Composite solid electrolyte and preparation method thereof

The oxygen-deficient titanium aluminum phosphate alkali metal material is prepared by hydrothermal reaction and heat treatment to combine with polyacrylonitrile to form a composite solid electrolyte, which solves the flexibility and interface contact performance of the lithium/sodium ion conductor structure and improves the electrochemistry of the battery Performance and cycle stability.

CN118943501APending Publication Date: 2024-11-12XINJIANG NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411277134.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing solid electrolytes of lithium/sodium ion conductor structures lack flexibility, poor interface contact performance, and cannot directly contact with metal lithium, resulting in poor electrochemical performance and limited cycle life of solid-state batteries; ionic conductances are present when using solid polymer electrolytes. The problems of low rate, low cation transfer number and poor oxidation resistance.

Method used

Hydrothermal reaction and heat treatment are used to prepare oxygen-deficient titanium aluminum alkali metal materials, and combined with polyacrylonitrile through solution casting to form a composite solid electrolyte, and oxygen vacancies are introduced to enhance the chemical interaction between inorganic electrolyte and organic polymer. It can promote the transmission and migration of lithium ions.

Benefits of technology

The ionic conductivity and mechanical strength of solid-state composite electrolytes are improved, the electrochemical window is broadened, and the electrochemical performance and cyclic stability of the battery are significantly improved, and the capacity retention rate reaches more than 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943501A_ABST
    Figure CN118943501A_ABST
Patent Text Reader

Abstract

The invention discloses a composite solid electrolyte and a preparation method thereof, and belongs to the technical field of battery electrolyte preparation, alkali metal salt, aluminum salt, a titanium source and phosphoric acid are used as raw materials, a precursor is obtained after hydrothermal reaction, drying and grinding are performed, the temperature is raised to 700-900 DEG C in an argon-hydrogen mixed atmosphere or an air atmosphere, annealing and cooling are performed, and an oxygen-deficient titanium aluminum phosphate alkali metal material is obtained; and mixing the polyacrylonitrile solution with the oxygen-deficient titanium aluminum phosphate alkali metal material, and drying to obtain the composite solid electrolyte. Organic-inorganic electrolyte compounding is adopted, so that the ionic conductivity is improved, the mechanical strength is enhanced, and an electrochemical window is widened. The introduction of oxygen vacancies (V-O) into the inorganic electrolyte not only affects the physical properties of the inorganic electrolyte, but also enhances the chemical interaction between the inorganic electrolyte and the polymer. The synergistic effect of oxygen deficiency between the inorganic electrolyte and the polymer promotes the transmission of lithium ions, so that the ionic conductivity is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrolyte preparation, and in particular to a composite solid electrolyte and a preparation method thereof. Background Art

[0002] Solid-state lithium batteries are a new type of battery technology that can meet the energy density requirements of charge and discharge while taking into account safety, cycle life and other performance. Compared with the lithium-ion batteries currently used in commercial applications, solid-state lithium batteries use solid electrolytes that are not easy to burn, which greatly improves the safety performance of the battery. Under ideal conditions, the diffusion rate of lithium in the solid state is higher than that in the liquid electrolyte, and theoretically higher output can be achieved, thereby increasing the power density of the battery. Secondly, solid electrolytes are not easy to decompose, so the operating voltage of the battery can be increased, thereby increasing the overall energy density of the battery. On the other hand, solid-state batteries do not need to encapsulate liquid electrolytes, which simplifies battery manufacturing technology.

[0003] Solid composite electrolytes are an emerging class of solid electrolytes that are expected to replace existing liquid electrolytes as electrolytes for future high energy density and power all-solid-state batteries. Composite electrolytes contain many solid-solid interfaces that affect ion transport paths, electrode-electrolyte compatibility and durability. Composite solid electrolytes contain internal interfaces formed by organic phases and inorganic phases and external interfaces formed by electrodes and solid electrolytes. Inorganic ion conductors can reduce the crystallinity of polymers. Inorganic ion conductors are usually thick (>500 mm) and difficult to manufacture on a large scale, but they have good transport properties (conductivity and migration number). In contrast, polymer ion conductors are easy to manufacture (<50 mm) and have better chemical stability in air than most inorganic materials. However, polymer electrolytes have lower migration numbers and ionic conductivity. Hybrid solid electrolytes aim to combine the advantages of two types of solid ion conductors for scalable applications in solid-state batteries. Solid composite electrolyte polymer-inorganic ceramics are considered to be a viable strategy to obtain high-performance solid electrolytes. Solid composite electrolytes are generally composed of a polymer matrix, an inorganic inert ceramic filler or a ceramic fast ion conductor, which can integrate the advantages of polymers and inorganic electrolytes. Compared with solid polymer electrolytes and inorganic solid electrolytes, solid composite electrolytes have excellent mechanical properties, high ionic conductivity, and good interface stability. Therefore, it is very necessary to develop organic-inorganic composite solid electrolytes with excellent performance.

