Composite material and preparation method thereof, diaphragm and battery

By using ZIF material as a substrate in the lithium battery separator and covering the rigid and ceramic material layers to form a porous composite material, the problem of insufficient energy density and safety performance of traditional ceramic materials in lithium batteries is solved, and the circulation of the battery is improved. Power performance.

CN118943647APending Publication Date: 2024-11-12JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411080547.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional inorganic ceramic materials lack pore structure and high density in lithium battery separators, resulting in insufficient energy density and safety performance of the battery, and toxic gases are generated during high-temperature carbonization, affecting structural stability and ion transportability.

Method used

Composite materials, including ZIF materials as the substrate, are coated with rigid material layers and ceramic material layers to form porous and highly rigid structures, improving the stability of the separator and the cycling and power performance of the battery.

Benefits of technology

By increasing the pore structure and rigidity of the composite material, the energy density and safety performance of the battery are improved, the battery quality is reduced, the wetting and adsorption of the electrolyte are enhanced, and the circulation, power performance and safety of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943647A_ABST
    Figure CN118943647A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a composite material, a preparation method thereof, a diaphragm and a battery. The composite material provided by the invention comprises a matrix, and the matrix comprises a ZIF material; the rigid material layer is coated on at least part of the surface of the base body; and the ceramic material layer coats at least part of the surface of the rigid material layer. The preparation method of the composite material comprises the following steps: preparing a ZIF precursor; and mixing the ZIF precursor with the rigid material precursor solution, introducing reactive gas, carrying out first heating treatment, then soaking in an alkaline solution to obtain a precursor, mixing the precursor with the ceramic material precursor solution, carrying out second heating treatment, and coating the surface of the rigid material layer with the ceramic material layer. The diaphragm comprises the composite material. The porosity and rigidity of the ceramic material can be improved, the structural stability of a diaphragm using the composite material is improved, and the safety, cycle performance and power performance of a battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a composite material and a preparation method thereof, a diaphragm and a battery. Background Art

[0002] In recent years, in order to improve the comprehensive performance of batteries (such as lithium batteries), more research has been invested in the research and development of diaphragms. Generally speaking, by coating the surface of lithium-ion battery diaphragms with inorganic ceramics to form a ceramic coating, it can be used to improve the various properties of the diaphragm. For example, first, the use of ceramic coatings can improve the thermal stability of the diaphragm and avoid the risk of short circuits in the battery caused by large shrinkage of the diaphragm; second, inorganic ceramics have high mechanical strength, which can improve the puncture ability of lithium-ion battery diaphragms and improve their safety performance; third, the higher pores of the ceramic coating can accommodate more electrolytes, increase the wettability and liquid retention of the diaphragm, and improve the cycle performance of the battery.

[0003] However, traditional inorganic ceramic materials often do not have a porous structure and have a high density, which is not conducive to improving the energy density of lithium batteries. Therefore, how to improve the energy density and safety performance of the battery without changing the composition of the ceramic coating has become one of the urgent problems that need to be solved.

[0004] Related technologies, such as the patent with publication number CN103553686A, use a polyurethane organic foam impregnation method to prepare foam ceramics. The pore size and porosity of the foam ceramics obtained by this method depend on the organic foam itself. The presence of an organic system during the sintering process will inevitably produce toxic gases, and the carbon material substrate after high-temperature carbonization has the characteristic of poor rigidity, which will reduce the structural stability of the porous alumina. After the structure collapses, the specific surface area is reduced, affecting the adsorption of harmful gases as well as the safety performance and ion transport of the battery.

[0005] In view of this, this application is hereby filed. Summary of the invention

[0006] In view of this, the present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention provides a composite material and a preparation method thereof, a diaphragm and a battery, which can enhance the porosity and rigidity of the ceramic material, improve the stability of the diaphragm using the composite material, and thus improve the cycle performance and power performance of the battery using the diaphragm.

[0007] In order to solve the above technical problems, this application is implemented as follows:

[0008] According to one aspect of the present application, an embodiment of the present application provides a composite material, the composite material comprising:

[0009] A substrate, the substrate comprising a ZIF material;

[0010] A rigid material layer covering at least a portion of the surface of the substrate;

[0011] The ceramic material layer is coated on at least a portion of the surface of the rigid material layer.

[0012] In addition, the composite material according to the present application may also have the following additional technical features:

[0013] In some of the embodiments, the ZIF material includes at least one of ZIF-8, ZIF-67, ZIF-90, ZIF-71, ZIF-5, ZIF-93, ZIF-97 or ZIF-20.

[0014] In some embodiments, the average particle size of the ZIF material is 0.5 μm to 2 μm.

[0015] In some embodiments, the rigid material layer includes at least one of titanium carbide, tungsten carbide, zirconium carbide or titanium nitride.

[0016] In some embodiments, the rigid material layer has a thickness of 0.2 μm to 0.8 μm.

[0017] In some embodiments, the ceramic material layer includes at least one of aluminum oxide, zirconium oxide, chromium oxide, cobalt oxide, nickel oxide, zinc oxide, titanium oxide, manganese oxide or yttrium oxide.

[0018] In some embodiments, the ceramic material layer has a thickness of 0.5 μm to 2 μm.

[0019] In some of the embodiments, the mass ratio of the substrate, the rigid material layer and the ceramic material layer is (5-20): (1-5): (80-95).

[0020] According to another aspect of the present application, an embodiment of the present application provides a method for preparing a composite material, which comprises the following steps:

[0021] Preparation of ZIF precursor;

[0022] The ZIF precursor is mixed with a rigid material precursor solution, a reactive gas is introduced, and a first heating treatment is performed to obtain a ZIF material coated with a rigid material layer;

[0023] The ZIF material coated by the rigid material layer is immersed in an alkaline solution to obtain a precursor, the precursor is mixed with a ceramic material precursor solution, and a second heating treatment is performed to coat the ceramic material layer on the surface of the rigid material layer.

[0024] In some embodiments, the preparation of the ZIF precursor includes: mixing a metal salt, an imidazole raw material and a solvent to obtain a mixed solution, and reacting the mixed solution at 100° C. to 200° C. for 1 h to 6 h to obtain the ZIF precursor.

[0025] In some embodiments, the rigid material precursor solution includes at least one of a titanium tetrachloride solution, a tungsten tetrachloride solution, or a zirconium chloride solution.

[0026] In some embodiments, the concentration of the rigid material precursor solution is 0.01-0.5 mol / L.

[0027] In some of the embodiments, the reactive gas is suitable for reacting with the rigid material precursor, and the reactive gas includes at least one of an alkane gas or ammonia; wherein the alkane gas includes at least one of methane, ethane, propane or butane.

[0028] In some embodiments, the first heat treatment is performed at a temperature of 800° C. to 1400° C. for a time of 2 h to 6 h.

[0029] In some embodiments, the alkaline solution includes at least one of a sodium hydroxide solution or a potassium hydroxide solution.

[0030] In some of the embodiments, the concentration of the alkaline solution is 0.5 to 1 mol / L;

[0031] In some embodiments, mixing the precursor with the ceramic material precursor solution includes: soaking the precursor in the ceramic material precursor solution for 0.5 h to 5 h.

