Polymer electrolyte and in-situ preparation method and application thereof

By using the in-situ polymerization technology of covalent organic frames in polymer electrolytes, the problem of uneven dispersion of covalent organic frames in polymer electrolytes is solved, the transmission efficiency and electrochemical performance of lithium ions are improved, and the preparation process is simplified And reduce costs.

CN118943502APending Publication Date: 2024-11-12HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411286578.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The covalent organic framework is difficult to disperse in large quantities in polymer electrolytes, resulting in problems such as large interface impedance, low ion transport efficiency and poor electrochemical stability.

Method used

By immersing the dispersion of the covalent organic frame with the separator and pre-freeze treatment, freeze drying and reaming to form holes or channels, and then in-situ polymerization is carried out on the surface of the diaphragm after the reaming, using the covalent organic frame Organic acid functional groups catalyze the ring-opening polymerization reaction of cyclolactone to prepare polymer electrolyte.

Benefits of technology

It improves the transmission efficiency and electrochemical performance of lithium ions, reduces the glass transition temperature and crystallinity of the polymer, simplifies the preparation process and reduces the cost, and improves the electrochemical performance of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943502A_ABST
    Figure CN118943502A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of polymer electrolytes, and relates to a polymer electrolyte, and an in-situ preparation method and application thereof. The polymer electrolyte is obtained by ring-opening polymerization of a covalent organic framework on the surface of a diaphragm and internal in-situ catalytic cyclic lactone. The preparation method is realized by catalyzing the ring-opening polymerization reaction of cyclic lactone by virtue of a covalent organic framework, and organic acid salt functional group sites on the covalent organic framework play a role in catalyzing in the ring-opening polymerization reaction of the cyclic lactone so as to promote the ring-opening polymerization reaction of the cyclic lactone. The covalent organic framework is loaded on the diaphragm, and through in-situ polymerization of an electrolyte precursor solution on the diaphragm, the problem that a large amount of the covalent organic framework is difficult to disperse in a polymer electrolyte precursor solution is solved, the electrochemical performance of the polymer electrolyte is improved, and the preparation process is simplified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer electrolytes and relates to a polymer electrolyte, an in-situ preparation method and application thereof. Background Art

[0002] Solid polymer electrolytes have been widely studied by researchers due to their advantages such as easy synthesis, high safety, effective compatibility with large-scale manufacturing processes, good mechanical strength and high toughness. However, polymer-based solid electrolytes exhibit low ion transport efficiency at room temperature. In polymer electrolytes, lithium ions are solvated by polymer chains and transported through continuous exchange of ligands in the solvation shell. The strong solvation of lithium ions by polymer chains, weak lithium salt dissociation ability and high crystallinity of polymers lead to low lithium ion transport efficiency.

[0003] In order to solve these problems, people try to compound polymers with other materials. Complementing and synergizing the advantages of composite materials and polymers is a relatively effective strategy to improve the ion transport efficiency of polymer electrolytes. Establishing Lewis acid-base interactions between fillers and polymer interfaces is an effective method to kinetically reduce the glass transition temperature and crystallinity of polymers. At the same time, the interaction between polymers and fillers can also improve lithium ion transport, mechanical strength and electrochemical stability.

[0004] Covalent organic framework materials are commonly used polymer crystal materials with advantages such as large specific surface area, high porosity, and tunable chemical structure. Various active groups and building blocks on the framework can be effectively fixed on the skeleton, and the high porosity can provide channels for lithium ion transmission. Therefore, blending covalent organic frameworks with polymers is a potential way to construct composite electrolytes. Therefore, in recent years, covalent organic frameworks as electrolyte materials have been widely and deeply studied.

[0005] However, the electrolyte materials prepared by covalent organic framework composite polymers have complex processing methods, low loading capacity, and uneven dispersion, and often need to be prepared and applied by hot pressing and casting. In addition, the obtained composite polymer electrolyte materials often have the following disadvantages: large interface impedance, low ion transfer efficiency, and low electrochemical stability (Angew. Chem. Int. Ed., 2024, https: / / doi.org / 10.1002 / anie.202406511).

[0006] In addition, if the covalent organic framework material prepared by the above method needs to be compounded with a polymer, it needs to be mixed with a lithium salt and then cast into a film in a non-in-situ manner, which has the disadvantages of large interfacial impedance and unsatisfactory chemical properties. If the polymer is formed in situ in the battery, a solvent and an organic acid-base catalyst are required to catalyze the polymerization. The non-ionic transport components in the battery will reduce the electrochemical performance and cycle life of the lithium-ion battery, making it difficult to obtain a high-performance polymer electrolyte (Batteries, 2023, 9(9): 432). Summary of the invention

[0007] In view of the defects of the prior art, the purpose of the present invention is to provide a polymer electrolyte, an in-situ preparation method and application thereof, aiming to solve the technical problems in the prior art that covalent organic frameworks are difficult to disperse in large quantities in polymer electrolytes and are difficult to prepare in situ, resulting in large interfacial impedance and poor electrochemical performance.

[0008] To achieve the above object, the present invention provides an in-situ preparation method of a polymer electrolyte, comprising the following steps:

[0009] (1) infiltrating a membrane with a dispersion of a covalent organic framework to obtain a membrane loaded with the dispersion of the covalent organic framework; and then pre-freezing the membrane loaded with the dispersion of the covalent organic framework, wherein the expansion of ice crystals during the freezing process exerts pressure on the pore walls of the membrane, causing the pore walls to deform or partially damage, thereby expanding the pores inside the membrane;

[0010] (2) freeze-drying the pre-frozen membrane to freeze-sublimate the ice crystals contained therein. After the ice crystals sublimate, the space originally occupied by the ice crystals is vacated to form holes or channels, thereby obtaining a membrane loaded with a covalent organic framework after the holes are expanded;

[0011] (3) transferring the electrolyte precursor solution obtained by uniformly mixing the cyclic lactone and the lithium salt to the surface of the diaphragm loaded with the covalent organic framework after the pore expansion in step (2), and assembling a lithium ion battery containing the diaphragm, wherein the cyclic lactone in the electrolyte precursor solution is in situ polymerized on the surface and pores of the diaphragm loaded with the covalent organic framework to prepare a polymer electrolyte;

[0012] The covalent organic framework is a covalent organic framework containing organic acid salt functional groups; and the dispersion of the covalent organic framework is obtained by dispersing the covalent organic framework containing organic acid salt functional groups in a solvent containing water.