[0004] NASICON solid electrolyte Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP) has many advantages, including high ionic conductivity (10 at room temperature) -4 -10 -5 S cm -1), high lithium ion transfer number, wide electrochemical window, remarkable stability in air / humid environment, and low manufacturing cost. However, LATP lacks flexibility and has poor interface contact performance. The more critical problem of LATP materials in practical applications is that they cannot come into direct contact with metallic lithium. When used as an all-solid-state lithium metal battery, metallic lithium will transfer Ti 4+ Reduction to Ti 3+ , the interface impedance between the solid electrolyte and the electrode is large, and solid-state batteries using LATP ceramic solid electrolytes always show poor electrochemical performance and limited cycle life. In addition, due to the brittleness and hardness of ceramic materials, their processing performance is poor. In contrast, solid polymer electrolytes are suitable for flexible battery design, but they also have problems such as low ionic conductivity, low cation transfer number and poor oxidation resistance. Summary of the invention

[0005] The present invention provides a composite solid electrolyte and a preparation method thereof, which effectively solves the problems that the existing solid electrolyte with lithium / sodium ion conductor structure lacks flexibility, has poor interface contact performance, and cannot directly contact with metallic lithium, thereby causing the solid-state battery to exhibit poor electrochemical performance and limited cycle life; the technical problems of low ion conductivity, low cation transfer number and poor oxidation resistance when using solid polymer electrolytes, and provides an oxygen-deficient lithium / sodium aluminum titanium phosphate and polyacrylonitrile composite solid electrolyte.

[0006] The first object of the present invention is to provide a method for preparing a composite solid electrolyte, comprising the following steps:

[0007] Aluminum salt and titanium source are added to ethanol to form solution A, and an alkali metal salt solution is added to solution A to obtain a mixed solution. Phosphoric acid is added to the mixed solution, stirred, and subjected to hydrothermal reaction at 180-200° C. to obtain an aluminum ion-doped oxygen-deficient precursor LiTiOPO. 4-y , drying, grinding, heating the precursor to 700-900° C. in a mixed gas synthesis atmosphere of a reducing atmosphere and a protective atmosphere, annealing, reducing the titanium element in the aluminum ion-doped oxygen-deficient precursor to obtain an oxygen-deficient titanium aluminum phosphate alkali metal material;

[0008] The oxygen-deficient aluminum titanium phosphate alkali metal material is added to a polyacrylonitrile solution, and an inorganic-organic composite is performed by a solution casting method to obtain a composite solid electrolyte.

[0009] As a preferred embodiment, the molar ratio of the alkali metal salt, the aluminum salt, the titanium source and the phosphoric acid is 1.3-2.6:3-6:17-34:60.

[0010] As a preferred embodiment, the mass ratio of the polyacrylonitrile to the oxygen-deficient aluminum titanium phosphate alkali metal material is 10 to 1:1.

[0011] As a preferred embodiment, the hydrothermal reaction time is 12 to 24 hours.

[0012] As a preferred implementation manner, the annealing time is 6 to 12 hours.

[0013] As a preferred implementation, the flow rate of the mixed gas is 20-40 sccm, the mixed gas is an argon-hydrogen mixed gas, and the mass ratio of argon to hydrogen is 19:1-3.

[0014] As a preferred implementation, the heating rate is 5°C / min.

[0015] As a preferred embodiment, the alkali metal salt is lithium hydroxide monohydrate, lithium hydroxide, lithium nitrate, lithium acetate, lithium carbonate, sodium hydroxide, sodium acetate, sodium nitrate or sodium carbonate; the aluminum salt is aluminum nitrate nonahydrate, aluminum oxide, aluminum hydroxide; the titanium source is titanium dioxide, hydrated titanium dioxide, titanium oxide, butyl titanate; the phosphorus source is phosphoric acid or ammonium dihydrogen phosphate.

[0016] The second object of the present invention is to provide a composite solid electrolyte prepared by the above preparation method.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] (1) The present invention provides a composite solid electrolyte and a preparation method thereof, which uses alkali metal salt, aluminum salt, titanium source and phosphoric acid as raw materials, undergoes hydrothermal reaction at 180-200°C, and obtains aluminum ion-doped precursor LiTiOPO with different oxygen defect levels by controlling different hydrothermal treatment times. 4-y , drying, grinding, heating the precursor to 700-900°C in a mixed gas synthesis atmosphere of a reducing atmosphere and a protective atmosphere, annealing, cooling, reducing the titanium element in the aluminum ion-doped oxygen-deficient precursor to a low-valent state, further inducing oxygen defects inside the material, and causing a phase transition to obtain an oxygen-deficient aluminum titanium phosphate alkali metal material; mixing a polyacrylonitrile solution with an oxygen-deficient aluminum titanium phosphate inorganic electrolyte, and performing an inorganic-organic composite by a solution casting method to obtain a composite solid electrolyte. Introducing oxygen vacancies (V··O) into inorganic matter will affect the physical properties of ceramics, which can strengthen the chemical interaction between the inorganic electrolyte and the organic polymer, and through the oxygen vacancies, the inorganic electrolyte and the organic polymer produce a synergistic effect, which can promote Li + Ion transport improves the ionic conductivity of the system. In the -C=N bond of the PAN molecular chain, the lone pair of electrons is located in the N atomic orbital, which is conducive to the formation of Li + coordinated electron donor-acceptor complexes, thereby facilitating Li+ Transport and migration. The present invention constructs a composite solid electrolyte composed of PAN, LATP / NATP and lithium salt, which not only successfully introduces oxygen defects, but also effectively regulates the oxygen defect concentration by regulating the aluminum ion doping concentration and the sintering temperature. A reasonable oxygen defect concentration can not only improve the ionic conductivity of the solid composite electrolyte, but also further provide a channel for ion insertion / extraction, thereby improving the electrochemical performance. The present invention adopts organic-inorganic composite to not only improve the ionic conductivity, but also enhance the mechanical strength and broaden the electrochemical window. The introduction of oxygen vacancies (VO) in the inorganic electrolyte not only affects the physical properties of the inorganic electrolyte, but also enhances the chemical interaction between the inorganic electrolyte and the polymer. The synergistic effect of oxygen defects between the inorganic electrolyte and the polymer promotes the transmission of lithium ions, thereby improving the ionic conductivity.

