Method and device for manufacturing PCB (Printed Circuit Board) locally plated with thick gold
The local treatment of PCB boards through the dry film plating method or the oil printing method, combined with dry film sealing and development etching technology, the problems of high production cost, low efficiency and low yield in local gold plating technology are solved, and the problem of high production cost, low efficiency and low yield rate is achieved. Efficient outer circuit production can avoid gold seepage and erosion and defects, and reduce production costs.
Patent Information
- Application Number
- CN202410948340.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-12
AI Technical Summary
The existing local gold plating technology has problems such as high production costs, low production efficiency and extremely low yield, especially after the outer layer etching, PAD gold seepage and line erosion and incomplete lines are prone to occur.
The target area of the PCB board is partially treated by selective dry film plating or printing and oil plating, and the outer line is made by dry film sealing, welding prevention, and development etching. The specific steps include needle brush surface treatment, film compression, Exposure and development, combined with nickel plating and gold plating, protect the target area using frames or blank spacers.
It fundamentally solves the problems of PAD gold seepage and line erosion and incomplete lines in traditional processes, reduces production processes, improves production efficiency, and significantly reduces the production cost of local gold plating.
Smart Images

Figure CN118946025A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the technical field of PCB manufacturing, and in particular to a method and device for manufacturing a partially thick gold plated PCB. Background Art
[0002] Circuit boards are an indispensable part of modern electrical equipment. They play an important role in transmitting and controlling signals. During the manufacturing process, the surface of the circuit board needs to be processed to improve its conductivity. In the field of electronics and electrical appliances, local gold plating technology is used to make various key connectors and contact points and other electronic components. It can not only form a layer of conductive metal on the surface of the circuit board to improve the conductivity of the circuit board, but also effectively reduce the generation of oxidation and corrosion, thereby improving the corrosion resistance and service life of the circuit board, and improving the welding performance to make the equipment run more stable. The current common practice in the industry is: 1. After the outer layer is etched, the wire is conductively plated with gold and then the lead is removed. For example, fake gold fingers and independent large PADs are prone to gold penetration and lead double drilling residue due to the height difference between the copper surface and the substrate. The increase in the process seriously affects the production cost and efficiency.
[0003] 2. After partial gold plating, the outer layer circuit is made. The height difference between the gold plating position and the copper surface will affect the tightness of the dry film and the copper surface. During etching, the solution will attack and cause the circuit to be corroded and defective, which cannot meet the quality requirements; the yield rate is extremely low. Summary of the invention
[0004] In view of the above problems, the embodiments of the present invention provide a method and device for manufacturing a partially thick gold-plated PCB, which are used to solve the problems of high production cost, low production efficiency and extremely low yield rate in the existing partial gold plating.
[0005] According to one aspect of an embodiment of the present invention, a method for manufacturing a partially gold-plated PCB is provided, the method comprising: Pre-process the PCB board; Filling holes with resin on the PCB board, and performing GAP electroplating on the surface of the PCB board; The target area of the PCB is locally treated by selective dry film plating or selective oil printing, and the target area is locally gold plated; The outer circuit of the PCB board is made by dry film sealing, solder mask, and developing and etching.
[0006] In some optional embodiments, The target area of the PCB board is locally treated by the selective dry film plating method, specifically including: The PCB board is surface treated by a needle brush with a microetching rate of 0.7 μm-1 μm and a line speed of 2.5 m / min; Laminating the gold-plated dry film onto the PCB board at a laminating speed of 2m / min, a pressure of 5kg / cm²-6kg / cm², and a temperature of 120±1°C, and laminating the PCB board for the second time by air pressing; The target area was exposed by an exposure machine with an energy of 270 mj and a PE value of 50 μm, and after standing for 30 minutes, it was developed at a line speed of 2.2 m / min and then air-exposed.
[0007] In some optional embodiments, the target area of the PCB is locally processed by the printing and oiling method, specifically including: Print the selected oil on the surface of the PCB board, and set a square area around the target area, the square area is 320 mil away from the edge of the target area; wherein the printed selected oil is printed by 36T screen printing with 2 knives and a thickness of 0.8 mil -1.5 mil; After printing is completed, the PCB board is pre-baked and the square area is exposed; Blue glue is pressed on the PCB board, and a blue glue window is opened at the target area, wherein the blue glue window area is 200 mils away from the edge of the target area.