[0032] In some embodiments, the ceramic material precursor solution includes at least one of an aluminum salt solution, a zirconium salt solution, a chromium salt solution, a cobalt salt solution, a nickel salt solution, a zinc salt solution, a titanium salt solution, a manganese salt solution or a yttrium salt solution.

[0033] In some embodiments, the second heat treatment is performed at a temperature of 1000° C. to 1500° C. for a time of 2 h to 6 h.

[0034] According to another aspect of the present application, an embodiment of the present application provides a diaphragm, which includes a base film and a ceramic coating provided on at least one side surface of the base film;

[0035] The ceramic coating comprises the aforementioned composite material or the composite material prepared by the aforementioned method, and a binder.

[0036] In some of the embodiments, the mass ratio of the composite material to the binder is (90-95):(5-10).

[0037] According to still another aspect of the present application, an embodiment of the present application provides a battery, which includes the aforementioned separator.

[0038] Implementing the technical solution of the present invention has at least the following beneficial effects:

[0039] In the present application embodiment, the composite material provided includes a matrix, a rigid material layer and a ceramic material layer, wherein the matrix includes a ZIF material. Thus, using the ZIF material as a substrate, and forming a rigid material layer on the surface of the ZIF material, and forming a ceramic material layer on the surface of the rigid material layer, the composite material can have a larger specific surface area and improve its adsorption performance; and the composite material has a larger rigidity, the structure is not easy to collapse, and the structural stability is strong; the composite material uses the ZIF material as a substrate, which can make the composite material have a large number of pore structures, can accommodate more electrolytes and improve the transmission of lithium ions. The structure of the composite material can make the material lighter, can reduce the mass of the battery, and improve the weight energy density.

[0040] Therefore, the application of the composite material in the diaphragm can improve the existing ceramic materials in the diaphragm, such as the lack of pore structure, high density, low rigidity and other problems. At the same time, the diaphragm applied to the composite material enhances the wettability and adsorption of the electrolyte, can adsorb gases such as oxygen in the lithium battery, avoid oxidation of the electrolyte, improve the thermal stability of the diaphragm, and provide more pathways for the transmission of ions, thereby helping to improve the cycle performance, power performance, rate performance and safety of the battery using the diaphragm.

[0041] Additional aspects and advantages of the present application will be given in part in the following description, and in part will become obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Shown is a schematic structural diagram of a composite material provided by an embodiment of the present invention.

[0043] Description of reference numerals:

[0044] 10-matrix;

[0045] 20- Rigid material layer;

[0046] 30-Ceramic material layer. DETAILED DESCRIPTION

[0047] The present application is further described below in conjunction with specific embodiments. It should be understood that these embodiments of the present application are only used to illustrate the present application and are not used to limit the scope of the present application.

[0048] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0049] Hereinafter, embodiments of the composite material, method for preparing the composite material, battery, etc. of the present application will be specifically disclosed with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0050] If there is no special description, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. If there is no special description, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.

[0051] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0052] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0053] As analyzed in the background technology of this application, by providing a ceramic coating on the surface of a traditional diaphragm, it is possible to improve the thermal stability of the diaphragm, improve the puncture ability of the diaphragm, etc. However, existing ceramic materials still have certain shortcomings. For example, pure inorganic ceramic materials often do not have a porous structure and have a large density, and have poor rigidity and poor structural stability, which affects the energy density and other properties of the battery, and further improvements are needed. In view of this, the present application provides a composite material and a preparation method thereof, a diaphragm and a battery, which improves the porosity and rigidity of ceramic materials (such as ceramic materials such as alumina) to promote the application of ceramic materials such as porous alumina in lithium batteries, so as to alleviate the above problems. The present application is described in detail below.

[0054] [Composite Materials]

[0055] See also Figure 1 As shown, in some embodiments, the present application provides a composite material, the composite material comprising:

[0056] A substrate 10, wherein the substrate 10 comprises a ZIF material;

[0057] A rigid material layer 20, covering at least a portion of the surface of the substrate 10;

[0058] The ceramic material layer 30 covers at least a portion of the surface of the rigid material layer 20 .

[0059] In the present application, the provided composite material can be used in a diaphragm, for example, in a ceramic coating of a diaphragm, to improve the problems existing in the ceramic material in the ceramic coating of the existing diaphragm, such as lack of pore structure, poor rigidity, high density, etc.

[0060] It should be pointed out that in the present application, the "coating" is not limited to direct coating, but also includes indirect coating. For example, the rigid material layer 20 coats the substrate 10, and there may be no other structure between the rigid material layer 20 and the outer surface of the substrate 10, or there may be one or more layers of other structures between the rigid material layer 20 and the outer surface of the substrate 10. Preferably, there is no other structure between the rigid material layer 20 and the outer surface of the substrate 10. Similarly, the ceramic material layer 30 coats the rigid material layer 20, and there may be no other structure between the ceramic material layer 30 and the outer surface of the rigid material layer 20, or there may be one or more layers of other structures between the ceramic material layer 30 and the outer surface of the rigid material layer 20.

[0061] The rigid material layer 20 is formed or coated on at least part of the surface of the substrate 10, which can improve the rigidity of the material and can be used to improve the structural stability of the composite material so that the structure of the material is not easy to collapse. The rigid material layer 20 is formed on at least part of the surface of the substrate 10, which means that the rigid material layer 20 can completely encapsulate the substrate 10 in the rigid material layer 20, or the rigid material layer 20 can only coat a part of the outer surface of the substrate 10; that is, the rigid material layer 20 can completely coat the substrate 10, or can coat a part of the surface of the substrate 10, preferably completely coat it.

[0062] The ceramic material layer 30 is formed or coated on at least part of the surface of the rigid material layer 20, which can improve the thermal stability of the composite material, improve the mechanical strength of the composite material, and enhance the electrochemical performance of the composite material. The ceramic material layer 30 is formed on at least part of the surface of the rigid material layer 20, which means that the ceramic material layer 30 can completely encapsulate the rigid material layer 20 in the ceramic material layer 30, or the ceramic material layer 30 can only coat a part of the outer surface of the rigid material layer 20; that is, the ceramic material layer 30 can completely coat the rigid material layer 20, or can coat a part of the surface of the rigid material layer 20, preferably completely coat it.

[0063] In the present application, ZIF material is used as the matrix 10 material. ZIF material is a zeolite imidazolate skeleton structure material, which is a type of metal organic framework material. ZIF material is a porous material that combines the high stability of inorganic zeolite with the high porosity and organic function of MOFs, and has the characteristics of high stability, high porosity and organic function.

[0064] Thus, the composite material provided is a core-shell structure, wherein the core is made of ZIF material, and the outer shell or shell layer includes a first coating layer and a second coating layer, that is, includes a rigid material layer 20 and a ceramic material layer 30, wherein the rigid material layer 20 is a rigid shell layer mainly formed of a rigid material, and the ceramic material layer 30 is a shell layer mainly formed of a ceramic material. In the embodiment of the present application, the ZIF material is used as a substrate, and the rigid material layer 20 is formed on the surface of the ZIF material, and the ceramic material layer 30 is formed on the surface of the rigid material layer 20, so that the composite material has a larger specific surface area and improves the adsorption performance of the composite material, such as adsorbing gases such as oxygen in the lithium battery to avoid oxidation of the electrolyte, thereby helping to improve the safety performance of the lithium battery.