[0019] (2) The electrochemical performance of the battery is greatly improved by using the composite solid electrolyte provided by the present invention. When the voltage range is 2.0-4.5V and the current density is 0.1C, the discharge capacity of the battery Li|LATP-PAN / composite solid electrolyte|LiFePO4 is 256.20mAh g -1 After 100 cycles, the discharge capacity is 231.80 mAh g -1 The capacity retention rate is 90.48%. The performance test of all-solid-state Li|NATP-PAN / composite solid electrolyte|LiFePO4 battery shows that the initial discharge specific capacity is 255.0mA hg at a current density of 0.1C. -1 After 100 cycles, the discharge capacity remains at 229.6 mAh g -1 , the capacity retention rate is 90.0%.

[0020] (3) The preparation method of the composite solid electrolyte provided by the present invention has simple process, low equipment requirements, convenient operation, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 XRD patterns of materials prepared in Examples 1 to 3 and Comparative Example 1 of the present invention; wherein (a) is the lithium aluminum titanium phosphate material of Comparative Example 1 and the oxygen-deficient lithium aluminum titanium phosphate material prepared in Examples 1 to 3; (b) is the composite solid electrolyte prepared in Examples 1 to 3 and the electrolyte of Comparative Example 1;

[0022] Figure 2 Fourier transform infrared spectrum test chart of the oxygen-deficient lithium titanium aluminum phosphate material prepared in Examples 1 to 3 of the present invention and the lithium titanium aluminum phosphate material prepared in Comparative Example 1;

[0023] Figure 3Electron paramagnetic resonance test graphs of the oxygen-deficient lithium titanium aluminum phosphate materials prepared in Examples 1 to 3 of the present invention and the lithium titanium aluminum phosphate material prepared in Comparative Example 1;

[0024] Figure 4 Nyquist plots of the composite solid electrolytes prepared in Examples 1 to 3 of the present invention and the electrolyte prepared in Comparative Example 1;

[0025] Figure 5 Arrhenius plots of the total conductivity of the composite solid electrolytes prepared in Examples 1 to 3 of the present invention and the electrolyte prepared in Comparative Example 1;

[0026] Figure 6 Arrhenius plots of the intracrystalline conductivity of the composite solid electrolytes prepared in Examples 1 to 3 of the present invention and the electrolyte prepared in Comparative Example 1;

[0027] Figure 7 Arrhenius plots of the grain boundary conductivity of the composite solid electrolytes prepared in Examples 1 to 3 of the present invention and the electrolyte prepared in Comparative Example 1;

[0028] Figure 8 At 25°C, 0.025 mA cm -2 A graph showing the change of polarization voltage over time of a symmetrical battery assembled using the composite solid electrolyte of Example 1 of the present invention and the electrolyte of Comparative Example 1 respectively, in a long cycle of periodic constant current charge and discharge for 1 h each;

[0029] Fig. 9 The discharge capacity diagram of the battery Li|diaphragm / composite solid electrolyte|LiFePO4 assembled with Celagrd separator and the solid composite electrolyte of Example 1 and the electrolyte of Comparative Example 1 respectively at a current density of 0.1C and a voltage range of 2.0-4.5V;

[0030] Fig.10 The discharge rate capacity diagram of the battery Li|membrane / composite solid electrolyte|LiFePO4 assembled with the Celagrd membrane and the solid composite electrolyte of Example 1 and the electrolytes of Comparative Example 1, Comparative Example 2, and Comparative Example 3 at a current density of 0.1C and a voltage range of 2.5-4.2V. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.

[0032] In view of the technical problems mentioned in the background technology of the present invention: the existing solid electrolytes with lithium / sodium ion conductor structures lack flexibility, have poor interface contact performance, and cannot directly contact with metallic lithium, resulting in poor electrochemical performance and limited cycle life of solid-state batteries; the use of solid polymer electrolytes has the technical problems of low ion conductivity, low cation transfer number and poor oxidation resistance. The present invention constructs a composite solid electrolyte and a preparation method thereof.

[0033] The technical contents of the composite solid electrolyte of the present invention are described in detail below.

[0034] A method for preparing a composite solid electrolyte comprises the following steps:

[0035] Alkali metal salt, aluminum salt, titanium source and phosphoric acid are used as raw materials. First, aluminum salt and titanium source are added to ethanol to form solution A, and the alkali metal salt solution is added to solution A to obtain a mixed solution. Phosphoric acid is added to the mixed solution, stirred, and hydrothermally reacted at 180-200°C to obtain an aluminum ion-doped oxygen-deficient precursor, which is dried, ground, heated to 700-900°C in an argon-hydrogen mixed atmosphere, annealed, and cooled to obtain an oxygen-deficient titanium aluminum phosphate alkali metal material. The present invention effectively adjusts the oxygen defect concentration in the precursor of the synthetic target product by conducting a hydrothermal reaction at 180-200°C. The sintering temperature range is selected to be 700-900°C. The primary reason is that the target product cannot be synthesized below this synthesis temperature. The oxygen defect concentration in the solid electrolyte can be effectively adjusted again within this temperature range.

[0036] The oxygen-deficient titanium aluminum phosphate alkali metal electrolyte material is added to the polyacrylonitrile solution, stirred, dried, and a composite solid electrolyte is obtained by a solution casting method.

