Manufacturing method of core board of packaging substrate

By using the combination of insulating substrate, copper column and pad in the production of package substrate core board, combined with the technology of film negative sheet and hard dry film, the problems of irregular pad structure and poor bonding force are solved, and the pad is realized Stable combination with the substrate and high-precision design reduce production costs.

CN118946048APending Publication Date: 2024-11-12JIANGSU SUHANG ELECTRONIC CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411067592.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing method of producing package substrate core boards, the pad structure is irregular and the bonding force is poor, which causes the pad to fall off easily, affecting product pass rate and production cost.

Method used

A core plate production method including insulating substrate, copper columns and pads is adopted to form cross-shaped, square or round pads through film negative sheets by reducing copper, drilling, copper depositing, pattern transfer and electroplating processes. The combination with the hard dry film ensures a stable bond between the pad and the substrate.

Benefits of technology

It improves the bonding force between the pad and the insulating substrate, reduces production costs, and ensures that the shape, size and position of the pad meets the design requirements, improving the accuracy and pass rate of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946048A_ABST
    Figure CN118946048A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a core board of a packaging substrate. The core board comprises an insulating substrate, a plurality of copper columns penetrating through the insulating substrate and a plurality of bonding pads arranged on the two side faces of the insulating substrate. Through primary copper thinning, it is guaranteed that a basic copper layer combined with an insulating substrate in a pressing and covering mode is reserved on the insulating substrate, a combination foundation of the bonding pad and the insulating substrate is provided for the bonding pad, through arranging a negative film and combining secondary copper reduction, the bonding pad is preliminarily formed on the basic copper layer, the bonding force of the bonding pad and the insulating substrate is guaranteed, and then through arranging a positive film and combining tertiary copper reduction, the bonding pad is formed on the bonding pad. And a bonding pad meeting the binding force requirement is formed on the insulating substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of packaging substrates, and in particular to a method for manufacturing a packaging substrate core board. Background Art

[0002] The packaging substrate can provide electrical connection, protection, support, heat dissipation, assembly and other functions for the chip, so as to achieve multi-pin, reduce the size of the packaged product, improve electrical performance and heat dissipation, ultra-high density or multi-chip modularization.

[0003] The packaging substrate is formed by stacking multiple layers of core boards with circuits to form a connecting circuit for connecting the IC chip and the PCB circuit board; the core board includes a substrate and a pad. The existing method is to form a pad on the substrate by exposure, development, and electroplating. The disadvantages of this manufacturing method are: Figure 1 As shown in the figure, when the pad is a cross-shaped structure, the periphery of the cross is irregular; secondly, because the pad diameter is 0.1mm and the height is at least about 50μm, the pad is plated on the substrate using an electroplating process, and the combination of two different materials results in poor bonding. As a result, when the core board is delivered to downstream production units, the pad often falls off due to poor bonding, resulting in a low product delivery qualification rate and high production costs. Summary of the invention

[0004] In order to overcome the above defects, the present invention provides a method for manufacturing a packaging substrate core board, which can not only ensure the pad structure but also ensure the bonding force between the pad and the substrate, and ensure that the pad will not fall off, thereby reducing production costs.

[0005] The technical solution adopted by the present invention to solve the technical problem is: to provide a method for manufacturing a package substrate core board, the core board comprising an insulating substrate, a plurality of copper pillars penetrating the insulating substrate, and a plurality of pads arranged on two side surfaces of the insulating substrate;

[0006] The pads include a first pad and a second pad, the first pads are respectively provided at both ends of the copper column, and at least a part of the two first pads facing the copper column are attached to the corresponding side surfaces of the insulating substrate; the bottom of the second pad is attached to the insulating substrate;

[0007] The manufacturing method of the core plate comprises:

[0008] Step 1: cutting a material to provide a double-sided copper-clad laminate, wherein the double-sided copper-clad laminate comprises an insulating substrate and conductive copper layers respectively disposed on two sides of the insulating substrate;

[0009] Step 2: a copper reduction process is used to etch the conductive copper layers on both sides of the double-sided copper clad laminate to form thin copper layers on both sides;

