Anion exchange composite membrane as well as preparation method and application thereof
By adding high-thermal conductivity inorganic materials to the anion exchange membrane to form a 3D thermal conductivity network, the problem of insufficient thermal conductivity of the anion exchange membrane is solved, and its durability and conductivity under the electrolytic cell conditions are significantly improved, thus achieving higher Thermal alkali stability and service life.
Patent Information
- Application Number
- CN202411304895.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-12
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The durability of anion exchange membrane in electrolytic cell conditions is much lower than that in an off-position environment. The main reason is that the thermal conductivity is low, which leads to heat accumulation, deterioration of mechanical properties and a decrease in ionic conductivity.
Add inorganic materials with high thermal conductivity, such as layered boron nitride and carbon nanotubes, to form a 3D thermal conductivity network, which improves the thermal conductivity and electrical conductivity of the film and reduces heat accumulation.
It significantly improves the in-situ durability and thermal alkali stability of the anion exchange composite membrane, extends its service life, and shows good application prospects in a variety of energy storage and conversion devices.
Smart Images

Figure CN118943440A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ion exchange membranes, and more specifically, relates to a durable organic / inorganic composite anion exchange composite membrane and a preparation method and application thereof, which are mainly used in water electrolysis, fuel cells, liquid flow batteries, and CO2 electrolysis. Background Art
[0002] Hydrogen energy is an important part of the future energy system and will promote the transformation of fossil energy and carbon emission reduction in the energy field. High-efficiency, low-cost, zero-emission renewable energy water electrolysis to produce hydrogen is a key technology for the utilization of hydrogen energy. The anion exchange membrane electrolyzer (AEMWE) integrates the advantages of the alkaline electrolyzer (AWE) and the proton exchange membrane electrolyzer (PEMWE), and has the advantages of high current density, high energy efficiency, fast response speed, and adaptability to elastic loads. In particular, AEMWE uses cheap transition metal catalysts instead of precious metal catalysts in PEMWE, which can significantly reduce the cost of the electrolyzer; using pure water or low-concentration alkaline aqueous solution as the electrolyte avoids the corrosion of the AWE strong alkaline solution to the equipment. Therefore, AEMWE is a water electrolysis hydrogen production technology with great cost and performance advantages.
[0003] Anion exchange membrane (AEM) is the core component of AEMWE, which is generally composed of a polymer skeleton, cation exchange groups and hydroxide ions to achieve OH - The key functions of AEM include OH transfer and gas isolation, which have an important impact on the efficiency and durability of hydrogen production by water electrolysis. - The ionic conductivity is generally low and the stability is insufficient under high temperature and strong alkaline environment.
[0004] At present, the research on AEM is mainly focused on designing the polymer main chain, side chain, and cation exchange group based on source chemistry, optimizing the size, structure, and structural orientation of ion channels, regulating the structure of membrane components, and regulating ion transport channels to improve the ionic conductivity and thermal alkaline stability of AEM. However, the actual durability of AEM under electrolytic conditions is far worse than the stability measured in an off-site environment. For example, the off-site stability of quaternary ammonium salt polymers is up to 1200h, while the durability of the electrolytic cell based on this polymer is less than 72h, which seriously limits the commercialization process of AEM-based electrochemical devices. Therefore, how to achieve excellent in-situ durability under electrolytic cell conditions is an important challenge in the development of AEM. Summary of the invention
[0005] 1. Problem to be solved
[0006] Many existing documents show that there is a huge difference between the AEM working condition and the off-site stability. However, there is no prior art to reveal the fundamental reason for this difference. In the present invention, the inventors found that the AEM temperature under the electrolytic cell working condition was high through in-situ temperature measurement experiments. After analyzing the reasons, it was found that the thermal conductivity of the AEM was at the lowest level among all the components of the electrolytic cell. The heat generated by the current in the electrolysis process, such as Joule heat, would accumulate in the AEM, leading to deterioration of mechanical properties, decrease in ionic conductivity, device failure and other problems. This problem has become the main reason for the huge difference between the AEM working condition and the off-site stability.
[0007] Based on the discovery of the above problems, in order to solve the problem of poor durability of the electrolytic cell of AEM in the prior art, the present invention intends to provide an anion exchange composite membrane from the perspective of improving the thermal conductivity of AEM by reducing the thermal conductivity difference between AEM and other components in the electrolytic cell. The anion exchange composite membrane can effectively dissipate heat and reduce the membrane temperature, thereby improving the durability of the anion exchange composite membrane, which is of great significance for improving the thermal and alkaline stability of the anion exchange membrane and provides a new idea for the future development of highly durable anion exchange membranes.