[0065] In the embodiments of the present application, the composite material provided uses the ZIF material as the substrate, which can effectively alleviate the defect that the existing simple inorganic ceramic material often does not have a pore structure. This is because ZIF has a large number of pores, which can make the composite material have a large number of pore structures, can accommodate more electrolyte and improve the transmission of lithium ions, that is, through the pore structure, not only can more electrolyte be accommodated, but also more pathways can be provided for the transmission of ions, which is conducive to improving the cycle performance and power performance of the battery.

[0066] In the embodiment of the present application, the composite material provided forms a rigid material layer 20 on the surface of the ZIF material. The composite material has greater rigidity, is not easy to collapse, and has strong structural stability. It can effectively alleviate the problems of poor structural stability of existing porous materials, reduced specific surface area after structural collapse, which affects the adsorption of harmful gases, as well as the safety performance and ion transport of batteries.

[0067] In the embodiments of the present application, the composite material provided can alleviate the problem of high density of traditional inorganic ceramic materials. The composite material can have a hollow structure through the coordinated arrangement of the above-mentioned matrix 10, rigid material layer 20 and ceramic material layer 30. The hollow structure can make the material lighter, reduce the mass of the battery, and thus help to improve the weight energy density.

[0068] Therefore, the composite material can be used in the diaphragm to improve the existing ceramic materials in the diaphragm, such as the lack of pore structure, high density, low rigidity and other problems. At the same time, the diaphragm used in the composite material enhances the wettability and adsorption of the electrolyte, can adsorb gases such as oxygen in the lithium battery, avoid oxidation of the electrolyte, improve the thermal stability of the diaphragm, reduce thermal shrinkage, and improve the mechanical strength of the diaphragm. It can also provide more pathways for the transmission of ions, thereby helping to improve the cycle performance, power performance, rate performance and safety of the battery using the diaphragm.

[0069] The inventors have found through in-depth research that when the composite material of the present application satisfies the above-mentioned design conditions and optionally satisfies one or more of the following conditions, the performance of the composite material can be further improved.

[0070] In some embodiments, the ZIF material includes, but is not limited to, any one or a combination of at least two of ZIF-8, ZIF-67, ZIF-90, ZIF-71, ZIF-5, ZIF-93, ZIF-97 or ZIF-20. For the sake of brevity, the combinations within the above range are no longer listed one by one.

[0071] Preferably, the ZIF material is selected from one or more of ZIF-8, ZIF-67 or ZIF-90. These ZIF materials have a wide range of raw material sources, are easy to obtain, and are easy to prepare, and have better application effects in this application.

[0072] The above-mentioned ZIF materials have a three-dimensional porous skeleton structure and have the characteristics of high stability and high porosity, which are conducive to accommodating more electrolyte and improving the transmission of lithium ions, thereby helping to improve the battery's cycle performance and other properties.

[0073] In some embodiments, the average particle size of the ZIF material (granular) is 0.5 μm to 2 μm. Preferably, in some embodiments, the average particle size of the ZIF material (granular) is 0.5 μm to 1.5 μm. As an example, the average particle size of the ZIF material can be any one of 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, or a range between any two of them.

[0074] By making the particle size of the ZIF material within the above-mentioned suitable range, the processing performance of the material can be improved, which is convenient for processing and can also make the comprehensive electrical properties of the composite material better.

[0075] In some embodiments, the rigid material layer 20 includes, but is not limited to, any one or a combination of at least two of titanium carbide, tungsten carbide, zirconium carbide or titanium nitride. For the sake of brevity, the combinations within the above range are not listed one by one.

[0076] Preferably, the rigid material layer 20 is selected from one or more of titanium carbide, tungsten carbide or titanium nitride.

[0077] In the present application, the material of the rigid material layer 20 can be selected from carbides or nitrides, which have a certain rigidity, and these carbides or nitrides are coated on the surface of the ZIF material to form a rigid material layer 20 of a certain thickness; that is, when the above-mentioned carbides or nitrides are in a coating relationship with the ZIF material, the modification effect of the above-mentioned carbides or nitrides can be exerted to a greater extent, thereby improving the structural strength of the material, so that the final composite material has greater rigidity and the structure is not easy to collapse.

[0078] It should be noted that the rigid material layer 20 can be selected from carbides or nitrides. Carbides and nitrides are not limited to the substances listed above. Other rigid conductive materials that can be used to improve the structural strength of the material do not limit the purpose of the present invention. Other similar carbides and nitrides can also be used in the present invention.

[0079] In some embodiments, the thickness of the rigid material layer 20 is 0.2 μm to 0.8 μm. Preferably, in some embodiments, the thickness of the rigid material layer 20 is 0.3 μm to 0.7 μm. As an example, the thickness of the rigid material layer 20 can be any one of 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, or a range between any two of them.

[0080] The thickness of the rigid material layer 20 can be adjusted according to the size of the matrix core. The appropriate thickness of the rigid material layer 20 can not only ensure that the composite material has good processing performance, but also avoid the thickness being too thick or the rigid material layer 20 having too much material, which may affect the timely release of active lithium, increase battery impedance or affect the cycle performance of the battery cell, or avoid the thickness being too thin to effectively exert the modification effect of the rigid material layer 20, that is, avoid the thickness being too thin to reduce the effect of the rigid material layer 20 in improving the structural strength of the material.

[0081] In some embodiments, the ceramic material layer 30 includes, but is not limited to, any one or a combination of at least two of aluminum oxide, zirconium oxide, chromium oxide, cobalt oxide, nickel oxide, zinc oxide, titanium oxide, manganese oxide or yttrium oxide. For the sake of brevity, the combinations within the above range are not listed one by one.

[0082] Preferably, the ceramic material layer 30 is selected from one or more of aluminum oxide, zirconium oxide, and chromium oxide. More preferably, the ceramic material layer 30 is selected from aluminum oxide. These ceramic materials are widely available and easy to obtain, which is conducive to reducing costs, and have better application effects in the present application.

[0083] In some embodiments, the thickness of the ceramic material layer 30 is 0.5 μm to 2 μm. Preferably, in some embodiments, the thickness of the ceramic material layer 30 is 0.5 μm to 1.5 μm. As an example, the thickness of the ceramic material layer 30 can be any one of 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, or a range between any two of them.

[0084] The thickness of the ceramic material layer 30 can be adjusted according to the size of the matrix core. The appropriate thickness of the ceramic material layer 30 can not only ensure that the composite material has good processing performance, but also avoid the thickness being too thick or the ceramic material layer 30 having too much material that affects the timely release of active lithium, increases battery impedance or affects the cycle performance of the battery cell, or it can also avoid the thickness being too thin to effectively exert the beneficial effects of the ceramic material layer 30.

[0085] In some embodiments, the mass ratio of the substrate 10, the rigid material layer 20 and the ceramic material layer 30 is (5-20): (1-5): (80-95). As an example, the mass ratio of the substrate 10, the rigid material layer 20 and the ceramic material layer 30 can be 5:2:93, 5:5:90, 10:1:89, 12:3:85, 15:5:80, 17:3:80, etc.

[0086] The above-mentioned composite material provided in the embodiment of the present application has greater rigidity, higher structural strength, better structural stability, larger specific surface area, a certain pore structure, and lighter weight (compared with traditional inorganic ceramic materials), which is beneficial to improving the battery's cycle performance, power performance, rate performance and energy density, as well as safety performance.