[0013] Preferably, the covalent organic framework containing organic acid salt functional groups contains at least one of lithium sulfonate, lithium carboxylate and lithium trifluoromethylsulfonyl imide, and the covalent organic framework containing organic acid salt functional groups includes TpPa-SO 3Li, TpPa-Double-SO 3 Li, TpPa-COOLi, TpPa-Double-COOLi, TpBDSA-Li or more; the mass percentage of the covalent organic framework containing organic acid salt functional group sites in the dispersion of the covalent organic framework is 3-10%.

[0014] Preferably, the solvent in step (1) contains, in addition to water, one or more of tetrahydrofuran, ethanol and acetone.

[0015] Preferably, the pre-freezing treatment in step (1) is carried out at a temperature of -10 to -20°C for 2 to 3 hours; the freeze-drying in step (2) is carried out at a temperature of -20 to -60°C for 5 to 10 hours, and the vacuum degree is 0.1-10Pa.

[0016] Preferably, the cyclic lactone in step (3) is at least one of valerolactone, caprolactone, lactide, trimethylene carbonate, and 1,4-dioxane-2-one; and the lithium salt includes one or more of lithium perchlorate, lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium nitrate, and lithium iodide.

[0017] Preferably, the in-situ polymerization is specifically: the polymerization reaction is carried out at a temperature of 80 to 100° C. for 24 to 72 hours.

[0018] According to another aspect of the present invention, a polymer electrolyte prepared by the in-situ preparation method is provided.

[0019] According to another aspect of the present invention, a lithium ion battery is provided, comprising the polymer electrolyte.

[0020] The present invention polymerizes the cyclic lactone monomer in the long-range ordered pores or at the surface interface of the covalent organic framework material by in-situ compounding. The present invention utilizes the principle that the volume of ice crystals expands after water is frozen to pre-freeze and freeze-dry the solvent in the covalent organic framework dispersion, so that the pore size inside the diaphragm is enlarged, so that the diaphragm can be loaded with a large amount of covalent organic framework on the surface and inside of the diaphragm without adding any adhesive. In the interior and surface interface of the diaphragm loaded with the covalent organic framework material, the electrolyte monomer and the covalent organic framework material are more efficiently and uniformly in-situ compounded to achieve the polymerization of the monomer in the pores of the covalent organic framework porous material. The polymerization of the monomer in the pores of the covalent organic framework has a certain confining effect on the anion transport of the lithium salt, and the anions fixed on the framework greatly increase the lithium ion migration number of the polymer electrolyte. The unique single ion structure increases the content of active lithium ions in the electrolyte, increases the carrier concentration, and improves the ionic conductivity. The polymer polymerized on the surface greatly reduces the glass transition temperature and crystallinity of the polymer under the plasticization effect of the covalent organic framework material. At the same time, this in-situ polymerization preparation method effectively improves the interface contact between the electrolyte and the electrode, thereby improving the electrochemical performance of the electrolyte. The schematic diagram of the covalent organic framework and the polymer in the polymer electrolyte of the present invention synergistically transferring lithium ions to improve the electrochemical performance is shown in the figure Figure 1 shown.

[0021] The present invention is achieved by catalyzing the ring-opening polymerization reaction of cyclic lactone by a covalent organic framework, wherein the organic acid salt functional group sites on the covalent organic framework catalyze the ring-opening polymerization reaction of the cyclic lactone, and these organic acid salt functional group sites activate the hydroxyl groups of trace water in the electrolyte to cause it to initiate the ring-opening polymerization reaction of the cyclic lactone. In the system, the covalent organic framework is loaded on the diaphragm by a freeze-drying pore expansion method, and the in-situ polymerization technology of dripping an electrolyte precursor liquid on the diaphragm is integrated to solve the problem that the covalent organic framework is difficult to disperse in large quantities in the polymer electrolyte. The strategy of in-situ composite of the covalent organic framework and the polymer electrolyte is adopted to improve the electrochemical performance of the polymer electrolyte, simplify the preparation process and reduce the cost, and provide a method for efficiently preparing a lithium ion battery of a covalent organic framework material in-situ composite polymer electrolyte.

[0022] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:

[0023] (1) The present invention disperses the covalent organic framework in a solvent containing water, and the mass fraction of the covalent organic framework can be controlled to adjust the loading amount on the diaphragm. Compared with the coating method and the hot pressing method, the present invention has a simpler operation process and flow, can shorten the cycle of traditional electrolyte preparation, and the catalysis of the covalent organic framework material can avoid the introduction of additional lactone ring-opening polymerization catalysts and solvents, and avoids the introduction of ion-conducting components in the non-electrolyte and components that affect battery performance.

[0024] (2) The present invention provides a method for in-situ construction of a covalent organic framework and polymer electrolyte composite material by heterogeneous ring-opening polymerization of cyclic lactone monomers of a covalent organic framework. The method disperses the covalent organic framework material well and increases its loading in the electrolyte. The covalent organic framework material can catalyze the ring-opening polymerization of lactone and the introduction of the covalent organic framework material into the polymer electrolyte greatly improves the electrochemical performance of the polymer electrolyte.