[0010] Step 3: drilling, using mechanical drilling to form a through hole on the double-sided copper-clad board, the through hole passing through the three-layer structure of the thin copper layer, the insulating substrate, and the thin copper layer;

[0011] Step 4: Copper deposition and flash plating, the whole board is sequentially subjected to chemical copper deposition and electroplating processes to deposit a certain thickness of surface copper layers on the thin copper layers on both sides of the double-sided copper clad board to form composite copper layers respectively, and at the same time, a certain thickness of conductive copper layers are deposited on the inner wall surface of the through hole to achieve connectivity of the composite copper layers on both sides;

[0012] Step 5: One-time graphic transfer, including film negative and photosensitive dry film,

[0013] Placing a photosensitive dry film and a film negative on the outer side of the composite copper layer of the double-sided copper clad laminate in sequence, and obtaining a pad area covered by the photosensitive dry film and a copper leakage area not covered by the photosensitive dry film through exposure and development;

[0014] The photosensitive dry film has a thickness of 30-50 μm and is pressed onto the outer surface of the composite copper layer by a laminating machine at a speed of 2.8 m per minute and a roller temperature of 100-120° C.

[0015] Step 6: Secondary copper reduction, after etching the surface copper layer of the copper leakage area until the thin copper layer at the corresponding position is exposed, use a film stripping liquid to remove the photosensitive dry film covering the pad area to obtain a semi-finished core board;

[0016] Step 7: Secondary graphic transfer, including film positive and hard dry film,

[0017] The hard dry film and the positive film are sequentially arranged on the outer side of the semi-finished core board, and the thin copper layer on the semi-finished core board is covered by the hard dry film through exposure and development, while the pad area is exposed;

[0018] The thickness of the hard dry film is 70-90um, and it is pressed on the outer surface of the semi-finished core plate by a laminating machine at a speed of 2m per minute and a pressing roller temperature of 100-120°C;

[0019] Step 8: pattern electroplating, the exposed through holes and pad areas on the semi-finished core board obtained in step 7 are filled with electroplated copper to form the copper pillars and pads on the insulating substrate;

[0020] Step 9: grinding and film removal, after the electroplated copper layer formed on both sides of the semi-finished core board is partially removed by the ceramic grinding process, the hard dry film covering the thin copper layer is removed to form a pad that meets the height and diameter design requirements;

[0021] Step 10: reducing copper three times, flash etching the thin copper layer other than the pad on the semi-finished core board until the insulating substrate at the corresponding position is exposed, to obtain the core board;

[0022] Step 11: Inspection before warehousing: by optical scanning, the circuit pattern produced in step 10 is compared with the design pattern, and the circuit pattern is checked and corrected; the circuit pattern is tested by peel strength test using IPC-TM-650 test method, and the bonding strength between the first pad on the core board and the insulating substrate and the copper column, and the bonding strength between the second pad and the insulating substrate, are tested;

[0023] After passing the test, the products will be divided into panels, packaged and put into storage according to the design requirements.

[0024] As a further improvement of the present invention, the thickness of the conductive copper layer is 15-18 μm, and the thickness of the thin copper layer is 3-8 μm;

[0025] In addition, before the first copper reduction, the double-sided copper clad laminate is placed in an oven at a controlled temperature of 180° C. and baked for 60 minutes to eliminate the internal stress of the double-sided copper clad laminate.

[0026] As a further improvement of the present invention, the diameter of the through hole is consistent with that of the copper column, which is 0.1-0.12 mm, the drilling speed is 185,000 revolutions per minute, the feed speed is 1.5 m per minute, and the retracting speed is 296 mm per second;

[0027] After drilling, the residual glue in the through hole is removed by a degumming process, and then a copper layer with a thickness of 2-4 um is deposited in the through hole by copper electroplating, so that a copper layer is formed on the bare surface of the insulating substrate in the through hole;

[0028] Among them, the degumming rate is 0.25-0.4 mg per square centimeter, the copper deposition rate is 0.3-0.8 um, and the micro-etching rate is 0.4-1.2 um.