[0087] [Method for preparing composite material]

[0088] In some embodiments, the present application provides a method for preparing a composite material, which comprises the following steps:

[0089] Preparation of ZIF precursor;

[0090] The ZIF precursor and the rigid material precursor solution are mixed, a reactive gas is introduced, and a first heating treatment is performed to obtain a ZIF material coated by the rigid material layer 20;

[0091] The ZIF material coated by the rigid material layer 20 is immersed in an alkaline solution to obtain a precursor, and the precursor is mixed with a ceramic material precursor solution, and a second heating treatment is performed to coat the surface of the rigid material layer 20 with the ceramic material layer 30 .

[0092] The method for preparing the composite material provided by the embodiment of the present invention is to mix the prepared ZIF precursor with the rigid material precursor solution, and obtain the ZIF material coated by the rigid material layer 20 after heat treatment, that is, to form the rigid material layer 20 on the surface of the ZIF material; then the ZIF material coated by the rigid material layer 20 is soaked in an alkaline solution and then mixed with the ceramic material precursor solution, and then heat treated to form a ceramic material layer 30 on the surface of the rigid material layer 20, that is, to obtain a composite material with a multi-layer coated structure. The preparation method is simple in process, easy to operate, highly feasible, and easy to realize industrialization; the composite material prepared by the method has good structural stability and good electrochemical properties.

[0093] It should be understood that all the features and advantages described above for the “composite material” are also applicable to the “composite preparation method” and will not be described in detail here.

[0094] In some specific embodiments, the method for preparing the composite material specifically comprises the following steps (a) to (c):

[0095] (a) Preparation of ZIF precursor.

[0096] In step (a), preparing the ZIF precursor includes: mixing a metal salt, an imidazole raw material and a solvent to obtain a mixed solution, and reacting the mixed solution at 100° C. to 200° C. for 1 h to 6 h to obtain the ZIF precursor.

[0097] In the present application, the matrix 10 of the composite material is a ZIF material, which may include at least one of ZIF-8, ZIF-67, ZIF-90, ZIF-71, ZIF-5, ZIF-93, ZIF-97 or ZIF-20; when different ZIF materials are selected, the synthetic raw materials such as metal salts, imidazole raw materials and solvents used in the preparation process are different.

[0098] As an example, when preparing a ZIF precursor, a metal salt such as a zinc salt or a cobalt salt (such as zinc nitrate hexahydrate, cobalt nitrate hexahydrate) and an imidazole raw material such as 2-methylimidazole can be uniformly mixed in a solvent such as water, DMF (N,N-dimethylformamide), ethylene glycol, methanol, etc. at a mass ratio of 1:3 to 6 to prepare a mixed solution of a certain concentration, and the concentration of the mixed solution ranges from 5 to 100 g / L.

[0099] Optionally, when the ZIF material is selected from ZIF-8, the zinc salt, 2-methylimidazole and methanol or water can be mixed to obtain a mixed solution.

[0100] Optionally, when the ZIF material is selected from ZIF-67, the cobalt salt, 2-methylimidazole and water can be mixed to obtain a mixed solution.

[0101] Optionally, when the ZIF material is selected from ZIF-90, the zinc salt, imidazole-2-carboxaldehyde and dimethylformyl may be mixed to obtain a mixed solution.

[0102] It should be understood that the preparation of ZIF materials can adopt known methods in the prior art. When the ZIF material is selected from other ZIF materials such as ZIF-71, ZIF-5, ZIF-93, etc., the corresponding metal salts, imidazole raw materials and solvents can be selected accordingly, and they are not listed one by one here.

[0103] Exemplarily, in step (a), a metal salt such as a zinc salt or a cobalt salt (such as zinc nitrate hexahydrate, cobalt nitrate hexahydrate) and an imidazole raw material such as 2-methylimidazole are uniformly mixed in a solvent such as water, DMF (N,N-dimethylformamide), ethylene glycol, methanol, etc. at a mass ratio of 1:3 to 6 (such as 1:3, 1:4, 1:5, 1:6, etc.) to prepare a mixed solution of a certain concentration, and the concentration of the mixed solution ranges from 5 to 100 g / L (such as 5 g / L, 10 g / L, 15 g / L, 20 g / L, 25 g / L, etc.). g / L, 30g / L, 50g / L, 80g / L, 100g / L, etc.); then, slowly heating the mixed solution to 100°C-200°C (such as 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 180°C, 200°C, or any range between two thereof) and reacting for 1h-6h (such as 1h, 2h, 3h, 4h, 5h, 6h, or any range between two thereof) to obtain a ZIF precursor.

[0104] (b) preparing a rigid material layer 20 , that is, preparing a ZIF material covered by the rigid material layer 20 .

[0105] In step (b), the ZIF precursor prepared in step (a) is mixed with a rigid material precursor solution, and a reactive gas is introduced under a protective atmosphere to perform a first heating treatment to obtain a ZIF material coated with a rigid material layer 20 .

[0106] In the present application, in step (b), the ZIF precursor obtained in step (a) can be washed with water first, and then the washed ZIF precursor is put back into the rigid material precursor solution, stirred and soaked for 0.5h to 2h, and then the soaked material is taken out, and a reactive gas is introduced under a protective atmosphere to perform a first heating treatment to obtain a ZIF material coated with a rigid material layer 20. In this process, by repeatedly reacting several times (by controlling the number of repetitions), a rigid material layer 20 of suitable thickness can be obtained.

[0107] In the present application, the rigid material layer 20 may be, but is not limited to, at least one of titanium carbide, tungsten carbide, zirconium carbide or titanium nitride.

[0108] In some embodiments, in step (b), the rigid material precursor solution includes but is not limited to at least one of a titanium tetrachloride solution, a tungsten tetrachloride solution, or a zirconium chloride solution.

[0109] In the present application, the rigid material precursor solution can be a titanium tetrachloride solution, a tungsten tetrachloride solution, a zirconium chloride solution, etc. Thus, at high temperature, titanium tetrachloride can react with reactive gases such as alkane gases to generate titanium carbide, tungsten tetrachloride can react with reactive gases such as alkane gases to generate tungsten carbide, zirconium chloride can react with alkane gases to generate zirconium carbide, and titanium tetrachloride can also react with reactive gases such as ammonia (NH3) to generate titanium nitride.

[0110] In some embodiments, in step (b), the concentration of the rigid material precursor solution is 0.01 to 0.5 mol / L. For example, the concentration of the titanium tetrachloride solution, the tungsten tetrachloride solution or the zirconium chloride solution can be 0.01 to 0.5 mol / L. As an example, the concentration of the rigid material precursor solution can be any one of 0.01 mol / L, 0.02 mol / L, 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L or a range between any two of them.

[0111] Optionally, in step (b), the protective atmosphere gas may be nitrogen (N2), or may be a rare gas such as helium or argon; preferably, the protective atmosphere gas is nitrogen.

[0112] In some embodiments, in step (b), the reactive gas is suitable for reacting with the rigid material precursor, for example, the reactive gas includes at least one of an alkane gas or an ammonia gas.