[0008] 2. Technical solution
[0009] The present invention proposes a strategy for developing a high thermal conductivity anion exchange composite membrane from the perspective of improving the thermal conductivity of the anion exchange membrane. Experimental results show that adding thermal conductive materials can effectively improve the in-situ durability of the AEM. Specifically, the present invention provides the following technical solutions:
[0010] [Anion exchange composite membrane]
[0011] The first aspect of the present invention provides an anion exchange composite membrane, the composite membrane comprising component A and component B;
[0012] The component A is a polymer material containing a cationic group, and the polymer material is selected from one or more of chitosan, polyaryl piperidines, polyvinyl alcohols, polyphenylene ethers, polyether ketones, polyphenylene sulfides, polybenzimidazoles, polyaryl pyridines, polyaryl alkylenes, polystyrenes, perfluorosulfonic acid resins, poly(styrene) oxides, polyethylenes and poly(ethylene-co-tetrafluoroethylene) polymer materials;
[0013] The component B is an inorganic material;
[0014] The thermal conductivity of component B is not less than 5 times the thermal conductivity of component A;
[0015] The thermal conductivity of the anion exchange composite membrane is not less than 1.5 W m –1 K –1 .
[0016] Preferably, component A and component B are physically mixed and non-covalently bonded.
[0017] As described herein, the test method of thermal conductivity is well known in the art. The theoretical thermal conductivity of general materials can be obtained from the literature or tested by the following method:
[0018] The thermal conductivity of the composite film can be obtained by laser pulse method, 3ω test method, photothermal reflection method, scanning thermal microscopy method, etc.
[0019] As used herein, a "polymeric material" refers to a high molecular weight (usually up to 10 4 ~10 6 ) compounds.
[0020] As used herein, "polymeric material containing cationic groups" refers to a polymer material having the backbone or side chains modified with cationic functional groups.
[0021] The invention improves the thermal conductivity of the anion exchange composite membrane by adding an inorganic material with high thermal conductivity into a polymer material containing a cationic group, thereby improving the durability of the electrolytic cell of the anion exchange composite membrane.
[0022] As a preferred embodiment of any embodiment of the first aspect of the present invention, the thermal conductivity of the anion exchange composite membrane is not less than 2Wm –1 K –1 , more preferably not less than 5W m –1 K –1 , not less than 10W m –1 K –1 The improvement of the thermal conductivity of the anion exchange composite membrane is beneficial to reduce the difference in thermal conductivity between the AEM and other components in the electrolyzer, reduce the heat accumulation of the AEM, and improve the thermal stability of the composite membrane.
[0023] As a preferred embodiment of any embodiment of the first aspect of the present invention, the theoretical thermal conductivity of the inorganic material is not less than 5Wm –1 K –1 , more preferably not less than 10W m –1 K –1 , not less than 20W m –1 K –1 , not less than 50W m –1 K –1 , not less than 100W m –1 K –1 , not less than 200W m –1 K –1 , not less than 300W m –1 K –1 , not less than 400W m–1 K –1 .
[0024] As a preferred embodiment of any embodiment of the first aspect of the present invention, the thermal conductivity of component B is not less than 8 times the thermal conductivity of component A, and further preferably, the thermal conductivity of component B is not less than 10 times the thermal conductivity of component A, the thermal conductivity of component B is not less than 20 times the thermal conductivity of component A, the thermal conductivity of component B is not less than 50 times the thermal conductivity of component A, the thermal conductivity of component B is not less than 100 times the thermal conductivity of component A, and the thermal conductivity of component B is not less than 200 times the thermal conductivity of component A.
[0025] It is worth noting that, from the perspective of improving the thermal conductivity of the anion exchange composite membrane, the inorganic material of component B with a higher thermal conductivity is preferred.
[0026] As used herein, "inorganic material" refers to inorganic materials, which are materials made of inorganic substances alone or mixed with other substances. It usually refers to materials prepared by certain processes from raw materials such as silicates, aluminates, borates, phosphates, germanates, etc. and / or raw materials such as oxides, nitrides, carbides, borides, sulfides, silicides, halides, etc.
[0027] As a preferred embodiment of any one of the first aspects of the present invention, the inorganic material is selected from one or more of boron nitride, silicon carbide, molybdenum disulfide, zirconium dioxide, silicon dioxide, magnesium oxide, carbon nanotubes, graphene, silicon nitride and aluminum oxide, preferably boron nitride and carbon nanotubes.
[0028] Among them, the theoretical thermal conductivity of boron nitride is about 600W m –1 K –1 The out-of-plane theoretical thermal conductivity is about 30 W m –1 K –1 The theoretical thermal conductivity of carbon nanotubes is about 6000 W m –1 K –1 The theoretical thermal conductivity of silicon carbide is about 490 W m –1 K –1 The theoretical thermal conductivity of MoS2 is about 40 W m –1 K –1 The theoretical thermal conductivity of zirconium dioxide is about 6.2 W m –1 K –1 The theoretical thermal conductivity of silicon dioxide is about 0.8 to 1.3 W m –1 K –1 The theoretical thermal conductivity of magnesium oxide is about 36 W m –1 K –1 , the theoretical thermal conductivity of graphene is about 5000 W m –1 K –1The theoretical thermal conductivity of silicon nitride is about 100 W m –1 K –1 The theoretical thermal conductivity of alumina is about 150 W m –1 K –1 .
[0029] The present invention introduces inorganic materials with intrinsic high thermal conductivity, such as boron nitride and carbon nanotubes, into a polymer membrane with fast ion conduction, thereby constructing a 3D continuous thermal conductive network in the AEM, thereby forming an AEM with a fast heat conduction channel and improving the in-situ durability of the AEM.