[0037] The composite solid electrolyte obtained by the above technical solution not only successfully introduces oxygen defects, but also effectively regulates the oxygen defect concentration by regulating the aluminum ion doping concentration and the sintering temperature. A reasonable oxygen defect concentration can not only improve the ionic conductivity of the solid composite electrolyte, but also further provide a channel for ion insertion / extraction, thereby improving the electrochemical performance. The present invention adopts organic-inorganic composites to not only improve the ionic conductivity, but also enhance the mechanical strength and broaden the electrochemical window. The introduction of oxygen vacancies (VO) in the inorganic electrolyte not only affects the physical properties of the inorganic electrolyte, but also enhances the chemical interaction between the inorganic electrolyte and the polymer. The synergistic effect of oxygen defects between the inorganic electrolyte and the polymer promotes the transmission of lithium ions, thereby improving the ionic conductivity.

[0038] In order to improve the ionic conductivity of the composite electrolyte, the mass ratio of the polyacrylonitrile to the oxygen-deficient titanium aluminum phosphate alkali metal material is 10 to 1:1. The oxygen-deficient titanium aluminum phosphate alkali metal material as a filler can increase the amorphous region inside the polyacrylonitrile and thus improve the ionic conductivity of the composite electrolyte. The composite electrolyte obtained within this mass ratio range has a high ionic conductivity and a certain mechanical strength.

[0039] In order to achieve better ionic conductivity, the molar ratio of the alkali metal salt, aluminum salt, titanium source and phosphoric acid is 1.3-2.6:3-6:17-34:60. Within this molar ratio range, the titanium aluminum phosphate alkali metal electrolyte material Li 1.3 Al 0.3 Ti 1.7 (PO4)3 or Na 1.3 Al 0.3 Ti 1.7 (PO4)3. The electrolyte material has the best ionic conductivity.

[0040] It should be noted that when the titanium source is butyl titanate or titanium dioxide, the molar ratio of the alkali metal salt, the aluminum salt, the titanium source and the phosphoric acid is 1.3-2.6:3-6:34:60.

[0041] When the titanium source is titanium trioxide, the mass ratio of the lithium salt, the aluminum salt, the titanium source and the phosphoric acid is 1.3-2.6:3-6:17:60.

[0042] In order to obtain a precursor material with better crystallinity, the hydrothermal reaction time is 12 to 24 hours. The precursor synthesized within this ratio range has better crystallinity. Beyond this range, the crystallinity of the synthesized material will be too low or too high, which is not conducive to subsequent synthesis and control of oxygen defect concentration.

[0043] In order to effectively adjust the oxygen defect concentration of the electrolyte material, the annealing time is 6 to 12 hours. Within this time range, the oxygen defect concentration inside the electrolyte material can be effectively adjusted. Too short or too long a time will cause the oxygen defect concentration to be too low or too high, which is not conducive to improving the ionic conductivity of the electrolyte material.

[0044] In order to balance the oxygen defect concentration inside the composite electrolyte material and the ionic conductivity of the material, the flow rate of the mixed gas is 20 to 40 sccm, and the mixed gas is an argon-hydrogen mixed gas, and the mass ratio of argon to hydrogen is 19:1 to 3. If the flow rate of the mixed gas is too slow, the gas flow in the tubular furnace cannot be guaranteed to be continuous, and if the flow rate is too fast, unnecessary waste of reaction gas will be caused. When the mass ratio of argon to hydrogen is 19:1 to 3, the hydrogenation treatment is easy to control. If the proportion of hydrogen is too low, the reaction time will be prolonged. If it is too high, the oxygen defect concentration inside the material will be too high, which is not conducive to improving the ionic conductivity of the electrolyte material. Secondly, within this numerical range, the safety of the experimental process can be guaranteed.

[0045] The technical effects of the present invention are described below in conjunction with specific embodiments and comparative examples.

[0046] Example 1

[0047] A method for preparing a composite solid electrolyte comprises the following steps:

[0048] S1, oxygen-deficient O-LATP material was prepared by hydrothermal method combined with heat treatment method: 1.09 g of lithium hydroxide monohydrate (LiOH·H2O) was weighed and dissolved in 20 mL of deionized water to form solution A, 20 mL of ethanol was measured and placed in the inner tank of the hydrothermal kettle, and 2.25 g of aluminum nitrate (Al(NO3)3·9H2O), 11.57 g of butyl titanate (C 16 H 36 O4Ti, TBT) to form B solution. After the two solutions are completely dissolved, A solution is quickly dripped into B solution. 5.88g phosphoric acid (H3PO4) is added to the mixed solution of A and B, and stirred for 2h. Finally, the hydrothermal autoclave containing the sample is placed in a blast drying oven and hydrothermally reacted at 180℃ for 12h. After the sample is cooled, the sample is dried in a blast drying oven at 80℃ for 12h, and then ground for 30min. Then, the precursor powder is placed in a tubular furnace and heated at 5℃min in an argon and hydrogen mixed atmosphere with a mass ratio of 19:1 and a flow rate of 30sccm. -1 The temperature was raised to 700 °C at a rate of 2.5 °C and annealed for 6 h to obtain an oxygen-deficient LATP material, named O-LATP-700.

[0049] S2, 0.09 g of PAN was completely dissolved in 10 mL of N-methylpyrrolidone (NMP) to obtain a yellow transparent solution, and then 0.01 g of O-LATP-700 inorganic solid electrolyte was added. The mixture was magnetically stirred for 24 h to form a uniform mixture, which was spread on a clean mold and naturally cast into a film to obtain a composite solid electrolyte.

