor: carbon carrier = 1:1, and the rest was the same as Example 1.

[0079] Figure 6 The S2p orbital XPS diagram of the S-modified carrier in Example 2 and the S functional groups on the carrier and their proportions are shown in FIG. Figure 6 The middle left picture is the S2p orbital XPS graph (light gray curve: actual test data; red curve: fitting data; green curve: two peaks correspond to the position of S-Ox, indicating the presence of S-Ox on the catalyst surface; blue curve: two peaks correspond to the position of CSC, indicating the presence of CSC on the catalyst surface), and the right picture is the S functional group on the carrier and its proportion. Figure 6 It shows that at a feed ratio of 1:1, the C carrier is successfully doped with S, and the main form is oxidized S (SOX ) and thiophene S (CSC) are modified on the surface of the carbon carrier; among them, thiophene S (CSC) accounts for as high as 76.24%, which is the most important functional group on the S-modified carbon carrier, and the thiophene S content of the modified carrier is further increased compared with the feed ratio of 1:2 in Example 1.

[0080] Figure 7 The ultra-low-load full cell (cathode loading 0.1 mg / cm2) prepared by the catalyst after carrier modification in Example 2 2 , anode loading 0.025mg / cm 2 , 80℃, 1.5bar, constant dosage ratio 1.5~2.0, IC ratio 0.5) oxygen mass transfer impedance-pressure diagram and performance diagram, Figure 7 The left figure in the middle is the oxygen mass transfer impedance-pressure diagram, and the right figure is the performance diagram. As can be seen from Figure 7, the ultra-low film electrode prepared by the carbon carrier modified with thiophene S (CSC) under the feed ratio of Example 2 still has obvious performance improvement over the commercial Pt / C catalyst, with a peak power of 1.24W / cm 2 The non-pressure oxygen mass transfer resistance of the membrane electrode is as low as 0.076s / cm. Although it has increased compared with the membrane electrode prepared by modifying the carrier with the optimal feed ratio of 1:2, it is still much lower than the membrane electrode prepared with commercial catalysts.

[0081] Example 3

[0082] The feed ratio of the S-containing precursor (sulfonated cobalt phthalocyanine) and the carbon carrier (EC300) was changed to S-containing precursor: carbon carrier = 1:3, and the rest was the same as in Example 1.

[0083] Figure 8 The S2p orbital XPS diagram of the S-modified carrier in Example 3 and the S functional groups on the carrier and their proportions are shown in FIG. Figure 8 The left picture in the middle is the S2p orbital XPS graph (light gray curve: test data; red curve: fitting data; green curve: two peaks correspond to the location of S-Ox, indicating the presence of S-Ox on the catalyst surface; blue curve: two peaks correspond to the location of CSC, indicating the presence of CSC on the catalyst surface), and the right picture is the S functional group on the carrier and its proportion. Figure 8 It can be seen that the modified carbon support was successfully doped with S element at a feed ratio of 1:3, and the S element was mainly in the oxidized state S (SO X ) and thiophene S (CSC) are modified on the surface of the carbon support; among them, thiophene S (CSC) accounts for 65.40% and is the most important functional group on the carbon support after S modification.

[0084] Fig. 9 The ultra-low-load full cell (cathode loading 0.1 mg / cm2) prepared by the catalyst after carrier modification in Example 3 2, anode loading 0.025mg / cm 2 , 80℃, 1.5bar, constant dosage ratio 1.5~2.0, IC ratio 0.5) oxygen mass transfer impedance-pressure diagram and performance diagram, Fig. 9 The left figure in the middle is the oxygen mass transfer impedance-pressure diagram, and the right figure is the performance diagram. Fig. 9 It can be seen that the performance of the ultra-low-loaded film electrode prepared by the carbon carrier modified with thiophene S (CSC) is still significantly improved compared with the commercial Pt / C catalyst at this feed ratio, with a peak power of 1.43 W / cm 2 The non-pressure oxygen mass transfer resistance of the membrane electrode is as low as 0.083s / cm. Although it has increased compared with the membrane electrode prepared by modifying the carrier with the optimal feed ratio of 1:2, it is still much lower than the membrane electrode prepared by commercial catalysts.

