Moisture power generation device based on vermiculite nanosheet film and preparation method thereof

By using the combination of vermiculite nanosheet film and electron conduction layer in moisture power generation technology, the problems of complex material preparation, high cost and poor stability in the prior art are solved, and efficient and stable moisture power generation effect is achieved. And simplifies the production process.

CN118944489APending Publication Date: 2024-11-12SHUIFU ENERGY TECH (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411002488.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing moisture power generation technology materials are complex in preparation and high in cost, the power generation efficiency is greatly affected by environmental humidity, poor stability, and the component structure design is complex, which is not conducive to large-scale production and application.

Method used

Using vermiculite nanosheet film as functional layer, combining electron-conducting layer and polymer electrolyte, a simple structure and preparation method is designed, including bottom electrode, functional layer, hygroscopic layer and top electrode, using corrosion-resistant metals and conductive polymers, through The screen printing process simplifies the preparation process.

Benefits of technology

It improves the power generation efficiency and stability of moisture power generation devices, reduces the impact on environmental humidity, simplifies the preparation process, reduces maintenance costs, and realizes independent structures between materials, avoiding short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118944489A_ABST
    Figure CN118944489A_ABST
Patent Text Reader

Abstract

The invention relates to a moisture power generation device based on a vermiculite nanosheet film and a preparation method thereof, the moisture power generation device comprises a functional layer, a moisture absorption layer and a top electrode, and the functional layer comprises a bottom electrode and a power generation sub-layer; the bottom electrode adopts a carrier coated with a conductive sub-layer, the power generation sub-layer adopts a vermiculite nanosheet film printed on the conductive sub-layer, a part of the power generation sub-layer on the bottom electrode is wiped off to expose the conductive sub-layer as an electrode, and the moisture absorption layer adopts a carrier which is placed on the power generation sub-layer and is soaked with a polymer electrolyte. The top electrode is placed on the moisture absorption layer, and the moisture absorption layer and the top electrode are narrower than the functional layer, so that the functional layer is exposed. Compared with the prior art, the influence of environment humidity on the power generation efficiency is small, the stability is good, short circuit caused by mistaken touch between materials is prevented through the multi-layer mutually-independent structure, single-layer local damage can be replaced independently, and the maintenance cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wet gas power generation, and relates to a wet gas power generation device based on vermiculite nanosheet film and a preparation method thereof. Background Art

[0002] With the development of science and technology, human demand for energy is growing, while the reserves of traditional non-renewable energy such as fossil fuels are limited, and they will cause a lot of environmental pollution during use. Therefore, the development of new renewable energy has become one of the hot spots of current research. Among them, wet gas power generation is a new type of energy conversion technology, which uses moisture in the environment (such as water vapor) as energy and converts it into electrical energy through specific materials and devices. This technology has the advantages of environmental protection, renewable, high energy density, etc., and has broad application prospects.

[0003] Existing wet gas power generation technology mainly uses special materials to absorb and convert the chemical potential energy in wet gas into electrical energy. However, the preparation process of these materials is complicated and costly, and their power generation efficiency is greatly affected by the ambient humidity and has poor stability.

[0004] The existing wet gas power generation technology has the following major problems: First, the materials used for wet gas power generation are mostly nano-scale microstructures, and their preparation process is complex and costly, which is not conducive to large-scale production and application; second, the power generation efficiency of these materials is greatly affected by the ambient humidity and has poor stability, which limits their application in real life; third, the components have poor stability and are prone to open circuits, short circuits, material aging, etc., and the maintenance cost is high; finally, the structural design and preparation methods of existing wet gas power generation devices are relatively complex, which is not conducive to simplification and optimization.

[0005] Patent CN117578911A discloses a moisture power generation device based on vermiculite nanosheet film and a preparation method thereof, wherein the moisture power generation device comprises a bottom electrode, a functional layer, a hygroscopic layer and a top electrode, wherein the functional layer is covered by the hygroscopic layer and the bottom electrode respectively; the functional layer adopts the vermiculite nanosheet film, and the hygroscopic layer adopts a polymer electrolyte; the method comprises: attaching the vermiculite nanosheet film to the bottom electrode after hydrophilic treatment to obtain the functional layer; drop-coating the polymer electrolyte solution on the functional layer, and obtaining the hygroscopic layer after drying; and pasting the top electrode on the hygroscopic layer to obtain the moisture power generation device based on the vermiculite nanosheet film. However, the patent uses metal copper electrodes, which will corrode rapidly in a high humidity environment and produce copper rust; high current and voltage involve metal redox phenomena, and most of the current comes from redox reactions, not simple moisture power generation, so it will cause rapid corrosion and last for a short time; the manufacturing process is relatively complicated, with many steps, requiring the use of heating, vacuum and other equipment, and the yield is low; there is no clear physical separation between the components, which is prone to accidental contact and short circuits. After local damage, the entire component will fail, increasing maintenance costs; as a laboratory component, the packaging is not completed, and the restrictions on usage conditions are relatively obvious. Summary of the invention