[0050] Example 2

[0051] A method for preparing a composite solid electrolyte comprises the following steps:

[0052] S1, oxygen-deficient O-LATP material was prepared by hydrothermal method combined with heat treatment method: 1.09 g of lithium hydroxide monohydrate (LiOH·H2O) was weighed and dissolved in 20 mL of deionized water to form solution A, 20 mL of ethanol was measured and placed in the inner tank of the hydrothermal kettle, and 2.25 g of aluminum nitrate (Al(NO3)3·9H2O), 11.57 g of butyl titanate (C 16 H 36 O4Ti, TBT) to form B solution. After the two solutions are completely dissolved, A solution is quickly dripped into B solution. 5.88g phosphoric acid (H3PO4) is added to the mixed solution of A and B, and stirred for 2h. Finally, the hydrothermal autoclave containing the sample is placed in a blast drying oven and hydrothermally reacted at 180℃ for 12h. After the sample is cooled, the sample is dried in a blast drying oven at 80℃ for 12h, and then ground for 30min. Then, the precursor powder is placed in a tubular furnace and heated at 5℃min in an argon and hydrogen mixed atmosphere with a mass ratio of 19:1 and a flow rate of 30sccm. -1 The temperature was raised to 800 °C at a rate of 1.5 °C and annealed for 6 h to obtain an oxygen-deficient LATP material, named O-LATP-800.

[0053] S2, 0.09 g of PAN was completely dissolved in 10 mL of N-methylpyrrolidone (NMP) to obtain a yellow transparent solution, and then 0.01 g of O-LATP-700 inorganic solid electrolyte was added. The mixture was magnetically stirred for 24 h to form a uniform mixture, which was spread on a clean mold and naturally cast into a film to obtain a composite solid electrolyte.

[0054] Example 3

[0055] A method for preparing a composite solid electrolyte comprises the following steps:

[0056] S1, oxygen-deficient O-LATP material was prepared by hydrothermal method combined with heat treatment method: 1.09 g of lithium hydroxide monohydrate (LiOH·H2O) was weighed and dissolved in 20 mL of deionized water to form solution A, 20 mL of ethanol was measured and placed in the inner tank of the hydrothermal kettle, and 2.25 g of aluminum nitrate (Al(NO3)3·9H2O), 11.57 g of butyl titanate (C 16 H 36O4Ti, TBT) to form B solution. After the two solutions are completely dissolved, A solution is quickly dripped into B solution. 5.88g phosphoric acid (H3PO4) is added to the mixed solution of A and B, and stirred for 2h. Finally, the hydrothermal autoclave containing the sample is placed in a blast drying oven and hydrothermally reacted at 180℃ for 12h. After the sample is cooled, the sample is dried in a blast drying oven at 80℃ for 12h, and then ground for 30min. Then, the precursor powder is placed in a tubular furnace and heated at 5℃min in an argon and hydrogen mixed atmosphere with a mass ratio of 19:1 and a flow rate of 30sccm. -1 The temperature was raised to 900 °C at a rate of 1.5 °C and annealed for 6 h to obtain an oxygen-deficient LATP material, named O-LATP-900.

[0057] S2, 0.09 g of PAN was completely dissolved in 10 mL of N-methylpyrrolidone (NMP) to obtain a yellow transparent solution, and then 0.01 g of O-LATP-700 inorganic solid electrolyte was added. The mixture was magnetically stirred for 24 h to form a uniform mixture, which was spread on a clean mold and naturally cast into a film to obtain a composite solid electrolyte.

[0058] The preparation methods of the composite solid electrolytes of Examples 1 to 3 are described as follows:

[0059] After hydrothermal reaction, aluminum ion-doped oxygen-deficient precursor LiTiOPO was obtained. 4-y ; The reaction process is: LiOH·H2O+C 16 H 36 O4Ti→LiTiOPO 4-y (Aluminum ion doped oxygen defect precursor), wherein butyl titanate is hydrolyzed to obtain water and titanium dioxide, which are then reacted with lithium hydroxide to obtain aluminum ion doped oxygen defect precursor LiTiOPO 4-y , aluminum ions are doped into LiTiOPO 4-y No phase change is induced inside the material.

[0060] Reducing gas and LiTiOPO 4-y The reaction causes some of the tetravalent titanium ions to be converted into trivalent titanium ions, which further induces oxygen defects in the material. The aluminum ion-doped oxygen-deficient precursor LiTiOPO 4-y When calcined at high temperature of 700-900℃, a phase transformation occurs to generate oxygen-deficient Li 1.3 Al 0.3 Ti 1.7 (PO4)3.

[0061] Polyacrylonitrile and oxygen-deficient aluminum titanium phosphate alkali metal materials were inorganic-organic composited to obtain a composite solid electrolyte LATP-PAN. The introduction of oxygen vacancies (V··O) into inorganic materials affects the physical properties of ceramics, which can enhance the chemical interaction between inorganic electrolytes and polymers. Oxygen vacancies can produce a synergistic effect between inorganic electrolytes and polymers, which can promote the Li + Ion transport improves the ionic conductivity of the system. In the -C=N bond of the PAN molecular chain, the lone pair of electrons is located in the N atomic orbital, which is conducive to the formation of Li + coordinated electron donor-acceptor complexes, thereby facilitating Li + transfer and migration.

[0062] The composite solid electrolyte prepared in the above Examples 1 to 3 was immersed in an electrolyte for 10 min (the electrolyte was a mixture of 1 mol L-1 LiPF6 + ethylene carbonate (EC+) and dimethyl carbonate (DMC), and the volume ratio of EC:DMC was 1:1). Then, the composite solid electrolyte, the positive electrode LiFePO4 / C, and the negative electrode metal lithium were used to form an all-solid-state battery, and the cycle and rate performance tests were carried out at a voltage range of 2-4.5V / 2.5-4.2V and a current density of 0.1C-0.5C.