[0008] In some optional embodiments, the locally gold-plating the target area specifically includes: Send the PCB board to the gold plating production line, and perform nickel plating and gold plating in sequence; Among them, the parameters of the gold plating production line are set as follows: gold content 2.5-3g / l, cobalt content 0.6-0.7g / l, pH value 4.0-4.5, specific gravity 10-14Be, Ni2+≤3500PPM, Cu2+≤10PPM, Fe2+≤25PPM, Zn2+≤10PPM, pb2+≤10PPM, spray pressure 1 kg / cm2-1.5kg / cm2, temperature 50±2℃, production line speed 0.6 m / min-1m / min, gold plating current density 30 ASF-32ASF, nickel plating current density 40 ASF-45ASF; the minimum gold thickness is 50 microinches, the nickel thickness is 100 microinches, and after completing the local gold plating of the target area, a frame or white paper or film is required to be used for the transportation of the PCB board.
[0009] In some optional embodiments, after locally treating the target area of the PCB board by selective dry film plating or selective oil printing, and before locally gold plating the target area, it also includes: attaching edge glue to three edges of the PCB board by tape.
[0010] In some optional embodiments, the dry film sealing specifically includes: sealing the plug-in holes of the PCB by means of a dry film.
[0011] In some optional embodiments, the solder resist, developing and etching specifically include the following steps: After printing 3 passes on the C side of the PCB using a 36T screen, place it in a horizontal rack and bake it at 75°C for 8 minutes; After printing 2 passes on the S side of the PCB using a 48T screen, place it in a horizontal rack and bake it at 75°C for 5 minutes; After printing is completed, the PCB board is pre-baked, and the PCB board is exposed, and then the PCB board is developed and DES etching is used to make the outer layer circuit.
[0012] In some optional embodiments, the pre-processing of the PCB board includes, in sequence, performing thick copper processing on the PCB board, performing controlled depth drilling on the PCB board, and performing resin plugging on the holes.
[0013] In some optional embodiments, after the outer layer circuit of the PCB board is produced by dry film sealing, solder mask, and developing and etching in sequence, it also specifically includes: performing outer layer AOI treatment on the PCB board, performing secondary solder mask treatment on the PCB board, and performing text, outer layer, gold deposition / film removal on the PCB board.
[0014] According to another aspect of an embodiment of the present invention, a device for manufacturing a partially gold-plated PCB is provided, wherein the device is used to execute the above-mentioned method for manufacturing a partially gold-plated PCB to manufacture a printed circuit board.
[0015] The method and device for manufacturing a PCB with local thick gold plating of the present invention have the following beneficial effects: the target area of the PCB board is locally processed by a selective dry film plating method or a selective oil printing method, and the target area is locally gold plated; the outer layer circuit of the PCB board is manufactured by dry film hole sealing, solder mask, and developing and etching in sequence. The undesirable problems such as PAD gold penetration and circuit erosion and incompleteness caused by local gold plating after outer layer etching in the traditional process are fundamentally improved, and multiple production processes are reduced to improve production efficiency; the production cost of local gold plating is greatly reduced.
[0016] The above description is only an overview of the technical solution of the embodiment of the present invention. In order to more clearly understand the technical means of the embodiment of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the embodiment of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings are only used to illustrate the embodiments and are not to be considered as limiting the present invention. In addition, the same reference symbols are used to represent the same components throughout the accompanying drawings. In the accompanying drawings: Figure 1 A schematic flow chart of a method for manufacturing a partially gold-plated PCB according to Embodiment 1 of the present invention is shown; Figure 2 A schematic diagram of a PCB board using a dry film selective plating method according to Example 1 of the present invention is shown; Figure 3 A schematic diagram showing defective products of Example 1 provided by the present invention is shown.
[0018] Figure 4 A schematic diagram of a PCB board of the printing and oiling method of Example 1 provided by the present invention is shown. DETAILED DESCRIPTION
[0019] Exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.
[0020] Embodiment 1, See also Figure 1 According to one aspect of an embodiment of the present invention, a method for manufacturing a partially gold-plated PCB is provided, the method comprising: 110, pre-processing the PCB board; In step 110, pre-processing the PCB board includes, in sequence, performing a thick copper treatment on the PCB board, performing controlled depth drilling on the PCB board, and performing resin plugging on the holes.