[0029] As a further improvement of the present invention, in step 4, the flash plating parameters are 6 amperes per square foot and the time is 40 minutes;

[0030] After flash plating, the thickness of the conductive copper layer in the through hole is 2-4 μm; the thickness of the surface copper layer is 2-4 μm, so that the thickness of the composite copper layer is 5-12 μm.

[0031] As a further improvement of the present invention, in step 5, before providing the photosensitive dry film, a flash etching process is used, and the surface of the composite copper layer and the conductive copper layer formed in step 4 is micro-etched by 0.5 μm at an etching rate of 0.5-1.2 μm per minute to remove the oxide layer formed on the surface of the copper layer;

[0032] In addition, in step 5, an LDI exposure machine is used for exposure with an exposure energy of 110 mJ / cm2, a development speed of 3-4.5 m / min, and a development point of 50-60%.

[0033] As a further improvement of the present invention, in step 7, an LDI exposure machine is used to perform exposure and development with an exposure energy of 280 mJ per square centimeter, a development speed of 1-2 m per minute, and a development point of 50-60%.

[0034] As a further improvement of the present invention, in step 10, a flash etching process is used to etch the thin copper layer outside the pad on the core board semi-finished product at a speed of 5 m per minute and a temperature of 25-35° C. until the insulating substrate at the corresponding position is completely exposed.

[0035] As a further improvement of the present invention, the pads on the core board include any one or more of a cross shape, a square shape, and a circle shape.

[0036] The first pad is a circular structure coaxially arranged with the copper column, and its diameter is 0.145-0.175 mm.

[0037] The second pad is a cross-shaped or square structure, and its width is 0.09-0.11 mm.

[0038] The beneficial effects of the present invention are:

[0039] 1. Thin copper once to ensure that a basic copper layer is reserved on the insulating substrate for lamination and bonding, providing a bonding foundation for the pad and the insulating substrate. Set a negative film and combine with a second copper reduction to make the pad initially formed on the basic copper layer to ensure the bonding strength between the pad and the insulating substrate. Then set a positive film and combine with a third copper reduction to form a pad on the insulating substrate that meets the bonding strength requirements;

[0040] 2. Through the combination of film negative and photosensitive dry film, the pad area and non-pad area are distinguished on the base copper layer. Combined with the film positive, the hard dry film is ensured to completely cover the non-pad area, ensuring effective electroplating of the pad area, thereby ensuring that the pad shape, size and position meet the design requirements, and the pad accuracy is guaranteed;

[0041] 3. The combination of photosensitive dry film and hard dry film is used to ensure the consistency of the pad area position, further ensuring the stability of the pad and the insulating substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The cross pad status display for the existing manufacturing method;

[0043] Figure 2 This is a schematic diagram of the core plate structure of the present invention;

[0044] Figure 3 Make a state diagram of the method steps for the present invention;

[0045] Figure 4 A diagram showing the cross-sectional state of a copper column and a first pad processed by the manufacturing method of the present invention;

[0046] Figure 5 The diagram shows the state of the second (cross-shaped) pad processed by the manufacturing method of the present invention.

[0047] Combined with the accompanying drawings, the following description is given:

[0048] 100, insulating substrate; 101, copper pillar; 102, first pad; 103, second pad; 200, conductive copper layer; 300, thin copper layer; 400, through hole; 500, surface copper layer; 600, pad area; 700, exposed copper area; A, composite copper layer; B, conductive copper layer; C, photosensitive dry film; D, hard dry film. DETAILED DESCRIPTION

[0049] A preferred embodiment of the present invention is described in detail below in conjunction with the accompanying drawings.

[0050] The present invention provides a method for manufacturing a packaging substrate core board, see Figure 2 The core board includes an insulating substrate 100, a plurality of copper pillars 101 penetrating the insulating substrate 100, and a plurality of pads arranged on the two side surfaces of the insulating substrate 100; the pads include a first pad 102 and a second pad 103, and the first pads 102 are respectively provided at both ends of the copper pillar 101, and the two first pads 102 are at least partially attached to the corresponding side surface of the insulating substrate 100 on one side facing the copper pillar 101; the bottom of the second pad 103 is attached to the insulating substrate 100.