[0063] In order to further illustrate the technical effect of the present invention, the present invention is also provided with a comparative example, as follows:

[0064] Comparative Example 1

[0065] A method for preparing a composite solid electrolyte comprises the following steps:

[0066] The high temperature solid phase method is used to prepare LATP ceramic materials, and the following steps are followed:

[0067] S1, weigh 1.09g of lithium hydroxide monohydrate (LiOH·H2O), dissolve it in 30mL of deionized water, then weigh 2.25g of aluminum nitrate (Al(NO3)3·9H2O), add 2.72g of titanium dioxide (TiO2) and 5.88g of phosphoric acid (H3PO4) to the above solution and stir it magnetically, heat the mixed solution at 80℃ to remove excess water until flocs are formed. Put the obtained flocs in a forced air drying oven and dry them for 6h, grind the dried sample in an agate mortar for 30min, put it into a 30mL crucible, and heat it in a muffle furnace at 5℃min -1 The sample was cooled to obtain LATP precursor powder, which was placed in an agate ball mill tank and wet-milled at a speed of 500 r / min for 12 h, and then dried at 100 °C to obtain LATP powder named LATP-700.

[0068] S2, PAN-LATP-700 solid composite electrolyte was prepared by natural extension method. 0.8g PAN was weighed and completely dissolved in 10mL NMP (N-methylpyrrolidone) to obtain a light yellow transparent solution, and then 0.2g of the prepared NATP solid electrolyte was added. The obtained solution was stirred under magnetic stirring for 24h to form a uniform mixed solution, which was spread on a clean glass plate and naturally cast into a film. After drying at 60°C in a vacuum drying oven for 6h, a solid organic-inorganic composite electrolyte membrane was obtained, and the dried electrolyte membrane was cut into 16mm discs for use.

[0069] The prepared composite solid electrolyte membrane was immersed in the electrolyte for 10 minutes (the electrolyte was 1 mol L-1 LiPF6 + ethylene carbonate (EC+) dimethyl carbonate mixed solution (DMC), and the volume ratio of EC:DMC was 1:1). The composite electrolyte was then combined with the positive electrode LiFePO4 / C and the negative electrode metal lithium to form an all-solid-state battery, and the cycle and rate performance tests were carried out at a voltage range of 2-4.5V / 2.5-4.2V and a current density of 0.1C-0.5C. In order to compare the performance with the commercial Celgard-2400 separator, Li|Celgard-2400|LiFePO4 / C was assembled for performance comparison.

[0070] Comparative Example 2

[0071] A method for preparing a composite solid electrolyte comprises the following steps:

[0072] The oxygen-deficient NATP ceramic material is prepared by a high-temperature solid phase method according to the following steps:

[0073] S1, weigh 2.756g of sodium carbonate (Na2CO3), dissolve it in 30mL of deionized water, then add 2.25g of aluminum nitrate (Al(NO3)3·9H2O), TiO2 (3.1960g) and H3PO4 (5.88g) to the above solution according to the stoichiometric ratio and stir magnetically, heat the mixed solution to 80℃ to remove excess water until flocs are formed. Dry it in a forced air drying oven for 6h, grind the dried precursor in an agate mortar for 30min, put it into a 30mL crucible, and heat it in a muffle furnace at 5℃min -1 The mixture was calcined at 700 °C for 6 h at a heating rate of 1.5 °C. After cooling to room temperature, NATP powder was obtained, which was placed in an agate mortar and ground for 15 min to obtain NTP powder named NTP-3.

[0074] S2, NATP-3-PAN solid composite electrolyte was prepared by natural extension method. 0.8g PAN was weighed and completely dissolved in 10mL NMP (N-methylpyrrolidone) to obtain a light yellow transparent solution, and then 0.2g of the prepared NATP solid electrolyte was added. The obtained solution was stirred under magnetic stirring for 24h to form a uniform mixed solution, which was spread on a clean glass plate and naturally cast into a film. After drying in a vacuum drying oven at 60°C for 6h, a solid organic-inorganic composite electrolyte membrane was obtained, and the dried electrolyte membrane was cut into 16mm discs for standby use.

[0075] The prepared composite solid electrolyte membrane was immersed in the electrolyte for 10 min (the electrolyte was 1 mol L -1 LiPF6+ethylene carbonate (EC+) dimethyl carbonate mixed solution (DMC), EC:DMC volume ratio is 1:1). Then the composite electrolyte is combined with positive electrode LiFePO4 / C and negative electrode metal lithium to form an all-solid-state battery, and the cycle and rate performance tests are carried out at a voltage range of 2-4.5V / 2.5-4.2V and a current density of 0.1C-0.5C.

[0076] Comparative Example 3

[0077] A method for preparing a composite solid electrolyte comprises the following steps:

[0078] The oxygen-deficient NTP ceramic material is prepared by a high-temperature solid phase method according to the following steps:

[0079] S1, weigh 2.12g of sodium carbonate (Na2CO3), dissolve it in 30mL of deionized water, then add 3.1960g of TiO2 and H3PO4 (5.88g) to the above solution according to the stoichiometric ratio and stir it magnetically, heat the mixed solution to 80℃ to remove excess water until flocs are formed. Put it in a forced air drying oven and dry it for 6h, grind the dried precursor in an agate mortar for 30min, put it into a 30mL crucible, and place it in a muffle furnace at 5℃min -1 The mixture was calcined at 700 °C for 6 h at a heating rate of 1.5 ℃. After cooling to room temperature, a white powder was obtained, which was placed in an agate mortar and ground for 15 min to obtain NTP powder.