[0006] The purpose of the present invention is to provide a moisture power generation device based on vermiculite nanosheet film and a preparation method thereof in order to overcome at least one defect of the above-mentioned prior art. The power generation efficiency of the present invention is less affected by the ambient humidity and has good stability. The multi-layer independent structure prevents accidental contact between materials to form a short circuit. Local damage to a single layer can be replaced separately, reducing maintenance costs.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] One of the technical solutions of the present invention is to provide a moisture power generation device based on vermiculite nanosheet film, the moisture power generation device comprises a functional layer, a moisture absorption layer and a top electrode, the functional layer comprises a bottom electrode and an electron-emitting layer;

[0009] The bottom electrode uses a carrier coated with a conductive sublayer, the light-emitting sublayer uses a vermiculite nanosheet film printed on the conductive sublayer, a portion of the light-emitting sublayer on the bottom electrode is wiped off to expose the conductive sublayer as an electrode, the hygroscopic layer uses a carrier soaked in a polymer electrolyte placed on the light-emitting sublayer, the top electrode is placed on the hygroscopic layer, the hygroscopic layer and the top electrode are narrower than the functional layer to expose the functional layer, so that the moisture power generation device can effectively absorb water molecules in the air, and the asymmetric upper and lower electrodes can form a humidity gradient inside the moisture power generation device.

[0010] Furthermore, the material of the conductive sublayer is selected from one or more of carbon nanotubes (CNTs), corrosion-resistant metals such as nickel, silver, gold, platinum, and conductive polymers such as polyaniline; the carrier is selected from one or more supporting materials of quick-drying cloth, non-woven fabric, cotton cloth, and bamboo fiber; the polymer electrolyte is selected from one or more of polydiallyldimethylammonium chloride (PDDA), sodium polystyrene sulfonate (PSS), and polyamide (PA); the material of the top electrode is selected from one or more of silver-plated steel, corrosion-resistant metals such as nickel, silver, gold, platinum, alloys, and conductive polymers such as polyaniline.

[0011] Furthermore, the thickness ratio of the carrier, the conductive sublayer and the vermiculite nanosheet film is (10-50):(2-20):(1-10), 5-25% of the area of ​​the functional layer of the electronic layer on the bottom electrode is wiped off, and the area of ​​the hygroscopic layer is 30-50% of the area of ​​the functional layer.

[0012] As a preferred technical solution, casings are provided on both sides of the wet gas power generation device for fixation.

[0013] As a preferred technical solution, outer shells are respectively provided on the outer sides of the bottom electrode and the top electrode for fixing, and two ends of the bottom electrode and the top electrode are respectively exposed from the outer shells.

[0014] As a preferred technical solution, the shell is made of a corrosion-resistant polymer selected from polyvinyl alcohol (PVA), polyethylene (PE), and polyethylene terephthalate (PET) by 3D printing, firing or pressing technology.

[0015] One of the technical solutions of the present invention is to provide a method for preparing the moisture power generation device based on vermiculite nanosheet film, the method comprising the following steps:

[0016] S1. Preparation of vermiculite slurry,

[0017] Add dispersant to submerge the vermiculite, and disintegrate it by ultrasonication intermittently. When most of the vermiculite is broken into vermiculite slurry and no large particles are visible to the naked eye, the vermiculite slurry is centrifuged for cleaning and dried;

[0018] S2, functional layer production,

[0019] The conductive sub-layer material is brushed on one side of the carrier, dried, and the surface is solidified to obtain a bottom electrode, the bottom electrode surface is plasma cleaned, an adhesive is added to the vermiculite slurry, mixed and stirred evenly, the mixed slurry is screen-printed on the surface of the conductive sub-layer, and dried to obtain an electronically emitting layer printed on the bottom electrode, that is, a functional layer;