[0030] As a preferred embodiment of any of the first aspect of the present invention, the inorganic material is preferably layered boron nitride. The confined space formed by the layered boron nitride helps to achieve rapid ion transport, thereby improving the conductivity of the anion exchange membrane.
[0031] As preferred in any embodiment of the first aspect of the present invention, the cationic group is selected from one or more of N-containing, S-containing, quaternary phosphonium-containing or metal complex-containing cationic groups. Wherein, the N-containing cationic group is selected from one or more of non-cyclic quaternary ammonium ions, heterocyclic quaternary ammonium ions, guanidine groups, and imidazolium salts. Wherein, the quaternary ammonium cation can be trimethyl quaternary ammonium salt, benzyltrimethyl quaternary ammonium salt, bicyclo aliphatic spiral alkane quaternary ammonium salt, 1-methyl methyl nitrogen quaternary ammonium salt, 1-methyl pyrrolinium quaternary ammonium salt, quinidine quaternary ammonium salt, 1-methyl piperidinium quaternary ammonium salt, 1,4-dimethyl piperidinium quaternary ammonium salt, 1,3,5 trimethyl piperidinium quaternary ammonium salt and 1,2,6-trimethyl piperidinium quaternary ammonium salt, etc.
[0032] As used herein, "quaternary ammonium cation" refers to a quaternary ammonium functional group modified on the backbone or side chains of a given polymer.
[0033] As a preferred embodiment of any one of the first aspects of the present invention, based on the total mass of the anion exchange composite membrane, the mass percentage of the inorganic material in the anion exchange composite membrane is selected from any value within any one of the following numerical ranges:
[0034] 1-50%, 2-50%, 3-50%, 4-50%, 5-50%, 10-50%, 15-50%, 20-50%, 25-50%, 30-50%, 35-50%, 40-50%, 45-50%;
[0035] 1~45%, 2~45%, 3~45%, 4~45%, 5~45%, 10~45%, 15~45%, 20~45%, 25~45%, 30~45%, 35~45%, 40~45%;
[0036] 1~40%, 2~40%, 3~40%, 4~40%, 5~40%, 10~40%, 15~40%, 20~40%, 25~40%, 30~40%, 35~40%;
[0037] 1~35%, 2~35%, 3~35%, 4~35%, 5~35%, 10~35%, 15~35%, 20~35%, 25~35%, 30~35%;
[0038] 1-30%, 2-30%, 3-30%, 4-30%, 5-30%, 10-30%, 15-30%, 20-30%, 25-30%;
[0039] 1-25%, 2-25%, 3-25%, 4-25%, 5-25%, 10-25%, 15-25%, 20-25%;
[0040] 1-20%, 2-20%, 3-20%, 4-20%, 5-20%, 10-20%, 15-20%;
[0041] 1-15%, 2-15%, 3-15%, 4-15%, 5-15%, 10-15%;
[0042] 1-10%, 2-10%, 3-10%, 4-10%, 5-10%;
[0043] 1~5%, 2~5%, 3~5%, 4~5%.
[0044] Preferably, the mass percentage of the inorganic material in the anion exchange composite membrane is 5% to 30% based on the total mass of the anion exchange composite membrane, excluding 30%; preferably 5% to 29%; further preferably 5% to 25%. The present invention improves the thermal conductivity of AEM by adding a high thermal conductivity inorganic material to a polymer material containing a cationic group, especially a quaternized polymer material, to reduce the thermal conductivity difference between AEM and other components in the electrolytic cell, reduce heat accumulation, and further improve the in-situ durability of AEM in electrolysis conditions. The higher the amount of high thermal conductivity inorganic material added, the higher the thermal conductivity of AEM, but excessive addition of inorganic material will cause changes in the mechanical properties of AEM. In addition, experiments show that the electrical conductivity of AEM is not positively correlated with the amount of high thermal conductivity inorganic material added. When the amount of high thermal conductivity inorganic material added reaches a certain value, the electrical conductivity of the anion exchange composite membrane decreases. Therefore, considering the mechanical properties and electrical conductivity of AEM, the amount of high thermal conductivity inorganic material added should be kept within a reasonable range.
[0045] As a preferred embodiment of any one of the first aspects of the present invention, the anion exchange composite membrane has a membrane thickness of 5 to 500 μm, preferably 20 to 100 μm, and more preferably 30 to 50 μm.
[0046] [Method for preparing anion exchange composite membrane]
[0047] The second aspect of the present invention provides a method for preparing an anion exchange composite membrane according to any embodiment of the first aspect of the present invention, comprising:
[0048] Step 1: preparing a casting solution: mixing a polymer material A containing a cationic group and an inorganic material B in a solvent;
[0049] Step 2: forming a membrane from the casting solution.
[0050] As a preferred embodiment of any embodiment of the second aspect of the present invention, the preparation method specifically comprises:
[0051] Step 1: preparing a casting solution;
[0052] Dissolving a polymer material A containing a cationic group in a solvent to obtain a polymer dispersion, and at the same time uniformly dispersing an inorganic material B in the same solvent to obtain an inorganic material dispersion, and mixing the two dispersions uniformly to obtain an A / B mixed casting solution; or
[0053] Directly dissolving or dispersing polymer material A and inorganic material B in the same solvent to obtain an A / B mixed casting solution;
[0054] Step 2: Forming a membrane from the casting solution:
[0055] The casting solution obtained in step 1 is used to form a membrane by different casting methods, wherein the casting method is selected from a casting method, a blade coating method and a coating method, to form an anion exchange composite membrane.