[0051] See also Figure 4 and 5 The pads on the core board include any one or more of a cross, a square, and a circle, and the pad height is 50-70 μm, wherein the first pad 102 is a circular structure coaxially arranged with the copper pillar 101, and its diameter is 0.145-0.175 mm. This embodiment takes the copper pillar 101 with a diameter of 0.1 mm and the first pad 102 connected to the copper pillar 101 and with a diameter of 0.16 mm as an example. The second pad is a cross or square structure, and its width is 0.09-0.11 mm. This embodiment takes the second pad 103 with a cross structure with a width of 0.1 mm as an example.

[0052] See also Figure 3 The method for manufacturing the core plate provided in this embodiment comprises the following steps:

[0053] Step 1: Cutting a material to provide a double-sided copper clad laminate, which includes an insulating substrate 100 and conductive copper layers 200 respectively disposed on two side surfaces of the insulating substrate 100 .

[0054] Among them, the double-sided copper clad laminate is purchased from existing raw materials on the market, that is, the conductive copper layer 200 is bonded to the insulating substrate (glass fiber epoxy resin board or ceramic substrate) by hot pressing, gluing, chemical copper plating and other methods, so as to ensure the bonding force between the conductive copper layer 200 and the insulating substrate 100. As a preference, this embodiment uses a double-sided copper clad laminate of the Hitachi brand E-705G model with a thickness of 0.6mm and a size of 310*310mm. The conductive copper layer 200 of the double-sided copper clad laminate of this brand has a thickness of 15-18μm, which is sufficient to support the bonding of a pad with a height of 50-70μm.

[0055] Step 2: Reduce copper once. Through the copper thinning process, the conductive copper layer 200 on both sides of the double-sided copper clad laminate is etched to form thin copper layers 300 on both sides. That is, full-board etching is adopted to etch the conductive copper layer 200 to a thickness of 3-8 μm, specifically a 5 μm thin copper layer 300, that is, a part of the original conductive copper layer is retained on the insulating substrate 100 (that is, the obtained thin copper layer 300 is bonded to the insulating substrate 100 at this time).

[0056] Among them, before the first copper reduction, the double-sided copper clad laminate needs to be placed in an oven at a controlled temperature of 180°C and baked for 60 minutes to remove moisture and eliminate the internal stress of the double-sided copper clad laminate.

[0057] Step 3: drilling, using mechanical drilling to drill a through hole 400 on the insulating substrate 100 having the thin copper layer 300 obtained in step 2, wherein the through hole 400 penetrates the three-layer structure of the thin copper layer 300, the insulating substrate 100, and the thin copper layer 300;

[0058] Among them, the diameter of the through hole 400 is consistent with that of the copper column 101, which is 0.1-0.12mm. The specific diameter of the through hole 400 is 0.1mm, and the drilling rig is controlled to drill at a speed of 185,000 revolutions per minute, a feed speed of 1.5m per minute, and a retracting speed of 296mm per second. While ensuring the quality of the through hole 400, the service life of the drill bit is also extended.

[0059] In addition, after drilling, a degumming process is used to remove residues in the through hole 400, such as the glue bonding the conductive copper layer and the insulating substrate, and then copper electroplating is used to deposit a copper layer with a thickness of about 0.4 μm in the through hole 400, so that a thinner copper layer is formed on the exposed surface of the insulating substrate in the through hole 400, which is convenient for the adhesion of copper in subsequent steps.

[0060] Among them, the degumming rate is 0.25-0.4 mg per square centimeter, the copper deposition rate is 0.3-0.8 um, and the micro-etching speed is 0.4-1.2 um, so the obtained copper layer is thinner. Because the copper layer is thinner, it can be better combined with the insulating substrate.

[0061] Step 4: flash plating, through the full-board electroplating process, a surface copper layer 500 with a thickness of 2-4μm is deposited on the thin copper layer 300 on both sides of the double-sided copper clad laminate to form a composite copper layer A with a thickness of 5-12μm respectively, and at the same time, a conductive copper layer B with a thickness of 2-4μm is deposited on the inner wall surface of the through hole 400 to achieve interlayer connectivity of the composite copper layers A on both sides; since the conductive copper layer B is deposited on the thinner copper layer in step 3, the conductive copper layer B can be firmly bonded to the thin copper layer in the through hole 400.