[0025] (3) The present invention provides a method for preparing a covalent organic framework material composite polymer electrolyte by in-situ composite polymer with a covalent organic framework material. The reaction system does not need to add additional catalysts, polar solvents or other compounds. The electrolyte precursor is obtained by mixing the cyclic lactone monomer and the lithium salt, and then the electrolyte precursor is added dropwise to the diaphragm loaded with the covalent organic framework to catalyze the ring-opening polymerization reaction of the cyclic lactone monomer. On the one hand, the reaction system relies on the covalent organic material loaded on the diaphragm as a catalyst, and does not require an external solvent, which can avoid the use of irrelevant parts of the polymer electrolyte related to ion conduction, and avoid the shortcomings of complex post-processing, high cost, and easy volatility of the solvent caused by catalysts and organic solvents. On the other hand, compared with other organic acid-base catalysts that damage the electrochemical performance of the battery, the covalent organic framework greatly improves the ionic conductivity and ion migration number of the polymer electrolyte after in-situ composite with the polymer electrolyte, thereby improving the electrochemical performance of the lithium-ion battery and reducing the cost.

[0026] (4) The covalent organic framework structure, loading amount and type of cyclic lactone monomer used in the present invention are adjustable, and the electrochemical properties of the electrolyte can be regulated according to actual needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the covalent organic framework and the polymer in the polymer electrolyte of the present invention synergistically transferring lithium ions to improve electrochemical performance.

[0028] Figure 2 This is the nuclear magnetic resonance spectrum of the copolymer of caprolactone and trimethylene carbonate catalyzed by the covalent organic framework with lithium carboxylate structure in Example 1.

[0029] Figure 3The conductivity of the polymer electrolytes prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 varies with temperature.

[0030] Figure 4 The electrochemical stability window bar graphs of the polymer electrolytes prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 are shown.

[0031] Figure 5 This is a bar graph of the lithium ion migration numbers of the polymer electrolytes prepared in Example 1 and Comparative Examples 1, 2, 3, and 4.

[0032] Figure 6 The voltage-time diagram of the constant current charge-discharge cycle of the lithium-lithium symmetric battery assembled with the polymer electrolyte prepared in Example 1 and Comparative Examples 1, 2, 3 and 4.

[0033] Figure 7 The discharge capacity, coulomb efficiency and cycle number of the full battery (lithium iron phosphate negative electrode) composed of the polymer electrolyte prepared in Example 1 and Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 are shown in FIG. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0035] The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0036] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0037] In the present invention, unless otherwise specified and / or described, all numerical values ​​involving the amounts of components are "parts by weight" from beginning to end. The process parameters in the following examples without specifying specific conditions are usually based on conventional conditions.

[0038] The present invention discloses an in-situ preparation method of a polymer electrolyte, comprising the following steps:

[0039] (1) infiltrating a membrane with a dispersion of a covalent organic framework to obtain a membrane loaded with the dispersion of the covalent organic framework; and then pre-freezing the membrane loaded with the dispersion of the covalent organic framework, wherein the expansion of ice crystals during the freezing process exerts pressure on the pore walls of the membrane, causing the pore walls to deform or partially damage, thereby expanding the pores inside the membrane;

[0040] (2) freeze-drying the pre-frozen membrane to freeze-sublimate the ice crystals contained therein. After the ice crystals sublimate, the space originally occupied by the ice crystals is vacated to form holes or channels, thereby obtaining a membrane loaded with a covalent organic framework after the holes are expanded;

[0041] (3) transferring the electrolyte precursor solution obtained by uniformly mixing the cyclic lactone and the lithium salt to the surface of the diaphragm loaded with the covalent organic framework after the pore expansion in step (2), and assembling a lithium ion battery containing the diaphragm, wherein the cyclic lactone in the electrolyte precursor solution is in situ polymerized on the surface and pores of the diaphragm loaded with the covalent organic framework to prepare a polymer electrolyte;

[0042] The covalent organic framework is a covalent organic framework containing organic acid salt functional groups; and the dispersion of the covalent organic framework is obtained by dispersing the covalent organic framework containing organic acid salt functional groups in a solvent containing water.

[0043] The present invention mentions that the membrane is infiltrated with the dispersion of the covalent organic framework, and the membrane is infiltrated with water. There are many ways to achieve "infiltration", such as soaking, dipping, dripping, etc.

[0044] In some embodiments, the covalent organic framework containing organic acid salt functional groups contains at least one of lithium sulfonate, lithium carboxylate and lithium trifluoromethylsulfonyl imide, and the covalent organic framework containing organic acid salt functional groups includes TpPa-SO 3 Li, TpPa-Double-SO 3 Li, TpPa-COOLi, TpPa-Double-COOLi, TpBDSA-Li or more; the mass percentage of the covalent organic framework containing organic acid salt functional group sites in the dispersion of the covalent organic framework is 3-10%.

[0045] Taking TpPa-COOLi as an example, its chemical structure diagram is shown in formula (1):

[0046]

[0047] In some embodiments, the solvent in step (1) contains, in addition to water, one or more of tetrahydrofuran, ethanol, and acetone.

[0048] In some embodiments, the pre-freezing treatment in step (1) is performed at a temperature of -10 to -20°C for 2 to 3 hours; the freeze-drying in step (2) is performed at a temperature of -20 to -60°C for 5 to 10 hours, and the vacuum degree is 0.1 to 10 Pa. During the freezing pre-treatment in step (1), the expansion of the ice crystals exerts pressure on the pore walls of the diaphragm, causing the pore walls to deform or partially damage, thereby expanding the pores inside the diaphragm; during the freeze-drying process in step (2), the ice crystals contained in the pores inside the diaphragm are frozen and sublimated. After the ice crystals sublimate, the space originally occupied by the ice crystals becomes empty, forming holes or channels, thereby obtaining an expanded diaphragm.