[0080] S2, prepare PAN-NTP solid composite electrolyte by natural extension method. Weigh 0.8g PAN, completely dissolve it in 10mL NMP (N-methylpyrrolidone), and after obtaining a light yellow transparent solution, add 0.2g of the prepared NTP solid electrolyte, namely NTP-PAN. Stir the obtained solution under magnetic stirring for 24h to form a uniform mixed solution, spread it on a clean glass plate, and naturally cast it into a film. After drying for 6h at 60°C in a vacuum drying oven, a solid organic-inorganic composite electrolyte membrane is obtained, and the dried electrolyte membrane is cut into 16mm discs for standby use.

[0081] The prepared composite solid electrolyte membrane was immersed in the electrolyte for 10 minutes (the electrolyte was 1 mol L-1LiPF6+ethylene carbonate (EC+) dimethyl carbonate mixed solution (DMC), and the volume ratio of EC:DMC was 1:1). Then the composite electrolyte was combined with the positive electrode LiFePO4 / C and the negative electrode metal lithium to form an all-solid-state battery, and the cycle and rate performance tests were carried out at a voltage range of 2-4.5V / 2.5-4.2V and a current density of 0.1C-0.5C.

[0082] The performance of the composite solid electrolytes prepared in the above examples and comparative examples was tested, and the results are as follows: Figures 1 to 10 shown.

[0083] Depend on Figure 1 (a) It can be observed that the XRD diffraction peaks of samples LATP-700, O-LATP-700, O-LATP-800, and O-LATP-900 are consistent with the LiTi2(PO4)3 standard card (PDF#35-0754). The experimental test results show that the synthesized materials are consistent with the LiTi2(PO4)3 phase. Figure 1 (b) is the XRD spectrum of PAN, LATP-700-PAN, O-LATP-700-PAN, O-LATP 800-PAN, O-LATP-900-PAN composite electrolytes. It can be seen from the figure that the solid composite electrolyte presents a composite phase structure of LATP and PAN or O-LATP and PAN. The data analysis results show that LATP and oxygen-deficient LATP are well composited with polyacrylonitrile.

[0084] The prepared samples were tested by Fourier transform infrared spectroscopy, and the obtained FT-IR graph is shown in Figure 2 As shown in the figure, it can be clearly observed that the peaks of O-LATP-700 are 1038, 778, 644 and 575 cm -1 644 and 575cm -1The vibration peak at represents the stretching vibration of OPO. The corresponding peak positions of the stretching vibration of POP and PO of O-LATP-700 appear at 778 cm -1 and 1038cm -1 The corresponding peak positions of the stretching vibration of POP of LATP-700 and PO appear at 758 cm -1 and 1025cm -1 Compared with LATP-700, the POP and PO peaks of oxygen-deficient O-LATP-700 move to higher wavenumbers. The appearance of oxygen deficiency may lead to a decrease in the PO bond length, thus causing a blue shift.

[0085] The samples were subjected to electron paramagnetic resonance tests, such as Figure 3 As shown. Sample LATP-700 does not show any signal peaks, indicating that it does not form oxygen defects. Samples O-LATP-700, O-LATP-800 and O-LATP-900 all show a pair of paramagnetic peaks at g=2.003, indicating that oxygen defects exist in all synthesized samples. The peak of O-LATP-700 is the sharpest, indicating that it has the highest oxygen defect content compared with the other two samples. The results show that increasing the annealing temperature in an argon and hydrogen mixed atmosphere reduces the concentration of oxygen defects.

[0086] Figure 4 The Nyquist curves of LATP-700, O-LATP-700, O-LATP-800, and O-LATP-900 materials show that the impedance distribution of all samples consists of a semicircle in the high-frequency range and a straight line in the low-frequency range. The semicircle at high frequency is due to the inter-grain impedance (R gb ), while the straight line in the low frequency range can indicate that Li + Migration in the electrolyte. Usually represents the intragranular impedance (R g ) is not shown in the figure because Li + The impedance value inside the die can only be tested within a higher frequency range, so the starting point of the semicircle in the figure can be estimated as the impedance inside the die (R g ). The total ionic conductivity of LATP-700, O-LATP-700, O-LATP-800, and O-LATP-900 materials were calculated to be 1.48×10 -4 , 7.55×10 -4 , 5.74×10 -4 , 4.32×10 -4 S cm -1 .

[0087] Figure 5-7The Arrhenius plots of the total conductivity, intracrystalline conductivity and grain boundary conductivity of LATP-700, O-LATP-700, O-LATP-800 and O-LATP-900 materials are further calculated by the formula σ=d / RS (R is the measured AC impedance spectrum and the accurate impedance value obtained by Z-View fitting, d is the thickness of the electrolyte; S is the effective area of ​​the electrolyte) to obtain the corresponding activation energy E a The activation energy E corresponding to the total conductivity of composite solid electrolytes of LATP-700, O-LATP-700, O-LATP-800, and O-LATP-900 samples a The activation energy of total ion conduction is lower than that of LATP-700. The activation energy E corresponding to the intracrystalline conductivity / grain boundary conductivity of composite solid electrolyte samples of LATP-700, O-LATP-700, O-LATP-800, and O-LATP-900 is a They are 0.261eV / 0.274eV, 0.244eV / 0.141eV, 0.221eV / 0.151eV, and 0.187eV / 0.189eV, respectively. Ionic conductivity is related to charge mobility and carrier concentration, while activation energy reflects charge mobility. After high-temperature treatment in an argon and hydrogen mixed atmosphere, the introduction of oxygen defects reduces the activation energy of LATP materials. Li + Ion transport migrates through the PAN polymer matrix, O-LATP inorganic material, and the interface between the polymer matrix and ceramic. As the calcination temperature increases, the activation energy gradually increases, the oxygen defect concentration continues to decrease, and the ionic conductivity decreases. The increase in the concentration of oxygen defects enhances the Coulomb attraction between the composite solid electrolyte and lithium ions, thereby increasing the ion conduction rate.