[0021] 120, resin-filling holes on the PCB board, and performing GAP electroplating on the surface of the PCB board; in step 120, the openings and blind holes on the PCB board are filled with resin, and the surface of the PCB board is electroplated with GAP copper plating solution. In this embodiment, the resin-filling holes on the PCB board specifically includes filling holes with local gold plating, and also filling holes for through holes and controlled depth holes on the entire board. In addition to electroplating the entire board to thicken the hole surface copper, the GAP electroplating on the surface of the PCB board also includes depositing copper on the surface of the through holes and controlled depth holes with resin plug holes and thickening the surface copper.
[0022] 130, locally treat the target area of the PCB board by selective dry film plating method or selective oil printing method, and locally gold plate the target area; in step 130, the selective dry film plating method locally treats the target area of the PCB board, specifically including: surface treating the PCB board by a needle brush with a micro-etching rate of 0.7μm-1μm and a line speed of 2.5m / min; laminating the gold-plated dry film onto the PCB board according to a laminating speed of 2m / min, a pressure of 5kg / cm²-6kg / cm², and a temperature of 120±1℃, and performing secondary laminating on the target area by air pressing; exposing the target area with an energy of 270mj and a PE value of 50μm by an exposure machine, and after standing for 30min, developing at a line speed of 2.2m / min and then air exposing. The target area of the PCB board is locally processed by the printing and selective oiling method, specifically comprising: printing selective oil on the surface of the PCB board, and setting a square area on the periphery of the target area, wherein the square area is 320 mils away from the edge of the target area, wherein the printing and selective oil is printed by 36T screen printing with 2 knives and a thickness of 0.8 mil-1.5 mil; pre-baking the PCB board after printing is completed, and exposing the square area; pressing blue glue on the PCB board, and opening a blue glue window at the target area, wherein the blue glue window area is 200 mils away from the edge of the target area.
[0023] 140, the outer layer circuit of the PCB board is produced by dry film sealing, solder mask, and developing and etching in sequence. Dry film sealing specifically includes: sealing the plug-in holes of the PCB by dry film. Solder mask and developing and etching specifically include the following steps: after printing 3 times on the C side of the PCB board with a 36T screen, place it on a horizontal rack and bake it at 75°C for 8 minutes; after printing 2 times on the S side of the PCB board with a 48T screen, place it on a horizontal rack and bake it at 75°C for 5 minutes; after printing, pre-bake the PCB board, expose the PCB board, and then develop the PCB board and produce the outer layer circuit by DES etching.
[0024] The present invention performs local processing on the target area of the PCB board by selective dry film plating or selective oil printing, and performs local gold plating on the target area; the outer layer circuit of the PCB board is manufactured by dry film hole sealing, solder mask, and developing and etching in sequence. The invention fundamentally improves the undesirable problems such as PAD gold penetration and circuit erosion and incompleteness caused by local gold plating after outer layer etching in the traditional process, and at the same time reduces multiple production processes and improves production efficiency; and greatly reduces the production cost of local gold plating.
[0025] In some optional embodiments, see Figure 2, the target area of the PCB board is locally treated by the selective dry film plating method, specifically including: surface treatment of the PCB board by a needle brush with a micro-etching rate of 0.7μm-1μm and a line speed of 2.5m / min; the gold-plated dry film is pressed onto the PCB board according to a lamination speed of 2m / min, a pressure of 5 kg / cm²-6kg / cm², and a temperature of 120±1℃, and the PCB board is pressed twice by air pressure; the target area is exposed by an exposure machine with an energy of 270mj and a PE value of 50μm, and after standing for 30min, it is developed at a line speed of 2.2m / min and then air-exposed. In this embodiment, the pre-treatment adopts a needle brush 500#+800#+super-roughening, a micro-etching rate of 0.7-1μm, and a line speed of 2.5m / min to ensure the bonding between the roughness of the copper surface and the selective gold-plated dry film. The gold-plated dry film can be DuPont dry film W250. The lamination speed is 2m / min, the pressure is 5-6kg / cm², and the temperature is 120±1℃. The dry film is laminated to the PCB board, and then air pressing is used for the second lamination. The exposure is specified by the LDI machine production. The target area BGA pad is exposed with an energy of 270mj and a PE value of 50μm. After exposure, it is allowed to stand for 30 minutes and then developed at a line speed of 2.2m / min and then air-exposed again. For special selected gold-plated dry film to resist the thick gold electroplating anti-gold plating solution and improve the roughness of the pre-treated copper surface, add an air press of the dry film after normal lamination, and add an air exposure after normal exposure and development. The overall effect is to improve the bonding strength between the selected gold-plated dry film and the copper surface to prevent such as Figure 3 The defects shown are gold seepage, chemical stains, etc., which will result in scrap.