[0049] In some embodiments, the step (1) of allowing the dispersion of the covalent organic framework to infiltrate the membrane comprises soaking the membrane in the dispersion of the covalent organic framework for 5 to 10 minutes, so that the dispersion of the covalent organic framework infiltrates the membrane; and the loading amount of the covalent organic framework in the membrane loaded with the covalent organic framework after the pore expansion is 0.5 to 2.5 mg / cm 2 ; The diaphragm is one of a cellulose diaphragm, a glass fiber diaphragm, and a polyethylene terephthalate diaphragm.

[0050] In some embodiments, the cyclic lactone in step (3) is at least one of valerolactone, caprolactone, lactide, trimethylene carbonate, and 1,4-dioxane-2-one; and the lithium salt includes one or more of lithium perchlorate, lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium nitrate, and lithium iodide.

[0051] In some embodiments, the mass fraction of the lithium salt in the electrolyte precursor solution is 2% to 40%.

[0052] In some embodiments, the cyclic lactone and the lithium salt are mixed and stirred at 20-60° C. for 5-25 minutes to obtain an electrolyte precursor solution.

[0053] In some embodiments, the in-situ polymerization is specifically: the polymerization reaction is carried out at a temperature of 80 to 100° C. for 24 to 72 hours.

[0054] In some embodiments, the step (3) of assembling a lithium-ion battery containing the diaphragm means stacking the steel sheet, the lithium sheet, and the diaphragm in sequence, dripping the electrolyte precursor solution, and then sequentially covering the positive electrode, the steel sheet, and the shrapnel, and packaging the battery to perform in-situ polymerization in the step (3). In some embodiments, the positive electrode can be made of lithium iron phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide (LiNi x Coy Mn 1-x-y O 2 )Ternary positive electrode material or nickel cobalt aluminum oxide ternary positive electrode material, the negative electrode uses metallic lithium.

[0055] The cyclic lactone in the electrolyte precursor solution of the present invention is in-situ polymerized in the pores of the diaphragm loaded with the covalent organic framework, and the organic acid salt functional group contained in the covalent organic framework acts as a catalyst to catalyze the ring-opening polymerization reaction of the cyclic lactone to prepare a polymer electrolyte. The in-situ polymerization of the cyclic lactone monomer can be the homopolymerization of one cyclic lactone or the copolymerization of multiple cyclic lactone monomers.

[0056] The polymer electrolyte prepared by the in-situ preparation method of the present invention can be used as an electrolyte for lithium ion batteries.

[0057] The invention discloses a method for preparing a covalent organic framework material composite polymer electrolyte by in-situ composite polymer of a covalent organic framework material. The method is realized by catalyzing the ring-opening polymerization reaction of a cyclic lactone by a covalent organic framework, wherein the organic acid salt functional group sites on the covalent organic framework play a catalytic role in the ring-opening polymerization reaction of the cyclic lactone, and these organic acid salt functional group sites activate the hydroxyl groups of trace water in the electrolyte to induce the ring-opening polymerization reaction of the cyclic lactone. In the system, the covalent organic framework is loaded on a diaphragm, and the problem that the covalent organic framework is difficult to disperse in a large amount in a polymer electrolyte precursor solution is solved by an in-situ polymerization technology of dripping an electrolyte precursor solution on the diaphragm. The strategy of in-situ composite of a covalent organic framework and a polymer electrolyte is adopted to improve the electrochemical performance of the polymer electrolyte, simplify the preparation process and reduce the cost, and provide a method for efficiently preparing a lithium ion battery of an in-situ composite polymer electrolyte of a covalent organic framework material.

[0058] According to the method of the present invention, an all-solid-state covalent organic framework polymer composite electrolyte catalyzed by the covalent organic framework for the ring-opening polymerization of cyclic lactone can be prepared. In a preferred embodiment, the electrochemical properties of the electrolyte are regulated by regulating the loading amount of the covalent organic framework material on the diaphragm, and the in-situ ring-opening polymerization of cyclic lactone is carried out to construct a polymer electrolyte, and the reaction time is 48 hours. The composite polymer electrolyte prepared according to the preparation method of the present invention is experimentally proved to be used as an electrolyte for lithium-ion batteries, and has a high ionic conductivity, and the conductivity can reach 5.6×10 at 60°C. -5 S cm -2 , the lithium ion migration number can reach 0.85, and the electrochemical stability window is 5.28 V. It has the potential to be used to match high-voltage positive electrode materials. The higher conductivity and migration number accelerate the transmission efficiency of ions in the electrolyte and greatly reduce the concentration polarization of lithium ions in the electrolyte.

[0059] The following are examples:

[0060] Example 1

[0061] A method for preparing a polymer electrolyte by in-situ catalytic ring-opening polymerization of a covalent organic framework, the preparation method of which is as follows:

[0062] (1) 0.15 g of the covalent organic framework material TPPa-COOLi containing lithium carboxylate functional groups was ultrasonically dispersed in 5 ml of deionized water for 30 min to obtain a uniform dispersion of the covalent organic framework. A cellulose membrane (commercial TF4030, with a diameter of 16 mm) was immersed in the dispersion for 5 min and then placed in a low-temperature refrigerator for pre-freezing at a temperature of -10 °C for 2 h. After pre-freezing, the membrane was freeze-dried in a freeze dryer at a temperature of -55 °C for 8 hours and a vacuum degree of 0.1 Pa.

[0063] (2) 0.2 g of caprolactone monomer, 0.045 g of trimethylene carbonate, 0.050 g of lithium bis(trifluoromethanesulfonyl)imide, and 0.005 g of lithium nitrate were mixed and stirred for 25 min at a stirring temperature of 60° C. to obtain an electrolyte precursor solution.