[0056] As a preferred embodiment of any embodiment of the second aspect of the present invention, in step 2, the volume percentage of the polymer dispersion is 99% to 1%, and the volume percentage of the inorganic material dispersion is 1% to 99%.
[0057] As a preferred embodiment of any embodiment of the second aspect of the present invention, the polymer material is chitosan.
[0058] As a preferred embodiment of any one of the second aspects of the present invention, the polymer material is a polyarylpiperidine polymer, such as poly(N-methyl-piperidine-co-p-terphenyl).
[0059] As a preferred embodiment of any one of the second aspects of the present invention, the inorganic material is boron nitride, preferably layered boron nitride.
[0060] As a preferred embodiment of any embodiment of the second aspect of the present invention, the inorganic material is carbon nanotubes.
[0061] As a preferred embodiment of any one of the second aspects of the present invention, in step 1, the concentration of A in the casting solution is 0.3 g / mL to 1.0 g / mL.
[0062] As a preferred embodiment of any of the second aspects of the present invention, in step 2, a film is formed from the casting liquid by a casting method, a doctor blade method or a coating method.
[0063] As a preferred embodiment of any of the second aspects of the present invention, in step 2, the ambient pressure of the evaporation film when the film is formed from the casting liquid is 100 Pa to 10 5 Pa.
[0064] As a preferred embodiment of any embodiment of the second aspect of the present invention, in step 2, the temperature of evaporation film formation is room temperature to 150°C.
[0065] [Membrane Electrode Assembly]
[0066] The third aspect of the present invention provides a membrane electrode assembly, which includes an anion exchange composite membrane according to any embodiment of the first aspect of the present invention, or an anion exchange composite membrane prepared according to any embodiment of the second aspect of the present invention; and a catalyst coated on both sides of the anion exchange composite membrane, the catalyst comprising a cathode catalyst and an anode catalyst.
[0067] As a preferred embodiment of any of the third aspects of the present invention, the cathode catalyst is selected from one or more of Pt / C, NiFe, NiFeV, and NiFeCo hydroxides.
[0068] As a preferred embodiment of any of the third aspects of the present invention, the anode catalyst is one or more of IrO2, RuO2, NiFe, NiFeV, and NiFeCo hydroxides.
[0069] [Electrolyzer]
[0070] The fourth aspect of the present invention provides an electrolytic cell, which includes the anion exchange composite membrane of any embodiment of the first aspect of the present invention, or includes the anion exchange composite membrane obtained by the preparation method of any embodiment of the second aspect of the present invention, or includes the membrane electrode assembly described in any embodiment of the third aspect of the present invention.
[0071] [Application of anion exchange composite membrane]
[0072] The fifth aspect of the present invention provides an anion exchange composite membrane according to any embodiment of the first aspect of the present invention, or an anion exchange composite membrane obtained by the preparation method of any embodiment of the second aspect of the present invention, or a membrane electrode assembly described in any embodiment of the third aspect of the present invention, and their use in water electrolysis, fuel cells, liquid flow batteries, supercapacitors or CO2 electrolysis.
[0073] 3. Beneficial effects
[0074] Compared with AEM technology (such as polymers containing cationic groups) without adding high thermal conductivity inorganic materials, the advantages of the present invention are as follows:
[0075] (1) The present invention has discovered for the first time an important factor that causes a huge difference between the working conditions and off-site stability of AEM, namely, among all the components of the electrolytic cell, the thermal conductivity of AEM is at the lowest level, and the heat such as Joule heat generated by the current in the electrolysis process is accumulated in the AEM, which leads to deterioration of mechanical properties, decrease in ionic conductivity, and device failure. Therefore, the electrolytic cell durability of AEM in the prior art is poor. In view of this problem, the present invention provides an anion exchange composite membrane, which is formed by adding a high thermal conductivity inorganic material to a polymer material containing a cationic group, so that the formed anion exchange composite membrane has a high thermal conductivity. Experimental results show that after adding the high thermal conductivity inorganic material, the anion exchange composite membrane has significantly improved in-situ durability.
[0076] (2) Furthermore, the experiments in the present invention show that inorganic materials construct a 3D thermal conductive network in the anion exchange composite membrane, which can form a structure with a fast heat conduction channel. The formed confined space is conducive to the rapid transmission of ions, thereby improving the conductivity of the anion exchange membrane.
[0077] (3) The present invention further proves that when the addition amount of high thermal conductivity inorganic materials, especially layered boron nitride, is within a specific range in the anion exchange composite membrane, the electrical conductivity and thermal conductivity of the anion exchange composite membrane can be simultaneously guaranteed, so that the anion exchange composite membrane maintains a high in-situ durability.
[0078] (4) The method for preparing the anion exchange composite membrane of the present invention only requires physically mixing the cationic group-containing polymer with the high thermal conductivity inorganic material to form a casting solution, and then preparing the membrane. The preparation process is simple, the material selection range is wide, and the conditions are simple.