[0026] In some optional embodiments, see Figure 4 , the target area of the PCB board is locally processed by the printing and selective oiling method, specifically including: printing selective oil on the surface of the PCB board, and setting a square area on the periphery of the target area, the square area is 320mil away from the edge of the target area, wherein the printing and selective oil is printed by 36T screen printing 2 knives with a thickness of 0.8mil-1.5mil; after printing, the PCB board is pre-baked and the square area is exposed; blue glue is pressed on the PCB board, and a blue glue window is opened at the target area, wherein the blue glue window area is 200mil away from the edge of the target area. In this embodiment, Figure 4In the figure, the enlarged area is the target area, the red frame on the outer side of the target area is the square area, and the yellow frame is the blue glue window area. Make the selective oil printing point to make a large square area to cover all the target areas of the gold-plated PAD. The spacing is more than 200mil from the edge of the target area, and the lower oil screen is 120mil larger than the single side of the square area. Use 36T screen printing 2 knives to control the thickness of 0.8-1.5mil. After printing, pre-bake according to normal parameters, expose the data to make the PAD the same size as the original, and expose the square area of the electro-gold PAD with a spacing of 320mil. Gold plating is normally pressed with blue glue, and the edge spacing of the display area is 200mil. Ensure that there is still 120mil of selective oil covered by blue glue to prevent gold from seeping at the junction of selective oil and blue glue and affecting the quality.
[0027] In some optional embodiments, the locally gold-plating the target area specifically includes: Send the PCB board to the gold plating production line, and perform nickel plating and gold plating in sequence; Among them, the parameters of the gold plating production line are set as follows: gold content 2.5-3g / l, cobalt content 0.6-0.7g / l, pH value 4.0-4.5, specific gravity 10-14Be, Ni2+≤3500PPM, Cu2+≤10PPM, Fe2+≤25PPM, Zn2+≤10PPM, pb2+≤10PPM, spray pressure 1 kg / cm2-1.5kg / cm2, temperature 50±2℃, production line speed 0.6 m / min-1m / min, gold plating current density 30 ASF-32ASF, nickel plating current density 40 ASF-45ASF; the minimum gold thickness is 50 microinches, the nickel thickness is 100 microinches, and after completing the local gold plating of the target area, a frame or white paper or film is required to be used for the transportation of the PCB board. In this embodiment, gold plating and nickel plating are both produced on the same vertical continuous gold plating line. The equipment process design is to first nickel plate and then gold plate. The parameters are the section where the production board reaches and the current will be automatically applied according to the set parameters. The two sections can be separated and the current is applied. The unit of thickness is u" which represents micro inches. Only by controlling the above parameters can it be ensured that the gold-nickel thickness and reliability meet the quality requirements. After gold plating, all process transportation needs to use a frame or white paper or film for transportation to prevent the target area from being scratched.
[0028] In some optional embodiments, after the target area of the PCB is locally treated by the selective dry film plating method or the selective oil printing method, before the target area is locally gold plated, it also includes: pasting edge glue on three sides of the PCB board by adhesive tape. In this embodiment, the tape model is: high temperature resistant brown tape 24mm*33m, wrapping 3 sides, leaving one short side with more copper exposed for gold plating clamping point conduction. Pasting edge glue on three sides of the PCB board by adhesive tape can prevent the copper on the board edge from being plated with gold to save costs, and only one side is left for conduction.