[0064] (3) Drop the electrolyte precursor of step (2) on the diaphragm of step (1), stack the steel sheet, lithium sheet and the diaphragm in sequence, drop the electrolyte precursor of step (2), cover the positive electrode, steel sheet and shrapnel in sequence, and package the battery, perform in-situ polymerization, so that the monomer is in-situ polymerized in the diaphragm and the pores of the covalent organic framework material, the polymerization temperature is 100°C, the polymerization time is 48h, and the diaphragm containing the polymer and the covalent organic framework is the polymer electrolyte prepared in situ. It has a high ionic conductivity, and the conductivity can reach 3.9×10 at 60°C. -5 S cm -2 , the lithium ion migration number is 0.85. The high conductivity and migration number are conducive to the conduction of ions in the electrolyte and greatly reduce the concentration polarization of lithium ions in the electrolyte.

[0065] Figure 2 This is the nuclear magnetic resonance spectrum of the copolymer of caprolactone and trimethylene carbonate catalyzed by the covalent organic framework with a lithium carboxylate structure in Example 1. It can be seen that the polymerization conversion rate of caprolactone monomer and trimethylene carbonate monomer under the catalysis of the covalent organic framework material is close to 100%.

[0066] Example 2

[0067] A method for preparing a polymer electrolyte by in-situ catalytic ring-opening polymerization of a covalent organic framework, the preparation method of which is as follows:

[0068] (1) 0.15 g of the covalent organic framework material TPPa-Double-COOLi containing lithium carboxylate functional groups was ultrasonically dispersed in a mixed solvent of 5 ml of deionized water and ethanol for 30 min to obtain a uniform dispersion of the covalent organic framework. A cellulose membrane (commercial TF4030, with a diameter of 16 mm) was immersed in the dispersion for 5 min and then placed in a low-temperature refrigerator for pre-freezing at a temperature of -10°C for 2 h. After pre-freezing, the membrane was freeze-dried and the freeze dryer temperature was set to -40°C for 10 hours with a vacuum degree set to 10 Pa.

[0069] (2) 0.2 g of caprolactone monomer, 0.037 g of lithium perchlorate and 0.005 g of lithium iodide were mixed and stirred for 25 min at a temperature of 60° C. to obtain an electrolyte precursor solution.

[0070] (3) Drop the electrolyte precursor of step (2) on the diaphragm of step (1), stack the steel sheet, lithium sheet and the diaphragm in sequence, drop the electrolyte precursor of step (2), cover the positive electrode, steel sheet and shrapnel in sequence, and package the battery, perform in-situ polymerization, so that the monomer is in-situ polymerized in the diaphragm and the pores of the covalent organic framework material, the polymerization temperature is 80°C and the polymerization time is 72h, and the diaphragm containing the polymer and the covalent organic framework is the polymer electrolyte prepared in-situ. It has a high ionic conductivity, and the conductivity can reach 8.2×10 at 60°C. -5 S cm -2 , the lithium ion migration number is 0.82. The high conductivity and migration number are beneficial to the conduction of ions in the electrolyte and greatly reduce the concentration polarization of lithium ions in the electrolyte.

[0071] Example 3

[0072] A method for preparing a polymer electrolyte by in-situ catalytic ring-opening polymerization of a covalent organic framework, the preparation method of which is as follows:

[0073] (1) 0.15 g of the covalent organic framework material TPPa-SO containing lithium sulfonate functional groups was added. 3 Li was ultrasonically dispersed in 5 ml of deionized water for 30 minutes to obtain a uniform dispersion of the covalent organic framework. The glass fiber membrane was immersed in the dispersion for 5 minutes and then placed in a low-temperature refrigerator for pre-freezing at -20°C for 2 hours. After the pre-freezing was completed, the membrane was freeze-dried and the freeze dryer temperature was set to -60°C for 5 hours, and the vacuum degree was set to 0.1 Pa.

[0074] (2) 0.2 g of trimethylene carbonate, 0.047 g of lithium bis(trifluoromethanesulfonyl)imide and 0.005 g of lithium iodide were mixed and stirred for 10 min at a temperature of 20° C. to obtain an electrolyte precursor solution.

[0075] (3) Drop the electrolyte precursor of step (2) on the diaphragm of step (1), stack the steel sheet, lithium sheet and the diaphragm in sequence, drop the electrolyte precursor of step (2), and then cover the positive electrode, steel sheet and shrapnel in sequence, and package the battery, and perform in-situ polymerization, so that the monomer is in-situ polymerized in the diaphragm and the pores of the covalent organic framework material, the polymerization temperature is 80°C and the polymerization time is 48h, and the diaphragm containing the polymer and the covalent organic framework is the polymer electrolyte prepared in situ. It has a high ionic conductivity, and the conductivity can reach 1.25×10 at 60°C. -5 S cm -2 , the lithium ion migration number is 0.75.

[0076] Example 4

[0077] A method for preparing a polymer electrolyte by in-situ catalytic ring-opening polymerization of a covalent organic framework, the preparation method of which is as follows:

[0078] (1) 0.15 g of the covalent organic framework material TPPa-Double-SO containing lithium sulfonate functional groups was added 3 Li was ultrasonically dispersed in a mixed solvent of 5 ml of deionized water and tetrahydrofuran for 30 minutes to obtain a uniform dispersion of the covalent organic framework. The glass fiber membrane was immersed in the dispersion for 5 minutes and then placed in a low-temperature refrigerator for pre-freezing treatment at a temperature of -10°C and a freezing time of 3 hours. After the pre-freezing was completed, the membrane was freeze-dried and the freeze dryer temperature was set to -20°C for 10 hours, and the vacuum degree was set to 10Pa.

[0079] (2) 0.2 g of 1,4-dioxane-2-one and 0.1 g of lithium perchlorate were mixed and stirred for 10 min at a temperature of 60° C. to obtain an electrolyte precursor solution.