[0020] S3, moisture absorption layer production,

[0021] The surface of the carrier is plasma cleaned, a polymer electrolyte is added to a solvent and mixed and stirred evenly to obtain a polymer electrolyte solution, the carrier is placed in the polymer electrolyte solution, and after being completely soaked, the carrier is taken out and allowed to stand until the polymer electrolyte solution no longer drips from the surface, and then dried to obtain a hygroscopic layer;

[0022] S4, assembly,

[0023] The functional layer is partially wiped off to expose the conductive layer as an electrode, the hygroscopic layer is placed on the functional layer, and the top electrode is placed on the hygroscopic layer as an electrode to obtain a moisture power generation device based on vermiculite nanosheet film.

[0024] Furthermore, in step S1, the dispersant is water;

[0025] The mass / volume ratio of vermiculite to dispersant is (1-5 g):15 mL, and the mass concentration of the vermiculite slurry is 10-15 g / L.

[0026] Furthermore, in step S2, the adhesive is sodium alginate;

[0027] The solid content of the slurry of the conductive sublayer material is 10-20%, and the ratio of the unit area usage to the thickness of the conductive sublayer is (0.2-1mL / cm 2 ):(0.1-1mm);

[0028] The volume / molar ratio of vermiculite slurry to adhesive is (50-70mL):1g, and the ratio of unit area usage of mixed slurry to the thickness of the electron-emitting layer is (0.02-0.1mL / cm 2 ):(0.1-1mm).

[0029] Furthermore, in step S3, the solvent is water;

[0030] The volume concentration of the polymer electrolyte solution is 40-80%.

[0031] Furthermore, in step S1, the power of the intermittent ultrasonic crushing is 800-1200W, the temperature is 0-20°C, the total time is 8-14h, the single time is 1-3h, and the water is prevented from boiling over, and the number of times is 5-9 times;

[0032] The speed of centrifugal washing is 2000-6000rpm, the temperature is room temperature, the time is 5-15min, the upper clear liquid is removed after each washing, the number of times is 3-7 times, and the sodium and magnesium ions contained in the vermiculite are completely removed;

[0033] The drying temperature is 60-100°C and the drying time is 8-12h.

[0034] Furthermore, in step S2, the drying temperature of the conductive sublayer is 40-80° C. and the drying time is 1-3 hours;

[0035] The power of plasma surface cleaning is 80-120W, the temperature is room temperature, and the time is 2-10min;

[0036] The mixing temperature is room temperature and the mixing time is 20-40 minutes;

[0037] The drying temperature is 40-80°C and the drying time is 0.5-1.5h.

[0038] Further, in step S3, the power of plasma surface cleaning is 80-120W, the temperature is room temperature, and the time is 2-10min;

[0039] The mixing temperature is room temperature and the mixing time is 20-40 minutes;

[0040] The soaking temperature is room temperature and the soaking time is 0.5-2h;

[0041] The temperature of the static state is room temperature, and the time is 10-30 minutes;

[0042] The drying temperature is 40-60°C and the drying time is 0.5-1.5h.

[0043] The present invention uses vermiculite nanosheet film as the functional layer: since vermiculite nanosheet has good hydrophilicity and ionic conductivity, it can effectively convert the chemical potential energy of water vapor into electrical energy. At the same time, its stable structural characteristics also ensure the stability of the wet gas power generation material and reduce the impact of environmental humidity on its power generation efficiency.

[0044] The present invention uses a polymer electrolyte as a hygroscopic layer: the polymer electrolyte has good hygroscopicity and ionic conductivity, can effectively absorb water vapor in the environment, and transfer it to the functional layer, thereby realizing wet gas power generation. The hygroscopic layer can use polydiallyldimethylammonium chloride, sodium polystyrene sulfonate, polyamide and other substances containing multiple functional groups and easy to dissociate. The dissociated ions can move as carriers, thereby increasing the current density. At the same time, the use of polymer electrolytes also simplifies the preparation process of wet gas power generation materials and reduces the preparation cost.