[0062] The flash plating parameters are 6 amperes per square foot and the time is 40 minutes.

[0063] That is to say, by reducing copper once, an original copper layer with a strong bonding force is reserved on the insulating substrate, and then a surface copper layer with a thickness of 2-4μm is flash-plated on the original copper layer. The surface copper layer serves as a connector between the thin copper layer and the electroplated filling layer of step 8, and the thinner surface copper layer can be firmly connected to the original copper layer, thereby ensuring a firm connection between the electroplated filling layer and the insulating substrate, improving the bonding force between the pad and the insulating substrate, and ensuring that the pad will not fall off.

[0064] Step 5: A pattern transfer, including a film negative and a photosensitive dry film C, is performed. The photosensitive dry film C and the film negative are sequentially arranged on the outer side of the composite copper layer A of the double-sided copper clad laminate, and a pad area 600 covered by the photosensitive dry film C and a copper leakage area 700 not covered by the photosensitive dry film C are obtained by exposure and development.

[0065] The thickness of the photosensitive dry film is 30-50 μm, and Changxing dry film HT9715M, a soft dry film with a thickness of 40 μm, is specifically selected. It is pressed on the outer surface of the composite copper layer by a laminator at a speed of 2.8 m per minute and a pressing roller temperature of 115°C.

[0066] Specifically, the photosensitive dry film is a photosensitive material, which is particularly sensitive to ultraviolet rays. A film negative with a circuit (pad pattern) is made according to the design requirements, and the film negative is placed on the photosensitive dry film. At this time, the part with the circuit on the film negative is transparent (pad area), and the non-circuit part is black (copper leakage area). The exposure is performed using an LDI exposure machine with an exposure energy of 110 millijoules per square centimeter, a development speed of 3-4.5m per minute, and a development point of 50-60%. Since light only penetrates the transparent part, the photosensitive dry film in the transparent part will undergo a polymerization reaction and solidify to prevent being etched; then the film negative is removed and a developing solution is used (development), causing the black part of the photosensitive dry film to be dissolved, exposing the copper layer, thereby completing the transfer of the pattern.

[0067] In addition, it should be pointed out that before a pattern transfer (i.e., between step 4 and step 5), in order to ensure that the thick electroplated copper layer is better combined with the composite copper layer and the conductive copper layer in the through hole, a flash etching process is adopted, and the etching rate is 0.5-1.2 μm per minute, so that the surface of the composite copper layer A and the conductive copper layer B is micro-etched by about 0.5 μm, so as to remove the oxide layer formed on the surface of the copper layer and improve the surface roughness of the copper layer to facilitate the adhesion of the subsequent electroplated copper layer.

[0068] Step 6: Second copper reduction, after etching the surface copper layer 500 of the copper leakage area 700 until the thin copper layer 300 at the corresponding position is exposed, use a film stripping solution to remove the photosensitive dry film C covering the pad area 600 to obtain a semi-finished core board.

[0069] After the second copper reduction, the shape (outer diameter) and position of the first pad and the second pad are initially formed on the insulating substrate, but the height does not meet the requirements, wherein the first pad is arranged around the through hole and connected to the conductive copper layer in the through hole.

[0070] Step 7: Secondary pattern transfer, including film positive and hard dry film D, the hard dry film D and the film positive are sequentially arranged on the outer side of the semi-finished core board, and an LDI exposure machine is used to expose and develop with an exposure energy of 280 millijoules per square centimeter, a development speed of 1-2 meters per minute, and a development point of 50-60%, so that the thin copper layer 300 on the semi-finished core board is covered by the hard dry film D, and the pad area 600 is exposed.

[0071] The thickness of the hard dry film is 70-90um, and the specific brand is Asahi Kasei AS21-80, with a thickness of 80um. It is pressed onto the outer surface of the semi-finished core board by a laminating machine at a speed of 2m per minute and a pressing roller temperature of 120°C.