[0079] (5) Due to its high thermal conductivity and electrical conductivity, the anion exchange composite membrane of the present invention can inhibit the degradation reaction of the polymer-based membrane and effectively extend the service life of the anion exchange membrane. It can have good application prospects in various energy storage and conversion devices, for example, it can be applied to multiple fields including water electrolysis to produce hydrogen, fuel cells, liquid flow batteries, CO2 electrolysis, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0080] Figure 1 A schematic diagram of the structure of the high thermal conductivity anion exchange composite membrane doped with inorganic materials of the present invention;
[0081] Figure 2 SEM cross-sectional images of the QCS / BN (left) prepared in Example 1 and the QAPPT / BN (BN volume ratio 8.9%) composite membrane (right) prepared in Example 6;
[0082] Figure 3 The test data diagram of the electrical conductivity and thermal conductivity of the QCS / BN composite film prepared in the embodiment and the comparative example;
[0083] Figure 4 The tensile strength data of the QCS / BN composite films prepared in the examples and comparative examples are shown in FIG.
[0084] Figure 5 The actual internal temperature data (left) and electrolytic water stability test data of the QCS / BN composite membrane prepared in the examples and comparative examples during operation (right);
[0085] Figure 6 It is a data chart of long-term stability test of QCS / BN composite membrane water electrolysis prepared in the examples and comparative examples;
[0086] Figure 7 The conductivity and tensile strength data of the QAPPT / BN composite membranes prepared in the examples and comparative examples are shown in FIG.
[0087] Figure 8 Data graphs showing the thermal conductivity (left) and long-term stability test of electrolyzed water (right) of the QAPPT / BN composite membranes prepared in the examples and comparative examples. DETAILED DESCRIPTION
[0088] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the term "and / or" used herein includes any and all combinations of one or more of the associated listed items.
[0089] The chitosan used in the examples was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0090] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0091] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.
[0092] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.
[0093] like Figure 1 The figure shows the structure of the high thermal conductivity ion exchange composite electrolytic cell doped with inorganic materials of the present invention. The AEM electrolytic cell is mainly composed of an anion exchange membrane, a catalyst layer, a gas diffusion layer and a bipolar plate. Working principle: It involves two half reactions: oxygen evolution reaction and hydrogen evolution reaction. Using pure water or alkaline solution as the electrolyte, the electrolysis device electrochemically decomposes water and produces oxygen and hydrogen under the drive of 1.8-2.5V voltage. The technical core of the AEM electrolytic cell is the anion exchange membrane, which converts OH - transport from cathode to anode while preventing gas crossover on both sides of the membrane.
[0094] In the examples and comparative examples, the thermal conductivity is obtained by directly measuring the film using a laser thermal conductivity analyzer (LFA467 Super Flash) under nitrogen atmosphere.
[0095] The present invention is further described below in conjunction with specific embodiments.
[0096] Example 1
[0097] This embodiment uses chitosan as a polymer to provide a method for preparing a high thermal conductivity anion exchange membrane by constructing a 3D thermal conductive network, which specifically includes the following steps:
[0098] Step 1: Preparation of casting solution;
[0099] (1) Preparation of quaternized chitosan polymer:
[0100] The chitosan is prepared by ring-opening reaction with a quaternary ammonium agent under alkaline conditions, specifically including the following contents:
[0101] Weigh 4g of chitosan (viscosity>400mPa.s) and dissolve it in 1% acetic acid solution. Stir mechanically at 1500rpm for 2 hours at 25℃, and slowly add NaOH solution. At this time, white flocculent precipitate appears in the solution. Wash it with deionized water 2-3 times to obtain a colloid.
[0102] Take another 12 g of quaternary ammonium agent 2,3-epoxypropyltrimethylammonium chloride and dissolve it in a certain amount of a mixed solution of water and isopropanol.
[0103] The obtained chitosan colloid was placed in a round-bottom flask, and an appropriate amount of water and isopropanol solution were poured in. The mixture was mechanically stirred at 1000 rpm at 80°C. The above-prepared 2,3-epoxypropyltrimethylammonium chloride solution was poured into the round-bottom flask in several times. The reaction was continued for 8 hours. The mixture was cooled and the product was washed with ethanol for 2 to 3 times. The quaternized chitosan polymer was obtained by drying for later use.
[0104] (2) Preparation of casting solution:
[0105] The quaternary ammonium chitosan polymer (QCS, 2.0 g) prepared in step (1) is dissolved in a 1% acetic acid solution. After the solution is completely dissolved, the layered boron nitride nanosheets are doped according to a volume percentage of 10.6% (the mass percentage of BN in the anion exchange composite membrane is 25%, and the mass of the anion exchange composite membrane is calculated based on the total mass of the quaternary ammonium chitosan polymer and BN) relative to the quaternary ammonium chitosan polymer. The above liquids are mixed evenly to obtain a QCS / BN casting solution.
[0106] Step 2: Preparation of high thermal conductivity anion exchange membrane;
[0107] The QCS / BN film casting solution prepared in step 1 was cast into a plastic culture dish and heated to 10 5 Pa conditions at room temperature to 150 ° C, the film was evaporated and cast, the obtained film was peeled off, immersed in NaOH solution for ion exchange, and the QCS / BN thermal conductive anion exchange composite membrane was obtained. The thickness of the anion exchange composite membrane is about 30 to 50 μm, and the thermal conductivity is about 6.2 W m –1 K –1 .