[0045] The present invention adopts a simple structural design and preparation method: the moisture power generation device of the present invention includes a bottom electrode, a functional layer, a moisture absorption layer and a top electrode, has a simple structure, and a relatively simple preparation method. It uses a screen printing process to increase the yield over a large area while reducing the cost. This simple structural design and preparation method makes the moisture power generation device easier to implement and optimize.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] (1) The present invention uses vermiculite nanosheet film as the functional layer. Compared with existing metal-organic framework materials (MOFs), carbon nanotubes and other materials, its preparation process is simpler and the cost is lower, which is conducive to large-scale production and application;

[0048] (2) The power generation efficiency of the wet gas power generation device of the present invention is less affected by the environmental humidity and has good stability. This is because the vermiculite nanosheet film has good hygroscopicity and dehumidification properties and can stably perform wet gas power generation under different humidity environments;

[0049] (3) The structural design and preparation method of the wet gas power generation device of the present invention are simpler and easier to implement; the device is manufactured using a screen printing process; this method greatly simplifies the preparation process of the wet gas power generation device and reduces the difficulty of preparation;

[0050] (4) The multi-layer independent structure of the present invention prevents accidental contact between materials to form a short circuit, and local damage to a single layer can be replaced separately, reducing maintenance costs;

[0051] (5) The wet gas power generation device of the present invention can simply and efficiently realize the continuous conversion of the chemical potential energy of water vapor into electrical energy, thereby improving the utilization efficiency of energy and helping to promote the development of renewable energy. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 Schematic diagram of the main structure of a moisture power generation device based on vermiculite nanosheet film in an embodiment of the present invention;

[0053] Figure 2 It is a schematic diagram of a top view of the structure of a moisture power generation device based on vermiculite nanosheet film without a housing in an embodiment of the present invention;

[0054] Figure 3 This is a current diagram of the continuous power generation effect of the wet gas power generation device based on vermiculite nanosheet film in an embodiment of the present invention at 75% humidity;

[0055] Figure 4 This is a voltage diagram of the continuous power generation effect of the wet gas power generation device based on vermiculite nanosheet film in an embodiment of the present invention at 75% humidity;

[0056] Figure 5 This is a current diagram of the continuous power generation effect of the wet gas power generation device in the comparative example of the present invention at 75% humidity;

[0057] Figure 6 This is a current diagram of the continuous power generation effect of the wet gas power generation device based on vermiculite nanosheet film in an embodiment of the present invention at 65% humidity;

[0058] Figure 7This is a current diagram of the continuous power generation effect of the moisture power generation device based on vermiculite nanosheet film at 55% humidity in an embodiment of the present invention.

[0059] Description of the markings in the figure:

[0060] 1—functional layer, 11—bottom electrode, 12—electron-emitting layer, 2—hygroscopic layer, 3—top electrode, 4—outer shell. DETAILED DESCRIPTION

[0061] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0062] Unless otherwise specified, the equipment used in the following examples are all conventional equipment in the art; the reagents used are all commercially available products or prepared by conventional methods in the art unless otherwise specified. Anything not described in detail in the following examples can be achieved by conventional experimental means in the art.

[0063] Example:

[0064] A moisture power generation device based on vermiculite nanosheet film, such as Figure 1 and Figure 2 As shown, from bottom to top, it is composed of a functional layer 1, a moisture absorbing layer 2 and a top electrode 3 in sequence, and the functional layer 1 is composed of a bottom electrode 11 and an electron-emitting layer 12 in sequence from bottom to top, and a housing 4 is provided on both sides of the moisture power generation device for fixing;

[0065] The bottom electrode 11 is made of quick-drying cloth coated with carbon nanotubes (CNTs), the electron-emitting layer 12 is made of vermiculite nanosheet film printed on CNTs, part of the electron-emitting layer 12 on the bottom electrode 11 is wiped off to expose the CNTs as electrodes, the hygroscopic layer 2 is made of quick-drying cloth soaked with polydiallyldimethylammonium chloride (PDDA) placed on the electron-emitting layer 12, the top electrode 3 is made of silver-plated steel bars placed on the hygroscopic layer 2, the hygroscopic layer 2 and the top electrode 3 are narrower than the functional layer 1 to expose the functional layer 1, so that the moisture power generation device can effectively absorb water molecules in the air, the asymmetric upper and lower electrodes can form a humidity gradient inside the moisture power generation device, the outer sides of the bottom electrode 11 and the top electrode 3 are respectively provided with shells 4 for fixing, the bottom electrode 11 and the top electrode 3 are respectively exposed at both ends of the shell 4, and the shell 4 is made of polyvinyl alcohol (PVA) 3D printing;

[0066] The material of quick-drying cloth is modified polyester, including polyester, nylon, polypropylene, as well as polyester-spandex, nylon-spandex and other ingredients.