[0113] In the present application, a reactive gas that can react with titanium tetrachloride, tungsten tetrachloride or zirconium chloride at high temperature is selected, such as alkane gas, ammonia gas and the like. At high temperature, a rigid conductive material such as titanium carbide, titanium nitride, tungsten carbide, zirconium carbide and the like can be generated by reacting alkane gas, ammonia gas and the like with a precursor such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride to obtain a rigid material layer 20.

[0114] Optionally, the alkane gas includes, but is not limited to, at least one of methane, ethane, propane or butane.

[0115] It should be noted that the alkane gas is not limited to the substances listed above, and can be used to react with precursors such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride, which does not limit the purpose of the present invention. Other similar alkane gases can also be used in the present invention.

[0116] In some embodiments, in step (b), the temperature of the first heat treatment is 800°C to 1400°C, and the time is 2h to 6h. As an example, the first heating temperature can be any one of 800°C, 900°C, 1000°C, 1100°C, 1200°C, and 1400°C, or a range between any two thereof; the time can be any one of 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, and 6h, or a range between any two thereof.

[0117] In the first heating treatment temperature range, precursors such as titanium tetrachloride, tungsten tetrachloride or zirconium chloride can react with reactive gases such as alkane gases and ammonia to generate rigid conductive materials such as titanium carbide, titanium nitride, tungsten carbide and zirconium carbide.

[0118] (c) preparing the ceramic material layer 30 , that is, forming the ceramic material layer 30 on the surface of the rigid material layer 20 .

[0119] In step (c), the ZIF material coated by the rigid material layer 20 obtained in step (b) is immersed in an alkaline solution to obtain a precursor, and the precursor is mixed with a ceramic material precursor solution, and a second heat treatment is performed to coat the surface of the rigid material layer 20 with a ceramic material layer 30 .

[0120] In the present application, in step (c), the ZIF material coated by the rigid material layer 20 obtained in step (b) can be first ball-milled into a corresponding size, and then immersed in an alkaline solution of a certain concentration and evenly stirred and immersed for 0.5h to 5h (preferably 0.5h to 2h). Subsequently, the precursor (ZIF material coated by the rigid material layer 20) after soaking in the alkaline solution is transferred to a ceramic material precursor solution (such as aluminum nitrate solution, etc.) and continued to be stirred and immersed for 0.5h to 5h (preferably 0.5h to 2h). Subsequently, the product is placed in a furnace and heated to 1000 to 1500°C under nitrogen protection. After a high-temperature reaction for 2 to 6h, the target product composite material can be obtained.

[0121] In the above step (c), the ZIF material coated with the rigid material layer 20 obtained in step (b) is immersed in an alkaline solution, so that the alkaline solution molecules can be adsorbed in the pores and on the surface of the ZIF material, and then the ZIF material immersed in the alkaline solution is mixed with a ceramic material precursor solution (such as aluminum nitrate solution), OH - The radical ions will react with aluminum ions to form solid aluminum hydroxide which will precipitate on the surface of ZIF and inside the pores.

[0122] In some embodiments, in step (c), the alkaline solution includes, but is not limited to, at least one of a sodium hydroxide solution or a potassium hydroxide solution.

[0123] In some embodiments, in step (c), the concentration of the alkaline solution is 0.5 to 1 mol / L. As an example, the concentration can be any one of 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, or a range between any two of them.

[0124] In some embodiments, mixing the precursor with the ceramic material precursor solution includes: soaking the precursor in the ceramic material precursor solution for 0.5h to 5h, preferably 0.5h to 2h, for example, it can be any one of 0.5h, 1h, 1.5h, 2h, 3h, 5h or a range between any two of them.

[0125] In some embodiments, in step (c), the ceramic material precursor solution includes at least one of an aluminum salt solution, a zirconium salt solution, a chromium salt solution, a cobalt salt solution, a nickel salt solution, a zinc salt solution, a titanium salt solution, a manganese salt solution, or a yttrium salt solution.

[0126] Optionally, the above-mentioned aluminum salt solution, zirconium salt solution, chromium salt solution, cobalt salt solution, nickel salt solution, zinc salt solution, titanium salt solution, manganese salt solution or yttrium salt solution can be a nitrate solution, sulfate solution, etc. of each metal, which is not limited in the present application.

[0127] In some embodiments, in step (c), the temperature of the second heat treatment is 1000° C. to 1500° C., and the time is 2 h to 6 h. As an example, the second heating temperature can be any one of 1000° C., 1100° C., 1200° C., 1400° C., and 1500° C., or a range between any two of them; and the time can be any one of 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, and 6 h, or a range between any two of them.

[0128] The preparation method of the composite material provided in the embodiment of the present application has simple process, strong feasibility, high efficiency and environmental protection, and is easy to realize large-scale production.

[0129] [Diaphragm]

[0130] In some embodiments, the embodiments of the present application provide a diaphragm, which includes a base film and a ceramic coating disposed on at least one side of the base film;

[0131] The ceramic coating comprises the aforementioned composite material or the composite material prepared by the aforementioned method, and a binder.

[0132] The diaphragm sheet includes the above-mentioned composite material provided in the embodiment of the present application. Therefore, the diaphragm also has all the characteristics and advantages of the above-mentioned composite material, which will not be repeated here.

[0133] The above-mentioned diaphragm includes a base film and a ceramic coating disposed on at least one surface of the base film, wherein the ceramic coating includes the composite material provided by any one of the above-mentioned embodiments of the present application. As an example, the base film has two surfaces opposite to each other in its own thickness direction, and the ceramic coating is disposed on any one or both of the two opposite surfaces of the base film.

[0134] The present application has no particular restrictions on the material of the base film in the diaphragm, as long as the purpose of the present application can be achieved, and can be selected according to actual needs. For example, in some embodiments, the base film may include polyethylene (PE), polypropylene (PP), etc. Of course, in other embodiments, other types of base films known in the art may also be used.

[0135] In some embodiments, in the ceramic coating of the diaphragm, the mass ratio of the composite material to the binder is (90-95):(5-10). As an example, the mass ratio of the composite material to the binder can be 90:10, 91:9, 92:8, 93:7, 94:6, 95:5, etc.

[0136] Optionally, in the ceramic coating of the diaphragm, the binder may be polyvinylidene fluoride (PVDF) or other binders well known in the art.

[0137] In some embodiments, in the diaphragm, the thickness of the base film is 4 μm to 20 μm, for example, it can be any point value among 4 μm, 5 μm, 6 μm, 8 μm, 10 μm, 15 μm, 20 μm or a range value between any two of them.

[0138] In some embodiments, in the diaphragm, the thickness of the ceramic coating is 1 μm to 10 μm, for example, it can be any one of 1 μm, 2 μm, 5 μm, 6 μm, 8 μm, 10 μm, or a range between any two of them.

[0139] [Battery]

[0140] In some embodiments, the present application provides a battery comprising the aforementioned separator.

[0141] In the embodiment of the present application, the battery may be a secondary battery or a primary battery, preferably a secondary battery. For example, the battery may be a lithium-ion secondary battery, a lithium primary battery, a sodium-ion battery, a magnesium-ion battery, etc., but is not limited thereto. The battery structure of the present application includes but is not limited to a soft-pack lithium-ion battery, a square hard-shell battery, or a cylindrical hard-shell battery, etc.