[0085] Comparative Example

[0086] In step (1) of Example 1, the addition of the S-containing precursor was omitted, the carbon support was not modified, and a commercial C support (EC300) was directly used. The rest was the same as Example 1.

[0087] Fig.10 The ultra-low-load full cell (cathode loading 0.1 mg / cm2) prepared by the catalyst without modifying the carrier is shown in the comparative example. 2 , anode loading 0.025mg / cm 2 , 80℃, 1.5bar, constant dosage ratio 1.5~2.0, IC ratio 0.5) performance diagram and oxygen mass transfer impedance-pressure diagram, Fig.10 The left figure is the performance diagram, and the right figure is the oxygen mass transfer impedance-pressure diagram. Fig.10 It can be seen that the ultra-low-load film electrode prepared by the catalyst without modifying the carbon carrier still has better performance than the commercial Pt / C catalyst. This is because the catalyst without modifying the carrier is a platinum-cobalt alloy catalyst, and the performance of the alloy catalyst is higher than that of the pure platinum-carbon catalyst. Fig.10 The left figure also shows that whether the carrier is modified is crucial to the performance improvement of the platinum-cobalt alloy catalyst. After the carrier is modified with thiophene sulfide (CSC), the performance is improved by more than 80%. Fig.10 The middle right figure shows that the non-pressure oxygen mass transfer resistance of the membrane electrode without carrier modification is 0.236s / cm, which is 4.21 times that of the membrane electrode after carrier modification with thiophene sulfur, indirectly indicating that the distribution of ionomers in the catalyst layer of the membrane electrode is uneven and oxygen transmission is hindered.

[0088] Figure 11 to Figure 13 TEM-Mapping images of different elements in three random regions of the membrane electrode prepared by the catalyst without modifying the carrier in Comparative Example 1. Fig.11 TEM-Mapping of membrane electrode area 1 prepared for catalyst without carrier modification. Fig.11(a) is the catalyst morphology of the region, (b) is the F signal distribution of the region, (c) is the Pt signal distribution of the region, and (d) is the superposition distribution of the morphology, F signal and Pt signal of the region. Fig.12 TEM-Mapping of membrane electrode area 2 prepared for catalyst without carrier modification. Fig.12 (a) is the catalyst morphology of the region, (b) is the F signal distribution of the region, (c) is the Pt signal distribution of the region, and (d) is the superposition distribution of the morphology, F signal and Pt signal of the region. Fig.13 3TEM-Mapping of the membrane electrode area prepared for the catalyst without carrier modification. Fig.13 (a) is the catalyst morphology of the area, (b) is the F signal distribution of the area, (c) is the Pt signal distribution of the area, and (d) is the superimposed distribution of the morphology, F signal and Pt signal of the area.

[0089] Figure 11 to Figure 13 It directly shows the distribution of ionomers in the catalyst layer of the membrane electrode prepared by the catalyst without modified thiophene sulfur on the carrier. In the figure, the F element represents the distribution of ionomers (nafion), and the Pt element represents the distribution of catalyst particles. It can be seen that without the interaction between thiophene S (CSC) on the carrier and ionomers, the ionomers are distributed very unevenly and aggregate into pieces, making it difficult for oxygen in this area to pass through the ionomers to reach the catalyst surface to participate in the reaction; and the ionomer content near the platinum particles is very low, making most of the catalyst particles naked. Without the ionomer wrapping in this area, protons cannot reach the catalyst surface to participate in the reaction, which ultimately leads to poor performance of the membrane electrode.