[0067] The preparation method of the above-mentioned vermiculite nanosheet film-based wet gas power generation device comprises the following specific steps:

[0068] S1. Preparation of vermiculite slurry,

[0069] Take 60g of vermiculite (Weijia Gardening Store, Suining County, 9-12mm white vermiculite), add 300mL of deionized water to submerge the vermiculite, place it in an ultrasonic crusher, and crush it intermittently at 1000W for 12h;

[0070] The crushing process requires the use of ice packs to cool down to 10°C, and the single time is 1.7 hours to prevent the water from boiling and overflowing. This process is repeated 7 times;

[0071] After most of the vermiculite is crushed into vermiculite slurry and no large particles are visible to the naked eye, it is placed in a centrifuge and cleaned at 4000 rpm and room temperature for 10 minutes;

[0072] After each cleaning, the supernatant was removed. This process was repeated 5 times to completely remove the sodium and magnesium ions contained in the vermiculite.

[0073] The product was collected in a beaker, dried at 80°C for 10 h, deionized water was added to dissolve the vermiculite, and the concentration was adjusted. After the adjustment, the mass concentration of the vermiculite slurry was 12 g / L, and the vermiculite slurry was prepared. The beaker was sealed and set aside for use.

[0074] S2, production of functional layer 1,

[0075] Cut a piece of 20×16cm×1.5mm quick-drying cloth (Wujiang Hehui Textile Co., Ltd., HHJ020) and apply 150mL (0.47mL / cm 2 ), CNT slurry with an average solid content of 12% (Beijing Tanyang Technology Co., Ltd., eYINK-W-176A), dried at 60°C for 2h, the surface solidified, and a bottom electrode 11 coated with a 0.5mm thick conductive sublayer was obtained;

[0076] The bottom electrode 11 is placed in a plasma surface cleaning machine, and the surface is treated for 6 minutes at 100W and room temperature;

[0077] Take 30mL of vermiculite slurry, add 0.5g of sodium alginate (Xilong Scientific Co., Ltd., chemically pure), mix and stir at room temperature for 30min, and then take 15mL (0.047mL / cm 2 ) Mix the slurry, use screen printing to cover the CNT surface, dry at 60° C. for 1 h, and obtain a 0.2 mm thick electron-emitting layer 12 printed on the bottom electrode 11, and the functional layer 1 is completed;

[0078] S3, making the moisture absorbing layer 2,

[0079] Cut a piece of quick-drying cloth of 10×14cm×1.5mm, put it into the plasma surface cleaning machine, 100W, room temperature surface treatment for 6 minutes;

[0080] Take 30 mL of PDDA, add 20 mL of deionized water, mix and stir at room temperature for 30 min to form a 60% uniform PDDA solution;

[0081] Put the quick-drying cloth into the PDDA solution, soak it completely at room temperature for 1 hour, then take it out and let it stand at room temperature for 15 minutes. After the PDDA solution stops dripping on the surface, dry it at 50°C for 1 hour. The moisture absorption layer 2 is completed.

[0082] S4, assembly,

[0083] Functional layer 1 was cut into 2 × 8 cm units, and 2 × 1 cm (12.5% ​​of the area of ​​functional layer 1) was erased to expose the CNT as the positive electrode;

[0084] The hygroscopic layer 2 was cut into 1×7 cm (43.75% of the area of ​​the functional layer 1) and placed on the functional layer 1. A 1×8 cm silver-plated steel bar top electrode 3 was placed on the top as the negative electrode. The 3D printed shell 4 was used to fit and fix the vermiculite nanosheet film. The moisture power generation device based on the vermiculite nanosheet film was assembled.

[0085] The long-term output test of the above-mentioned vermiculite nanosheet film-based wet gas power generation device is carried out in the following specific steps:

[0086] A closed desiccator was used, and a saturated salt solution was placed inside to stabilize the humidity (75% saturated sodium chloride solution, 65% saturated ammonium nitrate solution, 55% saturated magnesium nitrate solution). The device was placed inside and a DMM6500 electric meter produced by KEITHLEY was used to continuously record the readings and observe the power generation of the device.

[0087] like Figure 3 As shown, it can be seen that the current stability in this embodiment is extremely good. At 75% humidity and 20°C, the output is continuously output for more than 100 hours and the current can be stabilized at 70μA after 10,000s, and then slowly drops to 60μA after 70,000s. The current is relatively high in the early stage, which is caused by the movement of moisture; in the later stage, the moisture is saturated, the carrier movement rate decreases, and finally maintains a stable current.