[0142] It should be noted that, in the specific implementation manner, the present application is explained by taking a lithium-ion battery as an example of a secondary battery, but the battery of the present application is not limited to a lithium-ion battery.

[0143] In some embodiments, the battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and the above-mentioned separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet to play a role of isolation. The electrolyte plays a role of conducting ions between the positive electrode sheet and the negative electrode sheet.

[0144] In this embodiment, there is no limitation on the specific materials and structures of the current collector and the active material layer in the positive electrode sheet and the negative electrode sheet, and the positive electrode sheet and negative electrode sheet structures and components known in the art and applicable to secondary batteries can be selected.

[0145] The electrolyte that can be used in the embodiments of the present application can be an electrolyte known in the prior art. The specific type and structure of the electrolyte can be an electrolyte type that can be used in a secondary battery that is well known in the art, such as an ester electrolyte or an ether electrolyte, etc., which is not limited and will not be repeated here.

[0146] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in this area or the product instructions are used. If the manufacturer of the reagents, materials or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0147] Example 1

[0148] 1. Preparation of composite materials

[0149] (a) zinc salt (zinc nitrate hexahydrate) and 2-methylimidazole are uniformly mixed in a solvent such as water at a mass ratio of 1:4 to prepare a mixed solution with a concentration of 10 g / L; then, the mixed solution is slowly heated to 140°C and stirred for reaction for 4 hours to obtain a ZIF-8 precursor.

[0150] (b) The ZIF precursor obtained in step (a) is washed with water, and then the ZIF precursor is re-added to a 0.1 mol / L titanium tetrachloride solution after washing, stirred and soaked for 1 hour, and then the soaked material is taken out, and an alkane gas (such as methane) is introduced under a N2 protective atmosphere, and reacted at 1000°C for 3 hours. This process is repeated several times to obtain a ZIF material coated with a rigid material layer 20 with a thickness of 0.5 μm, that is, a precursor ZIF@titanium carbide with a rigid material layer of 0.5 μm is obtained.

[0151] (c) ball-milling the ZIF material coated with the rigid material layer obtained in step (b) into a corresponding size, and then soaking it in a 0.5 mol / L sodium hydroxide solution, stirring and soaking it evenly for 1 hour, then transferring the precursor (ZIF material coated with the rigid material layer) after soaking in the alkaline solution to an aluminum nitrate solution and continuing to stir and soak it for 1 hour, and then placing the product in a furnace, heating it to 1200°C under nitrogen protection, and reacting it at high temperature for 4 hours to obtain the target product composite material.

[0152] 2. Preparation of diaphragm

[0153] The prepared composite material and the binder polyvinylidene fluoride (PVDF) are uniformly dispersed in an N-methylpyrrolidone (NMP) solvent in a mass ratio of 95:5, and the viscosity is adjusted to a preset value to obtain a slurry containing the composite material; the slurry containing the composite material is applied to a PE base film by extrusion coating or spraying, and a ceramic coating with a thickness of 3 μm is formed on both sides of the PE base film to obtain a diaphragm.

[0154] 3. Preparation of negative electrode sheet

[0155] The negative electrode active material is made of graphite and silicon oxide (mass ratio is 8:2), the conductive agent is conductive carbon black (SP), the adhesive is polyacrylic acid (PAA) and styrene-butadiene rubber (SBR), and the negative electrode current collector is made of 6 μm thick copper foil;

[0156] The negative electrode active material, conductive agent, PAA, and SBR were mixed in a mass ratio of 95.5:1.5:2:1, and deionized water was added and stirred to form a uniform and stable negative electrode slurry. The negative electrode slurry was evenly coated on the negative electrode current collector with a coating surface density of 105 g / m 2 After drying, the negative electrode sheet is obtained, and the compaction density is 1.5g / cm 3 .

[0157] 4. Preparation of positive electrode

[0158] The positive electrode active material is ternary nickel cobalt lithium manganese oxide LiNi 0.8 Co 0.1 Mn 0.1 O2, the conductive agent is conductive carbon black (SP) and carbon nanotubes, the adhesive is polyvinylidene fluoride (PVDF5130), and the positive electrode current collector is 13μm thick aluminum foil;

[0159] The positive electrode active material, SP, carbon nanotubes and binder were mixed in a mass ratio of 96:2:1:1, and N-methylpyrrolidone (NMP) was added and stirred to form a uniform and stable positive electrode slurry. The positive electrode slurry was evenly coated on the positive electrode current collector with a coating surface density of 195 g / m 2After drying and cold pressing, the positive electrode sheet is obtained, and the compaction density is 3.4g / cm 3 .

[0160] 5. Preparation of electrolyte

[0161] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then a solute LiPF6 is added to the organic solvent to dissolve and mix evenly to obtain an electrolyte; wherein the concentration of LiPF6 is 1.2 mol / L.

[0162] 6. Battery assembly

[0163] Arrange the positive electrode sheet, separator, negative electrode sheet and separator in order, and use winding as the assembly method. Inject the electrolyte into the dry battery cell, soak for 24 hours, and then form it at 45℃. The formation process is: charge at 0.05C to 3.4V, and then charge at 0.2C to 3.75V; after aging at room temperature for 24 hours, the battery cell is completed.

[0164] Example 2

[0165] Embodiment 2 is substantially the same as Embodiment 1, except that:

[0166] In <Preparation of Composite Material>, in step (b), the high-temperature carbonization temperature of the rigid material layer is adjusted, that is, the reaction is carried out at 1200° C. for 3 hours.

[0167] The rest are the same as in Example 1.

[0168] Example 3

[0169] Embodiment 3 is substantially the same as Embodiment 1, except that:

[0170] In <Preparation of Composite Material>, in step (b), the high-temperature carbonization temperature of the rigid material layer is adjusted, that is, the reaction is carried out at 800° C. for 3 hours.

[0171] The rest are the same as in Example 1.

[0172] Example 4

[0173] Embodiment 4 is substantially the same as Embodiment 1, except that:

[0174] In <Preparation of composite material>, in step (b), the thickness of the rigid material layer is 1 μm.

[0175] The rest are the same as in Example 1.

[0176] Example 5

[0177] Example 5 is substantially the same as Example 1, except that:

[0178] In <Preparation of Composite Material>, in step (b), the thickness of the rigid material layer is 2 μm.

[0179] The rest are the same as in Example 1.

[0180] Example 6

[0181] Embodiment 6 is substantially the same as Embodiment 1, except that:

[0182] In <Preparation of Composite Material>, in step (b), the rigid material precursor solution is adjusted to a 0.1 mol / L tungsten tetrachloride solution to obtain the precursor ZIF@tungsten carbide.

[0183] The rest are the same as in Example 1.

[0184] Example 7

[0185] Example 7 is basically the same as Example 1, except that:

[0186] In <Preparation of composite materials>, in step (a), cobalt salt (cobalt nitrate hexahydrate) and 2-methylimidazole are uniformly mixed in a solvent such as water at a mass ratio of 1:4 to prepare a mixed solution with a concentration of 10 g / L; then, the mixed solution is slowly heated to 140°C and stirred for reaction for 4 hours to obtain a ZIF-67 precursor.

[0187] The rest are the same as in Example 1.