[0080] (3) Drop the electrolyte precursor of step (2) on the diaphragm of step (1), stack the steel sheet, lithium sheet and the diaphragm in sequence, drop the electrolyte precursor of step (2), and then cover the positive electrode, steel sheet and shrapnel in sequence, and package the battery, and perform in-situ polymerization, so that the monomer is in-situ polymerized in the diaphragm and the pores of the covalent organic framework material, the polymerization temperature is 100°C and the polymerization time is 24h. The diaphragm containing the polymer and the covalent organic framework is the polymer electrolyte prepared in situ. It has a high ionic conductivity, and the conductivity can reach 3×10 at 60°C. -6 S cm -2 , the lithium ion migration number is 0.52.

[0081] Example 5

[0082] A method for preparing a polymer electrolyte by in-situ catalytic ring-opening polymerization of a covalent organic framework, the preparation method of which is as follows:

[0083] (1) 0.15 g of a covalent organic framework material Tp-BDSA-Li containing trifluoromethylsulfonyl imide lithium functional groups was ultrasonically dispersed in a mixed solvent of 5 ml of deionized water and acetone for 30 min to obtain a uniform dispersion of the covalent organic framework. A polyethylene terephthalate membrane was immersed in the dispersion for 5 min and then placed in a low-temperature refrigerator for pre-freezing at a temperature of -20°C for 2 h. After the pre-freezing was completed, the membrane was freeze-dried and the freeze dryer temperature was set to -45°C for 10 hours, and the vacuum degree was set to 10 Pa.

[0084] (2) 0.2 g of a lactide derivative, 0.15 g of caprolactone and 0.1 g of lithium bis(trifluoromethanesulfonyl)imide were mixed and stirred for 25 min at a temperature of 80° C. to obtain an electrolyte precursor solution.

[0085] (3) Dropping the electrolyte precursor of step (2) on the diaphragm of step (1), that is, after stacking the steel sheet, the lithium sheet, and the diaphragm in sequence, dripping the electrolyte precursor of step (2), and then covering the positive electrode, the steel sheet, and the spring sheet in sequence, and encapsulating the battery, and performing in-situ polymerization, so that the monomer is in-situ polymerized in the diaphragm and the pores of the covalent organic framework material, the polymerization temperature is 100°C and the polymerization time is 24h. The diaphragm containing the polymer and the covalent organic framework is the polymer electrolyte prepared in situ. It has a high ionic conductivity, and the conductivity can reach 8×10 at 60°C. -6 S cm -2 , the lithium ion migration number is 0.88.

[0086] Example 6

[0087] A method for preparing a polymer electrolyte by in-situ catalytic ring-opening polymerization of a covalent organic framework, the preparation method of which is as follows:

[0088] (1) 50 g of the covalent organic framework material Tp-BDSA-Li containing lithium carboxylate functional groups was ultrasonically dispersed in 150 ml of deionized water for 30 min to obtain a uniform dispersion of the covalent organic framework. The cellulose membrane was immersed in the dispersion for 5 min and then placed in a low-temperature refrigerator for pre-freezing at a temperature of -20°C for 2 h. After the pre-freezing was completed, the membrane was freeze-dried and the freeze dryer temperature was set to -60°C for 10 hours. The vacuum degree was set to 0.1 Pa.

[0089] (2) 20 g of caprolactone, 4.5 g of trimethylene carbonate, 5 g of lithium bis(trifluoromethanesulfonyl)imide and 0.5 g of lithium nitrate were mixed and stirred for 25 min at a temperature of 60° C. to obtain an electrolyte precursor solution.

[0090] (3) Drop the electrolyte precursor of step (2) on the diaphragm of step (1), stack the steel sheet, lithium sheet and the diaphragm in sequence, drop the electrolyte precursor of step (2), and then cover the positive electrode, steel sheet and shrapnel in sequence, and package the battery, and perform in-situ polymerization, so that the monomer is in-situ polymerized in the diaphragm and the pores of the covalent organic framework material, the polymerization temperature is 100°C and the polymerization time is 48h. The diaphragm containing the polymer and the covalent organic framework is the polymer electrolyte prepared in situ. It has a high ionic conductivity, and the conductivity can reach 2.1×10 at 60°C. -5 S cm -2 , the lithium ion migration number is 0.79.

[0091] Comparative Example 1

[0092] The difference between Comparative Example 1 and Example 1 is that ethanesulfonic acid is directly used to catalyze the reaction of caprolactone and trimethylene carbonate, without using the covalent organic framework supported on the diaphragm for catalysis. Specifically:

[0093] (1) 0.2 g of caprolactone monomer, 0.045 g of trimethylene carbonate, 0.050 g of lithium bis(trifluoromethanesulfonyl)imide, 0.005 g of lithium nitrate, and 20 μL of ethanesulfonic acid were mixed and stirred for 5 min at a stirring temperature of 60° C. to obtain an electrolyte precursor solution.

[0094] (2) The electrolyte of step (1) is directly dripped onto the cellulose diaphragm, and the steel sheet, lithium sheet, and diaphragm are stacked in sequence, and then the electrolyte precursor solution of step (1) is dripped into it, and then the positive electrode, steel sheet, and shrapnel are sequentially covered, and the battery is packaged and in-situ polymerization is performed, and the polymerization temperature is 100° C. and the polymerization time is 48 h.

[0095] Figure 2 This is a graph showing the change in conductivity of the polymer electrolyte prepared in Comparative Example 1 with temperature. Figure 3 This is the electrochemical stability window diagram of the polymer electrolyte prepared in Comparative Example 1, and its oxidation voltage is 5.06V. Figure 4 Graph showing the lithium ion transference number of the polymer electrolyte prepared in Comparative Example 1. The lithium ion transference number is 0.66, which is much lower than the oxidation voltage and lithium ion transference number of Example 1.