[0088] like Figure 4 As shown, it can be seen that the voltage stability in this embodiment is good. At 75% humidity and 20°C temperature, the voltage can be stabilized at 0.5V after 30,000s after continuous output for more than 15h, and the rated power of the single chip can be stabilized to 20μW. During the voltage test, the circuit is in an open circuit state, and the charge accumulates to both sides with the carriers, and finally reaches a saturation state.

[0089] By connecting five devices in series to form a module, the voltage can be increased and stabilized to 3.0V.

[0090] After the two sets of modules are connected in parallel, the output power is stable at 120μW when a 1000Ω load is added and the humidity is 75%, and the LED light stays on stably for more than 24 hours.

[0091] Comparative Example:

[0092] A moisture power generation device is basically the same as the embodiment, except that the bottom electrode 11 is a copper electrode, there is no vermiculite nanosheet film electron-emitting layer 12, the moisture absorption layer 2 is impregnated with sodium polystyrene sulfonate (PSS), and the top electrode 3 is an aluminum electrode.

[0093] like Figure 5 As shown, it can be seen that the current and voltage in the comparative example both show obvious attenuation, a circuit breaker appears after 800s, and the electrode is corroded.

[0094] like Figure 6 As shown, it can be seen that in this embodiment, at 65% humidity and 20°C temperature, the current can be stabilized at 75μA after continuous output for more than 100 hours. The device is in an ideal operating state, the carrier movement rate is close to constant, and the current density is relatively stable.

[0095] like Figure 7 As shown, it can be seen that in this embodiment, at 55% humidity and 20°C temperature, the current can be stabilized at 40μA after continuous output for more than 100h and gradually increased to 60μA after 30000s. The humidity is low, the device is drier in the early stage of the test, and the carrier movement rate is slower; after absorbing moisture and reaching stability in the later stage, the carrier movement rate is constant and the current reaches the stable area.

[0096] The present invention uses silver-plated steel bars and carbon as electrodes to prevent metal corrosion; eliminates redox reactions, and uses moisture to generate electricity, which can be maintained for a long time; uses quick-drying cloth as a moisture-wicking layer, and since the quick-drying cloth itself is an excellent moisture-wicking material, it can greatly increase the moisture entry and exit rate and increase the current; the main component of the quick-drying cloth is modified polyester, which is very stable in the natural environment, is not affected by factors such as rain, sunlight, and airflow, and can be used sustainably without maintenance; the structure is a six-layer independent structure, which prevents short circuits caused by accidental touching between materials, solves the problem of easy short circuits of similar components, and local damage to a single layer can be replaced separately, which will not greatly affect the use of the components and reduces maintenance costs; 3D printed components are used for packaging to prevent uneven contact of components, and can be exposed to outdoor use, greatly improving stability.

[0097] The device of the present invention can continuously and stably convert the chemical potential energy of water vapor into electrical energy under different humidity environments of 45-90%.

[0098] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A wet gas power generation device based on vermiculite nanosheet film, characterized in that: The moisture power generation device comprises a functional layer (1), a moisture absorption layer (2) and a top electrode (3), wherein the functional layer (1) comprises a bottom electrode (11) and an electron-emitting layer (12); The bottom electrode (11) uses a carrier coated with a conductive sublayer, the electron-emitting layer (12) uses a vermiculite nanosheet film printed on the conductive sublayer, a portion of the electron-emitting layer (12) on the bottom electrode (11) is wiped off so that the conductive sublayer is exposed as an electrode, the hygroscopic layer (2) uses a carrier soaked in a polymer electrolyte placed on the electron-emitting layer (12), the top electrode (3) is placed on the hygroscopic layer (2), and the hygroscopic layer (2) and the top electrode (3) are narrower than the functional layer (1) so that the functional layer (1) is exposed.

2. A moisture power generation device based on vermiculite nanosheet film according to claim 1, characterized in that: The material of the conductive sublayer is selected from one or more of carbon nanotubes, nickel, silver, gold, platinum, and polyaniline; the carrier is selected from one or more supporting materials of quick-drying cloth, non-woven fabric, cotton cloth, and bamboo fiber; the polymer electrolyte is selected from one or more of polydiallyldimethylammonium chloride, sodium polystyrene sulfonate, and polyamide; and the material of the top electrode (3) is selected from one or more of silver-plated steel, nickel, silver, gold, platinum, and polyaniline.