[0188] Example 8

[0189] Example 8 is basically the same as Example 1, except that:

[0190] In <Preparation of composite material>, in step (c), the aluminum nitrate solution is adjusted to a zirconium nitrate solution, heated to 1400° C., and reacted at high temperature for 6 hours.

[0191] The rest are the same as in Example 1.

[0192] Example 9

[0193] Example 9 is basically the same as Example 1, except that:

[0194] In <Preparation of Composite Material>, in step (c), the aluminum nitrate solution is adjusted to a chromium nitrate solution, heated to 1000°C, and reacted at high temperature for 5 hours.

[0195] The rest are the same as in Example 1.

[0196] Comparative Example 1

[0197] Comparative Example 1 is substantially the same as Example 1, except that:

[0198] In <Preparation of Composite Material>, the rigid material layer is eliminated, that is, a ceramic material layer is directly formed on the surface of the ZIF material.

[0199] The rest are the same as in Example 1.

[0200] Comparative Example 2

[0201] Comparative Example 2 is substantially the same as Example 1, except that:

[0202] In <Preparation of composite materials>, the type of matrix was changed, and ordinary carbon materials (such as biomass carbon: chitosan, chitin, etc.) were used as the matrix to obtain a porous carbon base material through high temperature and acid washing; the rest was the same as Example 1.

[0203] Comparative Example 3

[0204] Comparative Example 3 is substantially the same as Example 1, except that:

[0205] In <Preparation of Composite Materials>, the ZIF material and the rigid material layer are eliminated, that is, ordinary alumina ceramic material is used as the composite material.

[0206] Comparative Example 4

[0207] Comparative Example 4 is substantially the same as Example 1, except that:

[0208] In <Preparation of Composite Materials>, the ceramic material layer is eliminated, that is, a rigid material layer is coated on the surface of the ZIF material to obtain a composite material.

[0209] Performance Testing

[0210] 1. The composite materials and diaphragms prepared in the above embodiments and comparative examples were tested for performance, including:

[0211] (1) Specific surface area test: Take the same mass of composite material samples prepared in the above embodiments and comparative examples respectively, place each composite material sample in a BET tester, introduce nitrogen (N2), and measure the specific surface area by N2 adsorption method. The specific surface area of ​​the material is characterized by the amount of gas adsorption. That is, after introducing nitrogen for a period of time, the specific surface area of ​​the composite material is represented by the amount of gas adsorption collected together.

[0212] (2) Maximum compaction density test: Because the rigid porous alumina ceramic powder of the present invention has good structural stability, the maximum pressure that can be withstood in the process of rolling the positive electrode sheet to increase the compaction density without breaking the structure, the standard test method is to extrude a certain amount of the composite powder samples prepared in each embodiment and comparative example under different pressures, such as 3.1 g / cm3 、3.2g / cm 3 、3.3g / cm 3 、3.4g / cm 3 、3.5g / cm 3 、3.6g / cm 3 Under the compaction of the same pressure (keep using different pressure rollers to press the composite powder sample until the composite material is observed to be broken), after the extrusion test, the SEM and CP of the cross section are used to determine whether the composite material is broken.

[0213] (3) Liquid retention test: Take the same area of ​​the diaphragms prepared in the embodiments and comparative examples, immerse them in the electrolyte for a certain period of time (such as 1 h to 4 h), and finally weigh the difference in mass before and after weighing to characterize the liquid retention performance.

[0214] (4) Diaphragm thermal shrinkage (shrinkage rate) test: The diaphragms prepared in each embodiment and comparative example are cut into 10*10CM strips, clamped with a clamp, placed in a 100°C environment for 8 hours, the length of the diaphragm is measured, and the shrinkage rate is calculated = (length after test - length before test) / length before test * 100%. This test can characterize the stability of the ceramic coating on the diaphragm strength.

[0215] The test results are shown in Table 1.

[0216] Table 1 Test results of membrane performance of various embodiments and comparative examples

[0217]

[0218] It can be seen from the data in Table 1 that, by comparing Examples 1 to 9 with Comparative Examples 1 to 4, the composite material prepared by the method described in the embodiments of the present invention and the diaphragm using the composite material have a larger specific surface area, increase the liquid retention capacity of the electrolyte, and also improve the thermal stability of the diaphragm and reduce its thermal shrinkage.

[0219] In addition, through the analysis and comparison of Example 1 and Example 3, it can be seen that Example 3 reduces the carbonization temperature of the rigid material layer, and the carbonization temperature of the rigid material layer determines the structural strength and stability of the material. Lowering the carbonization temperature will reduce the tempering strength, which will affect the compaction density of the material, that is, reduce the compaction density of the material, making it easy to break.

[0220] By comparing the analysis of Example 1 with Comparative Example 1, it can be seen that the rigid material layer is eliminated in Comparative Example 1, the compaction density is reduced, and the material is easier to break, which shows that by setting a rigid material layer on the surface of the substrate, the compaction density of the material can be increased and the structural strength of the material can be increased. By comparing the analysis of Example 1 with Comparative Example 2, it can be seen that the ordinary carbon material as the substrate has, on the one hand, a lower porosity than the ZIF substrate, and on the other hand, its stability is lower than the ZIF material, which reduces the specific surface area, compaction density and liquid retention.

[0221] Through the analysis and comparison of Example 1 and Comparative Example 3, it can be seen that Comparative Example 3 uses ordinary alumina ceramic materials. Compared with ordinary alumina ceramics, the composite material (porous rigid alumina ceramic) provided by the embodiment of the present invention greatly increases the specific surface area and the amount of electrolyte retained, and the structural strength is not reduced. Through the analysis and comparison of Example 1 and Comparative Example 4, it can be seen that Comparative Example 4 cancels the ceramic material layer. Through the diaphragm heat shrinkage test, it can be seen that the ordinary diaphragm provided by Comparative Example 4 is not resistant to high temperatures and has a high shrinkage rate. The surface of the embodiment of the present invention is coated with a ceramic coating, which can significantly improve the mechanical strength of the diaphragm and reduce the thermal shrinkage. Therefore, the thermal shrinkage of the diaphragm coated with a porous rigid coating (coated with a ceramic coating) of the present invention has not deteriorated, but is slightly better. This is mainly because the porous design is easier to absorb heat and dissipate heat.

[0222] 2. The performance tests were performed on the batteries prepared in the above embodiments and comparative examples, including:

[0223] (1) Rate retention rate: The battery cell is tested at different charge and discharge rates, including:

[0224] 1. Charge at 0.5C constant current to 4.25V, then charge at 4.25V constant voltage to 0.05C; 2. Let stand for 30 minutes; 3. Discharge at 0.5C current to the lower limit voltage of 2.5V; 4. Let stand for 30 minutes; then repeat steps 1-4 in sequence, and discharge at 1C, 2C, 3C, and 5C currents. Then, 5C rate retention rate = 5C discharge capacity / 1C discharge capacity.

[0225] (2) 1C cycle test: Perform charge and discharge tests according to the standard test process 0.5C / 1C system until the discharge capacity of the battery is lower than 80% of the initial capacity. The test is stopped and the capacity retention rate after 500 cycles is recorded.