[0096] Other conditions remain unchanged. Ethylenesulfonic acid is also used to catalyze the ring-opening polymerization of cyclic lactone. The difference is that ethanesulfonic acid is not modified on the co-framework organic framework. The experiment found that the conductivity of the prepared polymer electrolyte is 5.6×10 - 6 S cm -2The lithium ion migration number is 0.66. The introduction of the acid catalyst may make the interface between the polymer electrolyte and the lithium negative electrode unstable, because ethanesulfonic acid reacts with the lithium negative electrode to produce gas and an unstable electrode electrolyte interface, resulting in rapid cycle decay of the full battery, and it is impossible to obtain high electrochemical performance. The assembled lithium-ion battery cannot be stably charged and discharged.

[0097] Comparative Example 2

[0098] Comparative Example 2 is the same as Example 1 in other conditions, except that the long-range ordered covalent organic framework material is replaced by a random polymer covalent organic framework material.

[0099] The experiment found that when other conditions remain unchanged, the electrochemical performance is significantly lower than that of Example 1, probably because the random covalent organic framework material cannot provide a good channel for the transmission of lithium ions. The conductivity is only 3.5×10 -6 S cm -2 , the lithium ion migration number is only 0.72.

[0100] Comparative Example 3

[0101] Comparative Example 3 is the same as Example 1 in other conditions, except that lithium benzoate is blended with a covalent organic framework material that does not contain any organic acid salt, and lithium benzoate is not anchored on the covalent organic framework material. Probably because the benzoate anions and lithium ions provide additional ion sources, the experiment found that its conductivity is slightly higher than that of Example 1, but the migration number is lower. The conductivity measured at 60°C is 7.9×10 -5 S cm -2 , the lithium ion migration number is only 0.58. In lithium symmetric batteries, during long lithium deposition cycles, lithium benzoate, as a non-electrolyte component, easily forms a more unstable and more resistive electrode-electrolyte interface with the lithium sheet negative electrode, which is not conducive to the long cycle performance of the battery.

[0102] Comparative Example 4

[0103] The difference between Comparative Example 4 and Example 1 is that the pores of the diaphragm are not expanded. Instead, the diaphragm is immersed in the dispersion and then the solvent is removed by other means. The pores are not expanded by freeze drying, and the other steps are exactly the same.

[0104] (1) 0.15 g of the covalent organic framework material TPPa-COOLi containing lithium carboxylate functional groups was ultrasonically dispersed in 5 ml of deionized water for 30 min to obtain a uniform dispersion of the covalent organic framework. The cellulose membrane was immersed in the dispersion for 5 min and then directly placed in an oven for drying at 80 °C for 12 h to obtain a membrane loaded with a covalent organic framework without pore expansion.

[0105] (2) 0.2 g of caprolactone monomer, 0.045 g of trimethylene carbonate, 0.050 g of lithium bis(trifluoromethanesulfonyl)imide, and 0.005 g of lithium nitrate were mixed and stirred for 25 min at a stirring temperature of 60° C. to obtain an electrolyte precursor solution.

[0106] (3) Drop the electrolyte precursor of step (2) on the diaphragm of step (1), stack the steel sheet, lithium sheet and the diaphragm in sequence, drop the electrolyte precursor of step (2), and then cover the positive electrode, steel sheet and spring sheet in sequence, and package the battery, and perform in-situ polymerization, so that the monomer is in-situ polymerized in the diaphragm and the pores of the covalent organic framework material, the polymerization temperature is 100°C, and the polymerization time is 48h. Its electrochemical performance is significantly lower than that of the diaphragm after pore expansion in Example 1, with lower ionic conductivity and migration number, and the conductivity at 60°C is only 3.9×10 -5 S cm -2 , the lithium ion migration number is 0.76.

[0107] Figure 3 The conductivity of the polymer electrolytes prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4 varies with temperature. It can be seen that the all-solid polymer electrolyte prepared in Example 1 of the present invention has a high ionic conductivity. The conductivity can reach 5.6×10 -5 S cm -2 , which is higher than the conductivity of the polymer electrolyte in the comparative example.

[0108] Figure 4 The electrochemical stability window bar graph of the polymer electrolytes prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 shows that the polymer electrolyte prepared in Example 1 of the present invention has a higher electrochemical stability window than that of the comparative examples, and its oxidation voltage is 5.26V.

[0109] Figure 5 The lithium ion migration number bar graph of the polymer electrolytes prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4 shows that the lithium ion migration number of Example 1 prepared by the present invention is 0.85, which is much higher than the lithium ion migration number of the polymer electrolytes in the comparative examples. A high lithium ion migration number is beneficial to lithium ion conduction in the polymer electrolyte to reduce concentration polarization.

[0110] Figure 6 The voltage-time diagram of the constant current charge-discharge cycle of the lithium-lithium symmetric battery assembled with the polymer electrolyte prepared in Example 1 and Comparative Examples 1, 2, 3 and 4. It can be seen that at 60°C, the battery assembled with the polymer electrolyte of Example 1 can -2 , 0.1mAh cm -2It can perform constant current charge and discharge at a current density of 2.500 kWh and can stably cycle for more than 2500 h at a smaller polarization voltage. Compared with other comparison groups, it has a lower polarization voltage and longer cycle stability, indicating that its electrode electrolyte interface is more stable than that of other groups.

[0111] Figure 7 The discharge capacity, coulomb efficiency and cycle number of the full battery (lithium iron phosphate negative electrode) composed of the polymer electrolyte prepared in Example 1 and Comparative Examples 1, 2, 3 and 4 are shown in the figure. The battery corresponding to the polymer electrolyte of Example 1 has an initial discharge capacity of 157.6 mAh g-1 and an average coulomb efficiency of 99.74% at 60°C and 0.5C cycle conditions. The capacity retention rate after 300 cycles is 89%, indicating that the battery assembled with the polymer electrolyte of Example 1 has a more stable cycle charge and discharge performance, and its discharge specific capacity and capacity retention rate far exceed those of other comparison groups.