[0088] Figure 8 25℃, 0.025mA cm -2 The polarization voltage of the symmetrical battery assembled by the solid composite electrolyte changes with time in a long cycle of 1h of periodic constant current charge and discharge under current density. The symmetrical lithium battery composed of the solid composite electrolyte containing the O-LATP-700 sample shows a very stable voltage response of 0.035V during the 400h cycle. In contrast, the symmetrical lithium battery with the solid composite electrolyte containing LATP sample particles exhibits a larger overpotential and poorer stability. The excellent cycling performance and lower polarization indicate that the defective O-LATP-700 effectively improves the interfacial compatibility between lithium metal and the PAN-based solid composite electrolyte, thereby achieving reversible plating and stripping of lithium metal.

[0089] The charge and discharge cycle performance test was carried out at a current density of 0.1C in the voltage range of 2.0-4.5V. Fig. 9 As shown, the initial discharge capacity of Celgard and O-LATP is 179.3 mAh g -1 and 256.2mAh g -1 After 100 cycles, the capacity remained at 171.4 mAh g -1 and 231.8mAh g -1 , the capacity retention rates were 95.6% and 90.5% respectively.

[0090] At a current density of 0.1C and a voltage range of 2.5-4.2V, the rate charge and discharge cycle performance test was performed, such as Fig.10 As shown, the results show that the discharge capacities of the normal assembled battery (Celgarld), the battery assembled with the solid composite electrolyte containing LATP-700-PAN and O-LATP-700-PAN samples, and the battery assembled with the solid composite electrolyte containing NTP-PAN and NATP-3-PAN samples at the initial rate of 0.1C are 183.43, 218.28, 230.56 and 219.41, 189.70, 230.06 mAh g -1 When the cycle number reaches 70 times, the rate capacities are maintained at 191.82, 169.62, 225.79 and 218.07 mAh g -1 The all-solid-state Li|O-LATP-700-PAN|LiFePO4 with O-LATP-700-PAN as the composite electrolyte exhibited the best electrochemical performance.

[0091] In summary, the present invention constructs a composite solid electrolyte composed of PAN, LATP / NATP and lithium salt, which not only successfully introduces oxygen defects, but also effectively regulates the oxygen defect concentration by regulating the aluminum ion doping concentration and the sintering temperature. A reasonable oxygen defect concentration can not only improve the ionic conductivity of the solid composite electrolyte, but also further provide a channel for ion insertion / extraction, thereby improving the electrochemical performance. The present invention adopts organic-inorganic composite to not only improve the ionic conductivity, but also enhance the mechanical strength and broaden the electrochemical window. The introduction of oxygen vacancies (VO) in the inorganic electrolyte not only affects the physical properties of the inorganic electrolyte, but also enhances the chemical interaction between the inorganic electrolyte and the polymer. The synergistic effect of oxygen defects between the inorganic electrolyte and the polymer promotes the transmission of lithium ions, thereby improving the ionic conductivity.

[0092] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a composite solid electrolyte, characterized in that: The following steps are involved: Using alkali metal salt, aluminum salt, titanium source and phosphoric acid as raw materials, hydrothermally reacting at 180-200° C. to obtain an aluminum ion-doped oxygen-deficient precursor, heating the precursor to 700-900° C. in a mixed gas synthesis atmosphere of a reducing atmosphere and a protective atmosphere, annealing, reducing the titanium element in the aluminum ion-doped oxygen-deficient precursor, and obtaining an oxygen-deficient titanium aluminum phosphate alkali metal material; An oxygen-deficient aluminum titanium phosphate alkali metal material is added to a polyacrylonitrile solution, and an inorganic-organic composite is performed by a solution casting method to obtain a composite solid electrolyte.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the alkali metal salt, the aluminum salt, the titanium source and the phosphoric acid is 1.3-2.6:3-6:17-34:

60.

3. The preparation method according to claim 1, characterized in that: The mass ratio of the polyacrylonitrile to the oxygen-deficient aluminum titanium phosphate alkali metal material is 10 to 1:

1.

4. The preparation method according to claim 1, characterized in that: The hydrothermal reaction time is 12 to 24 hours.

5. The preparation method according to claim 1, characterized in that: The annealing time is 6 to 12 hours.

6. The preparation method according to claim 1, characterized in that: The flow rate of the mixed gas is 20-40 sccm, the mixed gas is an argon-hydrogen mixed gas, and the mass ratio of argon to hydrogen is 19:1-3.

7. The preparation method according to claim 1, characterized in that: The heating rate is 5°C / min.

8. The preparation method according to claim 1, characterized in that: The alkali metal salt is lithium hydroxide monohydrate, lithium hydroxide, lithium nitrate, lithium acetate, lithium carbonate, sodium hydroxide, sodium acetate, sodium nitrate or sodium carbonate; the aluminum salt is aluminum nitrate nonahydrate, aluminum oxide, aluminum hydroxide; the titanium source is titanium dioxide, hydrated titanium dioxide, titanium oxide, butyl titanate; the phosphorus source is phosphoric acid or ammonium dihydrogen phosphate.

9. A composite solid electrolyte prepared by the preparation method according to any one of claims 1 to 8.