[0029] In some optional embodiments, the dry film sealing specifically includes: sealing the plug-in holes of the PCB by dry film. Before the film sealing, the hole is sandblasted, and grinding and super-roughening are prohibited to avoid damaging the gold-plated gold layer; the outer layer exposure uses the cover hole material, and only the plug-in holes of the whole board are sealed to prevent the DES etching solution from biting the copper of the plug-in holes and causing the holes to break and open; In some optional embodiments, the solder mask, development and etching specifically include the following steps: after printing 3 cuts on the C surface of the PCB board with a 36T screen, place it in a horizontal rack and bake it at 75°C for 8 minutes; after printing 2 cuts on the S surface of the PCB board with a 48T screen, place it in a horizontal rack and bake it at 75°C for 5 minutes; after printing, pre-bake the PCB board, expose the PCB board, and then develop the PCB board to make the outer layer circuit through DES etching. Pre-treatment is sandblasting, and grinding, volcanic ash and super-roughening are prohibited to avoid damaging the sealing dry film and the gold-plated gold layer; the ink uses Sun Ink PPR-50-EB01, and the C surface is partially gold-plated with a 36T empty mesh and the S surface uses a 48T empty mesh. The specific method is: after printing 3 cuts on the C surface, place it in a horizontal rack and bake it at 75°C for 8 minutes. After printing 2 cuts on the S surface, place it in a horizontal rack and bake it at 75°C for 5 minutes, and then pre-bake and expose it normally.
[0030] Embodiment 2: Based on Example 1, the present invention provides a method for producing PCB boards. After each core board of the PCB board is made, the multi-layer core boards are pressed together to form a PCB board, and the PCB board is pre-treated, which includes, in sequence, a thick copper treatment on the PCB board, controlled depth drilling, and resin plugging on the PCB board; so that the PCB board meets the conditions for making partial gold plating. After the outer layer circuit of the PCB board is made by dry film sealing, solder mask, and developing etching in sequence, it also specifically includes: outer layer AOI treatment of the PCB board, secondary solder mask treatment of the PCB board, text, outer layer, gold plating / film removal of the PCB board. The outer layer of the PCB board is processed through the above steps so that it has the function of the outer layer.
[0031] Embodiment 3: According to another aspect of an embodiment of the present invention, a device for making a partially gold-plated PCB is provided, and the device is used to execute the above-mentioned method for making a partially gold-plated PCB to make a printed circuit board. The present invention performs a local treatment on the target area of the PCB board by a selective dry film plating method or a selective oil printing method, and performs local gold plating on the target area; the outer layer circuit of the PCB board is successively made by dry film sealing, solder masking, and developing and etching. It fundamentally improves the undesirable problems such as PAD gold penetration and circuit corrosion and incompleteness caused by local gold plating after outer layer etching in the traditional process, and at the same time reduces multiple production processes and improves production efficiency; greatly reduces the production cost of partial gold plating.
[0032] In the description provided herein, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. Similarly, in order to simplify the present invention and help understand one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, the various features of the embodiments of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. Wherein, the claims that follow the specific embodiment are hereby expressly incorporated into the specific embodiment, wherein each claim itself is a separate embodiment of the present invention.
[0033] Those skilled in the art will appreciate that the modules in the devices in the embodiments may be adaptively changed and arranged in one or more devices different from the embodiments. The modules or units or components in the embodiments may be combined into one module or unit or component, and further may be divided into a plurality of submodules or subunits or subcomponents. Except that at least some of such features and / or processes or units are mutually exclusive.
[0034] It should be noted that the above embodiments illustrate the present invention rather than limit it, and that those skilled in the art may design alternative embodiments without departing from the scope of the appended claims. In the claims, any reference symbol between brackets shall not be construed as a limitation on the claims. The word "comprising" does not exclude the presence of elements or steps not listed in the claims. The word "one" or "an" preceding an element does not exclude the presence of multiple such elements. The present invention may be implemented with the aid of hardware comprising several different elements and with the aid of appropriately programmed computers. In a unit claim that lists several systems, several of these systems may be embodied by the same hardware item. The use of the words first, second, and third, etc. does not indicate any order. These words may be interpreted as names. The steps in the above embodiments, unless otherwise specified, should not be understood as limitations on the order of execution.
Claims
1. A method for manufacturing a partially gold-plated PCB, characterized in that: The method comprises: Pre-process the PCB board; Filling holes with resin on the PCB board, and performing GAP electroplating on the surface of the PCB board; The target area of the PCB is locally treated by selective dry film plating or selective oil printing, and the target area is locally gold plated; The outer circuit of the PCB board is made by dry film sealing, solder mask, and developing and etching.