[0112] The present invention provides a method for loading a covalent organic framework material on a diaphragm. By dispersing the covalent organic framework material in a selected solvent, the mass fraction of the covalent organic framework can be controlled to adjust the loading amount on the diaphragm. Compared with the coating method and the hot pressing method, the method has a simpler operation process and flow, and can shorten the cycle of traditional electrolyte preparation. The solvent for dispersing the covalent organic framework material is not limited to one or more of the above embodiments.

[0113] The present invention provides a method for in-situ construction of a covalent organic framework and polymer electrolyte composite material by heterogeneous ring-opening polymerization of cyclic lactone monomers of a covalent organic framework. The multifunctional sites of organic acid salts on the covalent organic framework material can catalyze the ring-opening polymerization of cyclic lactones, and the use of the covalent organic framework material in the polymer electrolyte greatly improves the electrochemical performance of the polymer electrolyte. No need for an external solvent can avoid the use of parts irrelevant to ion conduction in the polymer electrolyte, and avoid the shortcomings of complex post-processing, high cost, and easy volatility of solvents caused by catalysts, organic solvents, etc. On the other hand, compared with other organic acid-base catalysts that damage the electrochemical performance of batteries, the covalent organic framework greatly improves the ionic conductivity and ion migration number of the polymer electrolyte after in-situ compounding with the polymer electrolyte, thereby improving the electrochemical performance of lithium-ion batteries and reducing costs. The covalent organic framework material that plays a catalytic function of ring-opening polymerization is not limited to one or more of the above embodiments.

[0114] The cyclic lactone monomers used in the present invention are numerous and can be adjusted according to the specific electrochemical performance requirements. The cyclic lactone monomers used are not limited to one or more of the above embodiments.

[0115] The present invention provides a method for preparing a covalent organic framework in-situ composite polymer electrolyte and its application. The reaction system of the present invention does not need to add additional catalysts, polar solvents or other compounds. After the electrolyte precursor is obtained by mixing the cyclic lactone monomer and the lithium salt, the electrolyte precursor is dripped onto the diaphragm loaded with the covalent organic framework, which can catalyze the ring-opening polymerization reaction of the cyclic lactone monomer.

[0116] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An in-situ preparation method of a polymer electrolyte, characterized in that: The steps include: (1) infiltrating a membrane with a dispersion of a covalent organic framework to obtain a membrane loaded with the dispersion of the covalent organic framework; and then pre-freezing the membrane loaded with the dispersion of the covalent organic framework, wherein the expansion of ice crystals during the freezing process exerts pressure on the pore walls of the membrane, causing the pore walls to deform or partially damage, thereby expanding the pores inside the membrane; (2) freeze-drying the pre-frozen membrane to freeze-sublimate the ice crystals contained therein. After the ice crystals sublimate, the space originally occupied by the ice crystals is vacated to form holes or channels, thereby obtaining a membrane loaded with a covalent organic framework after the holes are expanded; (3) transferring the electrolyte precursor solution obtained by uniformly mixing the cyclic lactone and the lithium salt to the surface of the diaphragm loaded with the covalent organic framework after the pore expansion in step (2), and assembling a lithium ion battery containing the diaphragm, wherein the cyclic lactone in the electrolyte precursor solution is in situ polymerized on the surface and pores of the diaphragm loaded with the covalent organic framework to prepare a polymer electrolyte; The covalent organic framework is a covalent organic framework containing organic acid salt functional groups; and the dispersion of the covalent organic framework is obtained by dispersing the covalent organic framework containing organic acid salt functional groups in a solvent containing water.

2. The in-situ preparation method according to claim 1, characterized in that: The covalent organic framework containing organic acid salt functional groups contains at least one of lithium sulfonate, lithium carboxylate and lithium trifluoromethylsulfonyl imide, and the covalent organic framework containing organic acid salt functional groups includes one or more of TpPa-SO3Li, TpPa-Double-SO3Li, TpPa-COOLi, TpPa-Double-COOLi and TpBDSA-Li; The mass percentage of the covalent organic framework containing organic acid salt functional group sites in the dispersion of the covalent organic framework is 3-10%.

3. The in-situ preparation method according to claim 1, characterized in that: The solvent in step (1) contains, in addition to water, one or more of tetrahydrofuran, ethanol and acetone.

4. The in-situ preparation method according to claim 1, characterized in that: The pre-freezing treatment in step (1) is performed at a temperature of -10 to -20°C for 2 to 3 hours; and / or The freeze-drying temperature in step (2) is -20 to -60°C, the time is 5 to 10 hours, and the vacuum degree is 0.1 to 10 Pa.

5. The in-situ preparation method according to claim 1, characterized in that: In step (1), the membrane is infiltrated with the dispersion of the covalent organic framework, that is, the membrane is immersed in the dispersion of the covalent organic framework for 5 to 10 minutes, so that the dispersion of the covalent organic framework infiltrates the membrane; The loading amount of the covalent organic framework in the diaphragm loaded with the covalent organic framework after pore expansion is 0.5 to 2.5 mg / cm 2 ; The separator is one of a cellulose separator, a glass fiber separator and a polyethylene terephthalate separator.

6. The in-situ preparation method according to claim 1, characterized in that: The cyclic lactone in step (3) is at least one of valerolactone, caprolactone, lactide, trimethylene carbonate, and 1,4-dioxane-2-one; The lithium salt includes one or more of lithium perchlorate, lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium nitrate and lithium iodide.

7. The in-situ preparation method according to claim 1, characterized in that: The mass fraction of the lithium salt in the electrolyte precursor solution is 2% to 40%.

8. The in-situ preparation method according to claim 1, characterized in that: The in-situ polymerization specifically comprises: performing the polymerization reaction at a temperature of 80 to 100° C. for 24 to 72 hours.

9. The polymer electrolyte prepared by the in-situ preparation method according to any one of claims 1 to 8.

10. A lithium ion battery, characterized in that: Containing the polymer electrolyte as claimed in claim 9.