[0108] Example 2
[0109] The steps of this embodiment are basically the same as those of embodiment 1, except that in step (2), the volume percentage of layered boron nitride nanosheets relative to the quaternized chitosan polymer is 1.8% (the mass percentage of BN in the anion exchange composite membrane is 5%).
[0110] The thickness of the obtained anion exchange composite membrane is about 30-50 μm, and the thermal conductivity is about 2.9 W m –1K –1 .
[0111] Example 3
[0112] The steps of this embodiment are basically the same as those of embodiment 1, except that in step (2), the volume percentage of layered boron nitride nanosheets relative to the quaternized chitosan polymer is 5.9% (the mass percentage of BN in the anion exchange composite membrane is 15%).
[0113] The thickness of the obtained anion exchange composite membrane is about 30-50 μm, and the thermal conductivity is about 4.0 W m –1 K –1 .
[0114] Example 4
[0115] The steps of this embodiment are basically the same as those of embodiment 1, except that in step (2), the volume percentage of layered boron nitride nanosheets relative to the quaternized chitosan polymer is 16.1% (the mass percentage of BN in the anion exchange composite membrane is 35%).
[0116] The thickness of the obtained anion exchange composite membrane is about 30-50 μm, and the thermal conductivity is about 13.2 W m –1 K –1 .
[0117] Comparative Example 1
[0118] The steps of this comparative example are basically the same as those of Example 1, except that no layered boron nitride nanosheets are added in step (2).
[0119] The obtained QCS anion exchange membrane has a thickness of about 30 to 50 μm and a thermal conductivity of about 1.3 W m –1 K –1 .
[0120] Example 5
[0121] This example is a test example of the anion exchange membrane obtained in Examples 1 to 4 and Comparative Example 1.
[0122] 1. SEM
[0123] The composite films with different doping ratios of boron nitride nanosheets in Examples 1 to 4 and Comparative Example 1 were dried, and the SEM cross-sectional images of the composite films were measured. The SEM cross-sectional images of the composite film prepared in Example 3 are as follows: Figure 2 (Left) As shown, flaky boron nitride nanosheets are successfully dispersed in the polymer matrix to construct a 3D continuous thermal conductive network.
[0124] (II) Electrochemical performance test
[0125] The thermal conductivity and electrochemical performance tests were performed on the composite films with different doping ratios of layered boron nitride nanosheets in Examples 1, 3 and 4 and Comparative Example 1.
[0126] The thermal conductivity of the composite film was directly measured by a laser thermal conductivity analyzer (LFA467 Super Flash) under nitrogen atmosphere.
[0127] In OH - Before the conductivity measurement, the composite membranes were immersed in 1 M NaOH for 24 h and washed with deionized water. The in-plane OH of the composite membranes was measured using the four-electrode method in water at temperatures ranging from 25 °C to 90 °C. – Conductivity. Electrochemical impedance spectroscopy (EIS) was performed on an electrochemical station (frequency from 100 kHz to 1 Hz). The σ hydroxide conductivity was calculated using the following formula:
[0128]
[0129] Where L is the distance between the two electrodes in cm, R is the resistance obtained by EIS test (the actual axis value at the high frequency intercept) in Ω, and S is the cross-sectional area of the membrane in cm 2 .
[0130] like Figure 3 As shown in the figure, as the BN doping volume percentage (relative to the polymer material containing cationic groups) increases from 0 to 15%, the thermal conductivity of the composite membrane gradually increases, but in the ratio range of 5% to 10% of the BN doping volume percentage, the electrical conductivity of the composite membrane reaches the highest. Therefore, the preferred doping volume percentage of BN in the QCS / BN anion exchange composite membrane is 5% to 10%.
[0131] (III) Mechanical properties test
[0132] At a stretching speed of 6 mm min -1 The tensile strength test was carried out on a tensile testing machine (ETNALN YTN-D5-PC) and the average value was obtained from at least three tests. The size of the sample was 1.5 cm*0.5 cm.
[0133] The results show that in Examples 1 to 4 and Comparative Example 1, as the doping ratio of boron nitride nanosheets increases, the tensile strength of the composite film is significantly improved, reaching the highest value when the volume ratio is between 5% and 10% (e.g. Figure 4 However, when the doping ratio of boron nitride nanosheets continues to increase, the tensile strength of the composite film decreases.
[0134] (IV) Conducting electrolytic water stability test on the composite membrane.
[0135] Activation: The composite anion exchange membranes prepared in Examples 1, 2 and 4 and Comparative Example 1 were placed in a 1M potassium hydroxide solution for activation for at least 12 hours, then washed with deionized water until the pH value of the membrane surface was about 7, and dried for later use.
[0136] Prepare anode catalyst slurry and cathode catalyst slurry separately:
[0137] Preparation of anode catalyst slurry: Commercial IrO2 (RuO2 or non-precious metal catalysts can also be used) is used as an electrode catalyst for electrocatalytic oxygen evolution reaction (OER). The anode catalyst (IrO2) and ion-conducting ionomer (FAA-3) with a mass ratio of 5:1 are added to an isopropanol solvent, and then ultrasonically treated in an ice water bath for 30-40 minutes to obtain an anode electrode ink, i.e., an anode catalyst slurry.