2. The method for manufacturing a partially gold-plated PCB according to claim 1, characterized in that: The target area of the PCB board is locally treated by the selective dry film plating method, specifically including: The PCB board is surface treated by a needle brush with a microetching rate of 0.7 μm-1 μm and a line speed of 2.5 m / min; Laminating the gold-plated dry film onto the PCB board at a laminating speed of 2m / min, a pressure of 5kg / cm²-6kg / cm², and a temperature of 120±1°C, and laminating the PCB board for the second time by air pressing; The target area was exposed by an exposure machine with an energy of 270 mj and a PE value of 50 μm, and after standing for 30 minutes, it was developed at a line speed of 2.2 m / min and then air-exposed.
3. The method for manufacturing a partially gold-plated PCB according to claim 1, characterized in that: The target area of the PCB board is locally processed by the printing and oiling method, specifically including: Print the selected oil on the surface of the PCB board, and set a square area around the target area, the square area is 320 mil away from the edge of the target area; wherein the printed selected oil is printed by 36T screen printing with 2 knives and a thickness of 0.8 mil -1.5 mil; After printing is completed, the PCB board is pre-baked and the square area is exposed; Blue glue is pressed on the PCB board, and a blue glue window is opened at the target area, wherein the blue glue window area is 200 mils away from the edge of the target area.
4. The method for manufacturing a partially gold-plated PCB according to claim 2 or 3, characterized in that: The local gold plating of the target area specifically includes: Send the PCB board to the gold plating production line, and perform nickel plating and gold plating in sequence; Among them, the parameters of the gold plating production line are set as follows: gold content 2.5-3g / l, cobalt content 0.6-0.7g / l, pH value 4.0-4.5, specific gravity 10-14Be, Ni2+≤3500PPM, Cu2+≤10PPM, Fe2+≤25PPM, Zn2+≤10PPM, pb2+≤10PPM, spray pressure 1 kg / cm2-1.5kg / cm2, temperature 50±2℃, production line speed 0.6 m / min-1m / min, gold plating current density 30 ASF-32ASF, nickel plating current density 40 ASF-45ASF; the minimum gold thickness is 50 microinches, the nickel thickness is 100 microinches, and after completing the local gold plating of the target area, a frame or white paper or film is required to be used for the transportation of the PCB board.
5. The method for manufacturing a partially gold-plated PCB according to claim 4, characterized in that: After the target area of the PCB is locally processed by the selective dry film plating method or the selective oil printing method, and before the target area is locally gold plated, the method further includes: pasting edge glue on three edges of the PCB by means of adhesive tape.
6. The method for manufacturing a partially gold-plated PCB according to claim 1, characterized in that: The dry film sealing specifically includes: sealing the plug-in holes of the PCB by using a dry film.
7. The method for manufacturing a partially gold-plated PCB according to claim 1, characterized in that: The solder resist and developing etching specifically include the following steps: After printing 3 passes on the C side of the PCB using a 36T screen, place it in a horizontal rack and bake it at 75°C for 8 minutes; After printing 2 passes on the S side of the PCB using a 48T screen, place it in a horizontal rack and bake it at 75°C for 5 minutes; After printing is completed, the PCB board is pre-baked, and the PCB board is exposed, and then the PCB board is developed and DES etching is used to make the outer layer circuit.
8. The method for manufacturing a partially gold-plated PCB according to claim 1, characterized in that: The pre-processing of the PCB board includes, in sequence, performing a thick copper treatment on the PCB board, performing controlled depth drilling on the PCB board, and performing resin plugging on the holes.
9. The method for manufacturing a partially gold-plated PCB according to claim 1, characterized in that: After the outer layer circuit of the PCB board is made by dry film sealing, solder mask, developing and etching, it also includes: outer layer AOI treatment of the PCB board, secondary solder mask treatment of the PCB board, text, outer layer, gold deposition / film removal of the PCB board.
10. A device for manufacturing a partially gold-plated PCB, characterized in that: The device is used to execute the method for manufacturing a partially gold-plated PCB as described in any one of claims 1 to 9 to manufacture a printed circuit board.
Citation Information
Cited By
Circuit board golden finger processing method and circuit board
CN121310431A