[0226] The specific process of the 1C cycle test includes: leaving the battery at 25°C for 30 minutes, charging at 0.5C constant current to 4.25V, then charging at 0.05C constant voltage, leaving it at 30 minutes, discharging at 1C to 2.5V, recording the discharge capacity of the first cycle as the initial capacity, and stopping the test until the discharge capacity of the battery is lower than 80% of the initial capacity, recording the capacity retention rate after 500 cycles, then the capacity retention rate of the 500th cycle = discharge capacity of the 500th cycle / discharge capacity of the first cycle.

[0227] (3) Energy density test: The battery was placed in a 25°C environment for 30 min, charged at 0.5C constant current to 4.25 V, then charged at 0.05C constant voltage, placed for 30 min, and discharged at 1C to 2.5 V. The discharge capacity and discharge voltage data of the test were collected. Then, 1C energy density = 1C discharge capacity * 1C discharge average voltage / total weight of the battery.

[0228] (4) Gas volume test: The gas volume test is carried out using the water displacement method and a volume tester. Based on the initial weight m1 of the battery cell and the mass m2 immersed in water, the buoyancy of the battery cell in water = ρgV, which is proportional to the weight. The density ρ and mass acceleration g of water are known, so the volume V = (m1-m2) / ρg.

[0229] (5) Hot box test: According to the 0.5C / 1C test, fully charge the battery cell, place it in a hot box, and heat it to 130°C at a rate of 5°C per minute and hold it for half an hour. Observe for half an hour. If there is no fire or smoke, continue to heat it at a rate of 5°C and test the failure temperature every 5°C until the battery fails. The temperature at this time is the failure temperature.

[0230] (6) Power performance test (DCR test): 1. Charge at 0.5C constant current to 4.25V, then charge at 4.25V constant voltage to 0.05C; 2. Let stand for 30 minutes; 3. Discharge at 0.5C current for 60 minutes, then discharge at 5C current for 30 seconds, and record the voltage at the end of the test. A higher voltage indicates faster lithium ion transmission, so the power performance is better.

[0231] The test results are shown in Table 2.

[0232] Table 2 Battery performance test results of various embodiments and comparative examples

[0233]

[0234] It can be seen from the data in Table 2 that, by comparing Examples 1 to 9 with Comparative Examples 1 to 4, the composite material prepared by the method described in the embodiment of the present invention improves the structural stability of the material, increases the structural strength, and can increase the compaction density and improve the energy density of the battery in practical lithium batteries; and the battery using the composite material provided by the embodiment of the present invention can improve the rate performance, and can also improve the cycle performance, power performance, etc. of the battery to a certain extent.

[0235] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0236] The basic principle of the present invention is described above in conjunction with specific embodiments. However, it should be pointed out that the advantages, strengths, effects, etc. mentioned in the present invention are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. must be possessed by each embodiment of the present invention. In addition, the specific details disclosed above are only for the purpose of illustration and facilitation of understanding, rather than limitation, and the above details do not limit the present invention to being implemented by adopting the above specific details.

[0237] It should be noted that the term "and / or" or " / " used in this document is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. The singular forms of "a", "the" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0238] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0239] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite material, characterized in that: The composite material comprises: A substrate, the substrate comprising a ZIF material; A rigid material layer covering at least a portion of the surface of the substrate; The ceramic material layer is coated on at least a portion of the surface of the rigid material layer.

2. The composite material according to claim 1, characterized in that The ZIF material includes at least one of ZIF-8, ZIF-67, ZIF-90, ZIF-71, ZIF-5, ZIF-93, ZIF-97 or ZIF-20; And / or, the average particle size of the ZIF material is 0.5 μm to 2 μm.

3. The composite material according to claim 1, characterized in that The rigid material layer includes at least one of titanium carbide, tungsten carbide, zirconium carbide or titanium nitride; And / or, the thickness of the rigid material layer is 0.2 μm to 0.8 μm.

4. The composite material according to claim 1, characterized in that The ceramic material layer includes at least one of aluminum oxide, zirconium oxide, chromium oxide, cobalt oxide, nickel oxide, zinc oxide, titanium oxide, manganese oxide or yttrium oxide; And / or, the thickness of the ceramic material layer is 0.5 μm to 2 μm.

5. The composite material according to any one of claims 1 to 4, characterized in that: The mass ratio of the substrate, the rigid material layer and the ceramic material layer is (5-20): (1-5): (80-95).

6. A method for preparing a composite material, characterized in that: The steps include: Preparation of ZIF precursor; The ZIF precursor is mixed with a rigid material precursor solution, a reactive gas is introduced, and a first heating treatment is performed to obtain a ZIF material coated with a rigid material layer; The ZIF material coated by the rigid material layer is immersed in an alkaline solution to obtain a precursor, the precursor is mixed with a ceramic material precursor solution, and a second heating treatment is performed to coat the ceramic material layer on the surface of the rigid material layer.

7. The method for preparing a composite material according to claim 6, characterized in that: The preparation of the ZIF precursor comprises: mixing a metal salt, an imidazole raw material and a solvent to obtain a mixed solution, reacting the mixed solution at 100° C. to 200° C. for 1 h to 6 h to obtain a ZIF precursor; and / or, the rigid material precursor solution includes at least one of a titanium tetrachloride solution, a tungsten tetrachloride solution or a zirconium chloride solution; and / or, the concentration of the rigid material precursor solution is 0.01 to 0.5 mol / L; And / or, the reactive gas is suitable for reacting with the rigid material precursor, and the reactive gas includes at least one of an alkane gas or ammonia; wherein the alkane gas includes at least one of methane, ethane, propane or butane; And / or, the temperature of the first heat treatment is 800° C. to 1400° C., and the time is 2 h to 6 h.

8. The method for preparing a composite material according to claim 6 or 7, characterized in that: The alkaline solution includes at least one of a sodium hydroxide solution or a potassium hydroxide solution; and / or, the concentration of the alkaline solution is 0.5 to 1 mol / L; And / or, the mixing of the precursor with the ceramic material precursor solution comprises: soaking the precursor in the ceramic material precursor solution for 0.5h to 5h; and / or, the ceramic material precursor solution includes at least one of an aluminum salt solution, a zirconium salt solution, a chromium salt solution, a cobalt salt solution, a nickel salt solution, a zinc salt solution, a titanium salt solution, a manganese salt solution or a yttrium salt solution; And / or, the temperature of the second heat treatment is 1000° C. to 1500° C., and the time is 2 h to 6 h.

9. A diaphragm, characterized in that: It includes a base film and a ceramic coating disposed on at least one side of the base film; The ceramic coating comprises the composite material according to any one of claims 1 to 5 or the composite material prepared by the method according to any one of claims 6 to 8, and a binder; The mass ratio of the composite material to the binder is (90-95):(5-10).

10. A battery, characterized in that: The diaphragm according to claim 9 is included.

Citation Information

Patent Citations

  • Titanium dioxide coated carbon-cobaltosic oxide composite material as well as preparation method and application thereof

    CN111613787A

  • Battery diaphragm, preparation method thereof and battery

    CN113113721A

  • Metal-N co-doped / porous carbon oxygen reduction catalyst coated with mesoporous silica shell layer and preparation method and application thereof

    CN113437310A

  • Inorganic-organic composite solid electrolyte lithium battery and preparation method thereof

    CN115642296A

  • Composite coating diaphragm for ion battery and preparation method of composite coating diaphragm

    CN116435709A