3. A moisture power generation device based on vermiculite nanosheet film according to claim 1, characterized in that: The thickness ratio of the carrier, the conductive sublayer and the vermiculite nanosheet film is (10-50):(2-20):(1-10), 5-25% of the area of ​​the functional layer (1) is wiped off the electron-emitting layer (12) on the bottom electrode (11), and the area of ​​the hygroscopic layer (2) is 30-50% of the area of ​​the functional layer (1).

4. A method for preparing a moisture power generation device based on vermiculite nanosheet film according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: S1. Preparation of vermiculite slurry, Add a dispersant to submerge the vermiculite, break it by ultrasonication intermittently to form vermiculite slurry, wash the vermiculite slurry by centrifugation, and dry it; S2, production of functional layer (1), The conductive sub-layer material is brushed onto one side of the carrier, and dried to obtain a bottom electrode (11); the bottom electrode (11) is plasma cleaned on the surface; an adhesive is added to the vermiculite slurry, and mixed; the mixed slurry is screen-printed on the surface of the conductive sub-layer, and dried to obtain an electronically emitting layer (12) printed on the bottom electrode (11), that is, a functional layer (1); S3, making a moisture absorbing layer (2), Plasma cleaning of the carrier surface, adding a polymer electrolyte to a solvent and mixing to obtain a polymer electrolyte solution, soaking the carrier in the polymer electrolyte solution, taking it out, standing it, and drying it to obtain a hygroscopic layer (2); S4, assembly, A portion of the electron-emitting layer (12) of the functional layer (1) is wiped off to expose the conductive layer as an electrode, a hygroscopic layer (2) is placed on the functional layer (1), and a top electrode (3) is placed on the hygroscopic layer (2) as an electrode, thereby obtaining a moisture power generation device based on vermiculite nanosheet film.

5. The method for preparing a moisture power generation device based on vermiculite nanosheet film according to claim 4, characterized in that: In step S1, the dispersant is water; The mass / volume ratio of vermiculite to dispersant is (1-5 g):15 mL, and the mass concentration of the vermiculite slurry is 10-15 g / L.

6. The method for preparing a moisture power generation device based on vermiculite nanosheet film according to claim 4, characterized in that: In step S2, the adhesive is sodium alginate; The solid content of the slurry of the conductive sublayer material is 10-20%, and the ratio of the unit area usage to the thickness of the conductive sublayer is (0.2-1mL / cm 2 ):(0.1-1mm); The volume / mass ratio of the vermiculite slurry to the adhesive is (50-70 mL):1 g, and the ratio of the unit area dosage of the mixed slurry to the thickness of the electron-emitting layer (12) is (0.02-0.1 mL / cm 2 ):(0.1-1mm).

7. The method for preparing a moisture power generation device based on vermiculite nanosheet film according to claim 4, characterized in that: In step S3, the solvent is water; The volume concentration of the polymer electrolyte solution is 40-80%.

8. The method for preparing a moisture power generation device based on vermiculite nanosheet film according to claim 4, characterized in that: In step S1, the power of intermittent ultrasonic crushing is 800-1200W, the temperature is 0-20°C, the total time is 8-14h, the single time is 1-3h, and the number of times is 5-9 times; The speed of centrifugal washing is 2000-6000rpm, the temperature is room temperature, the time is 5-15min, and the number of times is 3-7 times; The drying temperature is 60-100°C and the drying time is 8-12h.

9. The method for preparing a moisture power generation device based on vermiculite nanosheet film according to claim 4, characterized in that: In step S2, the conductive sublayer is dried at a temperature of 40-80° C. for 1-3 hours; The power of plasma surface cleaning is 80-120W, the temperature is room temperature, and the time is 2-10min; The mixing temperature is room temperature and the mixing time is 20-40 minutes; The drying temperature is 40-80°C and the drying time is 0.5-1.5h.

10. The method for preparing a moisture power generation device based on vermiculite nanosheet film according to claim 4, characterized in that: In step S3, the power of plasma surface cleaning is 80-120W, the temperature is room temperature, and the time is 2-10min; The mixing temperature is room temperature and the mixing time is 20-40 minutes; The soaking temperature is room temperature and the soaking time is 0.5-2h; The temperature of the static state is room temperature, and the time is 10-30 minutes; The drying temperature is 40-60°C and the drying time is 0.5-1.5h.