[0138] Preparation of cathode catalyst slurry: Commercial Pt / C (non-precious metal catalysts can also be used) is used as the electrocatalytic hydrogen evolution reaction (HER) electrode catalyst. The cathode catalyst (Pt / C) and ion-conducting ionomer (FAA-3) with a mass ratio of 5:1 are added to an isopropanol solvent, and then ultrasonically treated in an ice water bath for 30-40 minutes to obtain a cathode electrode ink, i.e., a cathode catalyst slurry.
[0139] The anode catalyst slurry and cathode catalyst slurry are directly sprayed on both sides of the membrane, and the thickness of the obtained membrane electrode MEA is about 60-80 μm, and the membrane electrode assembly (MEA) is obtained. 2 MEA.
[0140] Before the test, the prepared MEA was immersed in 1 M KOH aqueous solution for 12 h.
[0141] The performance of the single cell was evaluated on a water electrolysis apparatus at controlled temperature with 3M KOH as the electrolyte in both electrodes and a flow rate of 10 mL min –1 , at 1A cm -2 The durability of the composite films was studied in constant current mode at a current density of 2.50 Å and 60 °C.
[0142] While the electrolytic cell is in operation, the temperature of the electrolytic cell during operation is monitored.
[0143] like Figure 5 As shown, with the increase in the volume ratio of the thermally conductive material boron nitride nanosheets, the in-situ temperature of the composite membrane during the actual operation of the electrolytic cell can be effectively reduced; the voltage stability of the electrolyzed water is significantly improved.
[0144] like Figure 6 As shown in the long-term stability test, the composite membrane with added boron nitride nanosheets has significantly improved stability compared with the polymer membrane.
[0145] Example 6
[0146] This embodiment uses polyaryl piperidine as a polymer to provide a method for preparing a high thermal conductivity anion exchange membrane by constructing a 3D thermal conductive network, and specifically includes the following steps:
[0147] (I) Preparation of quaternized poly (N-methyl-piperidin-co-p-terphenyl) (QAPPT):
[0148] 1.69 g of p-terphenyl was dissolved in 8 mL of dichloromethane solution in a 25 mL three-necked round-bottom flask equipped with mechanical stirring. Subsequently, 1.26 g of N-methyl-4-piperidone was added and mixed thoroughly. 0.72 mL of trifluoroacetic acid and 6 mL of trifluoromethanesulfonic acid were slowly added at 0 ° C. Stirring, the solution was further reacted until it became viscous, and then precipitated in ice CH3OH (75 mL). The bulk material was sheared to terminate the local reaction and then washed with deionized water to neutrality. N-methyl-piperidin-co-p-terphenyl polymer was obtained after drying at 60 ° C for 24 hours.
[0149] 1 g of the above polymer was dissolved in 20 mL of DMSO, K2CO3 (0.89 g) was added, and 0.92 g of CH3I was added to the reaction system under light-shielding conditions. The mixture was kept at 40°C for 48 h. After that, the mixed solution was centrifuged to remove K2CO3 and then precipitated in ethyl acetate. The mixture was repeatedly washed with ethyl acetate and dried at 70°C to obtain the product quaternized poly (N-methyl-piperidin-co-p-terphenyl).
[0150] (ii) Preparation of QAPPT / BN casting solution: The steps are the same as those for the preparation of casting solution in step 1 (2) of Example 1, except that the quaternized chitosan is replaced by the quaternized poly(N-methyl-piperidinyl-co-terphenyl) obtained in this example, and the doping mass ratio of boron nitride nanosheets to the anion exchange composite membrane can be (0.05-0.25):1 (mass ratio). In this example, QAPPT / BN casting solutions with doping volume ratios of boron nitride nanosheets to quaternized poly(N-methyl-piperidinyl-co-terphenyl) of 4.4%, 8.9%, 13.5% and 18% were prepared, which were converted into doping mass percentages of BN to the anion exchange composite membrane of 5%, 10%, 15% and 20%, respectively).
[0151] (III) Preparation of QAPPT / BN composite membrane:
[0152] The steps are the same as those in Example 1, step 2: preparation of a high thermal conductivity anion exchange membrane, except that QCS / BN is replaced with QAPPT / BN with different added volume ratios, and the thickness is about 30-50 μm. The thermal conductivity of QAPPT / BN with a doping volume ratio of 8.9% is 11.9 W m –1 K –1 .
[0153] Comparative Example 2
[0154] The steps of this comparative example are basically the same as those of Example 6, except that no boron nitride nanosheets are added.
[0155] The obtained QAPPT anion exchange membrane has a thickness of about 30-50 μm and a thermal conductivity of about 0.95 W m –1 K –1 .
[0156] Example 7
[0157] This example is a test example of the anion exchange membrane prepared in Example 6 and Comparative Example 2, and the test conditions are the same as those in Example 5.
[0158] like Figure 2 (Right) Boron nitride nanosheets are successfully dispersed in a polymer matrix.