[0090] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A cathode catalyst layer of a proton exchange membrane fuel cell, characterized in that: The invention comprises a platinum-based catalyst and an ionomer, and the preparation method of the platinum-based catalyst comprises the following steps: Mixing a sulfur-containing precursor, a carbon support and a solvent and evaporating them under reduced pressure to obtain a first precursor mixture; Subjecting the first precursor mixture to a first heat treatment in an inert atmosphere to obtain a sulfur-doped carbon support; Mixing a cobalt salt, a platinum salt, a solvent and the sulfur-doped carbon support and evaporating the mixture under reduced pressure to obtain a second precursor mixture; The second precursor mixture is subjected to a second heat treatment in a reducing atmosphere, and then the obtained material is subjected to an annealing treatment to obtain the platinum-based catalyst.

2. The cathode catalyst layer of a proton exchange membrane fuel cell according to claim 1, characterized in that: The sulfur-containing precursor includes one or more of sulfonated phthalocyanine salts, thiophene, dithiophene, propanethiol, pentamethylenethiol, cyclohexanethiol, thiourea and aminosulfonate; the carbon carrier includes carbon black; the mass ratio of the sulfur-containing precursor to the carbon carrier is 10:1 to 1:

10.

3. The cathode catalyst layer of a proton exchange membrane fuel cell according to claim 1 or 2, characterized in that: The temperature of the first heat treatment is 900-1000° C., and the time is 1.5-6 hours.

4. The cathode catalyst layer of a proton exchange membrane fuel cell according to claim 1, characterized in that: The molar ratio of the Co element in the cobalt salt to the Pt element in the platinum salt is 1:1 to 1:3, and the mass of the Pt element in the platinum salt is 5 to 60% of the mass of the sulfur-doped carbon carrier.

5. The cathode catalyst layer of a proton exchange membrane fuel cell according to claim 1 or 4, characterized in that: The mixture of the cobalt salt, the platinum salt, the solvent and the sulfur-doped carbon carrier also includes adding small molecule sulfur, which includes one or more of elemental sulfur, propyl mercaptan, 1,3-propanediol, 11-mercaptohexadecanoic acid, 2-mercaptobenzimidazole, 1-mercaptopropane and sodium thioglycolate; the molar ratio of the small molecule sulfur to the Pt element in the platinum salt is 3:1 to 1:

1.

6. The cathode catalyst layer of a proton exchange membrane fuel cell according to claim 1, characterized in that: The reducing atmosphere is a mixed atmosphere of hydrogen and argon, the temperature of the second heat treatment is 750-950° C., and the time is 1.5-3 hours.

7. The cathode catalyst layer of a proton exchange membrane fuel cell according to claim 1, characterized in that: The annealing treatment is performed at a temperature of 400 to 600° C. and for a time of 2 to 5 hours.

8. The cathode catalyst layer of a proton exchange membrane fuel cell according to claim 1, characterized in that: The ionomer comprises one or more of perfluorosulfonic acid resin, sulfonated polyarylethersulfone, sulfonated polyarylether(sulfide), sulfonated polyetheretherketone, sulfonated polyimide and polybenzimidazole; the mass ratio of the ionomer to the sulfur-doped carbon carrier in the platinum-based catalyst is 0.2 to 1:

1.

9. A proton exchange membrane fuel cell membrane electrode, characterized in that: It comprises a proton exchange membrane, a cathode catalyst layer composited on one side surface of the proton exchange membrane and an anode catalyst layer composited on the other side surface of the proton exchange membrane, wherein the cathode catalyst layer is the cathode catalyst layer of the proton exchange membrane fuel cell according to any one of claims 1 to 8, and the anode catalyst layer is a Pt / C catalyst layer.

10. The proton exchange membrane fuel cell membrane electrode according to claim 9, characterized in that: The Pt loading in the cathode catalyst layer is 0.1-0.5 mg / cm 2 The Pt loading in the anode catalyst layer is 0.01 to 0.05 mg / cm 2 .