[0159] like Figure 7 As shown in the results of the conductivity test of the polyaryl piperidine composite membrane, the higher the doping ratio of boron nitride nanosheets, the higher the conductivity of the anion exchange composite membrane, reaching the highest value in the range of about 10%-15% (volume ratio). This shows that BN constructs a 3D thermal conductive network in the anion exchange composite membrane, which can form a structure with a fast heat conduction channel. The confined space formed is conducive to the rapid transmission of ions, thereby improving the conductivity of the anion exchange membrane.
[0160] At the same time, the tensile strength of the anion exchange composite membrane also reaches a maximum value in the range of about 10%-15% (volume ratio).
[0161] like Figure 8 As shown, compared with the QAPPT anion exchange membrane without BN addition, the QAPPT / BN composite membrane (8.9% BN by volume) has significantly improved thermal conductivity and voltage stability (400 h) for water electrolysis.
[0162] According to the principle of the present invention, the addition of thermal conductive materials can effectively improve the thermal conductivity of the polymer film and can significantly enhance the stability of the composite film in the application of electrolysis of water; when the amount of thermal conductive materials added is within a certain range, the mechanical strength of the polymer film can be effectively improved; in the case of a confined space formed by the thermal conductive materials, the electrical conductivity of the polymer film can be further effectively improved. Therefore, in addition to the examples shown in the above embodiments, other thermal conductive materials can be replaced for doping, such as inorganic thermal conductive materials such as silicon carbide, molybdenum disulfide, zirconium dioxide, silicon dioxide, magnesium oxide, graphene, silicon nitride and aluminum oxide, etc., which can improve the thermal conductivity and electrolytic stability of the ion exchange membrane to a certain extent.
[0163] The above content is a schematic description of the present invention and its implementation methods, which is not restrictive. What is shown in the embodiment is only one of the implementation methods of the present invention, and the actual implementation method is not limited thereto. Therefore, if a person of ordinary skill in the art is inspired by it and designs implementation methods and embodiments similar to the technical solution without creative design without departing from the purpose of the invention, they should all fall within the scope of protection of the present invention.
Claims
1. An anion exchange composite membrane, characterized in that: The composite film comprises component A and component B; Wherein, component A is a polymer material containing a cationic group, wherein the polymer material is selected from one or more of chitosan, polyaryl piperidines, polyvinyl alcohols, polyphenylene ethers, polyether ketones, polyphenylene sulfides, polybenzimidazoles, polyaryl pyridines, polyaryl alkylenes, polystyrenes, perfluorosulfonic acid resins, poly(styrene) oxides and poly(ethylene-cotetrafluoroethylene) polymer materials; Component B is an inorganic material; the thermal conductivity of component B is not less than 5 times the thermal conductivity of component A; The thermal conductivity of the anion exchange composite membrane is not less than 1.5 W m –1 K –1 .
2. The anion exchange composite membrane according to claim 1, characterized in that: The thermal conductivity of the anion exchange composite membrane is not less than 2 W m –1 K –1 ; preferably not less than 5W m –1 K –1 More preferably, not less than 10W m –1 K –1 .
3. The anion exchange composite membrane according to claim 1 or 2, characterized in that: The thermal conductivity of the inorganic material is not less than 5 W m –1 K –1 ; Preferably, the inorganic material is selected from one or more of boron nitride, silicon carbide, molybdenum disulfide, zirconium dioxide, silicon dioxide, magnesium oxide, carbon nanotubes, graphene, silicon nitride and aluminum oxide.
4. The anion exchange composite membrane according to claim 3, characterized in that: The cationic group is selected from one or more of N-containing, S-containing, quaternary phosphonium-containing or metal complex-containing cationic groups.
5. The anion exchange composite membrane according to claim 1 or 2, characterized in that: Based on the total mass of the anion exchange composite membrane, the mass percentage of the inorganic material in the anion exchange composite membrane is 1% to 50%.
6. The anion exchange composite membrane according to claim 1 or 2, characterized in that: The anion exchange composite membrane has a thickness of 5 to 500 μm.
7. The method for preparing an anion exchange composite membrane according to any one of claims 1 to 6, characterized in that: include: Step 1: preparing a casting solution: mixing component A and component B in a solvent; Step 2: forming a membrane from the casting solution.
8. A membrane electrode assembly, comprising the anion exchange composite membrane according to any one of claims 1 to 6; and a catalyst coated on both sides of the anion exchange composite membrane.
9. An electrolytic cell, comprising the anion exchange composite membrane according to any one of claims 1 to 6, or comprising the membrane electrode assembly according to claim 8.
10. Use of the anion exchange composite membrane according to any one of claims 1 to 6 or the membrane electrode assembly according to claim 8 in water electrolysis, fuel cells, flow batteries, supercapacitors or CO2 electrolysis.
Citation Information
Patent Citations
Anion exchange composite membrane as well as preparation method and application thereof
CN113621170A
Multifunctional radical scavenger, polymer electrolyte membrane including same, catalyst layer, membrane electrode assembly, and fuel cell
CN118302887A
Indigenous diaphragm and non-noble bi-functional catalysts based alkaline wastewaters electrolyzer
IN202441052211A
Method and apparatus for providing foley sound using artificial intelligence