[0072] Step 8: Graphic electroplating, the exposed through holes 400 and the pad area 600 on the semi-finished core board obtained in step 7 are filled with copper electroplating to form the copper pillars 101 and pads on the insulating substrate 100; a full-board electroplating process is used to ensure that there are no voids in the holes while also ensuring the filling of the pad area.

[0073] Step 9: Grind the plate and remove the film. The electroplated copper layer formed on the two sides of the semi-finished core board is reduced to a copper layer thickness of 70-80um (basically the thickness of the hard dry film) through a ceramic grinding process, and the hard dry film D covering the thin copper layer 300 is removed to form a pad that meets the design height requirements while ensuring the bonding strength of the pad. In addition, grinding the plate first and then removing the film also ensures that the diameter of the pad and the shape profile meet the design requirements.

[0074] Step 10: Three times of copper reduction, using flash etching process, at 5m per minute, temperature 25-35℃, etch the thin copper layer 300 outside the pads on the semi-finished core board until the insulating substrate 100 at the corresponding position is completely exposed, so as to avoid short circuits between pads and obtain the core board required by the design. Figure 4 The cross section of the copper column and the first pads disposed at the upper and lower ends of the copper column and the reference Figure 5 The state of the cross-shaped second pad displayed under the microscope not only meets the size requirements, but also has a flat pad shape to ensure the pad accuracy.

[0075] Step 11: Inspection before warehousing. Compare the circuit pattern produced in step 10 with the design pattern through optical scanning method, check and correct the circuit pattern, and use the industry's IPC-TM-650 test method to test the bonding strength between the first pad on the core board and the insulating substrate and copper column, as well as the bonding strength between the second pad and the insulating substrate. After passing the test, separate the boards, package them, and put them into warehouse according to the design requirements.

[0076] As follows, the bonding strength of the pads produced by the manufacturing method of the present invention and the manufacturing method of the traditional process are tested.

[0077] Specifically, in order to show the obvious difference between the manufacturing method of the present invention and the traditional manufacturing method, the peel strength test is carried out by taking the connection between the second pad and the insulating substrate as an example. And the second pad is selected as a cross shape with a smaller contact surface with the insulating substrate as an example for testing and comparison, which further illustrates that the manufacturing method of the present invention ensures the bonding strength between the pad and the insulating substrate.

[0078] A 5PCS core board is manufactured by the present invention, and a 5PCS core board is manufactured by a traditional method. The peel strength of the cross-shaped pad is tested according to the IPC-TM-650 test method, and the data unit is N / mm. The standard value of the pad peel strength in the industry is ≥1.050N / mm.

[0079] 1 2 3 4 5 Production method of the present invention 1.463 1.437 1.454 1.462 1.456 Traditional production method 0.216 0.225 0.218 0.242 0.213

[0080] It can be seen from the test data that the peel strength between the pad and the substrate of the core board made by the present invention far exceeds the industry standard value and has a high bonding strength. In addition, it can also be seen from the table that the traditional manufacturing method is far from meeting the industry requirements.

[0081] In addition, the appearance of the pad is tested under a microscope:

[0082] See also Figure 1 The cross-shaped pad is made by the traditional method under a microscope. Its outer contour is close to a circle, and each turn is in the shape of an arc;

[0083] See also Figure 5 The cross pad produced by the method of the present invention under a microscope has a shape that meets the cross requirements and has clear edges and corners.

[0084] Therefore, the core board obtained by the manufacturing method of the present invention has high precision, high peel strength and appearance that meet high standards in the industry.

[0085] In summary, the method for manufacturing a packaging substrate core board provided by the present invention thins copper once to ensure that a basic copper layer is reserved on the insulating substrate for pressure-coating and bonding with it, so as to provide a bonding basis for the pad to be bonded with the insulating substrate; sets a film negative film in combination with secondary copper reduction so that the pad is initially formed on the basic copper layer to ensure the bonding strength between the pad and the insulating substrate; and then sets a film positive film in combination with third copper reduction to form a pad that meets the bonding strength requirements on the insulating substrate; combines the film negative film with the photosensitive dry film to distinguish the pad area and the non-pad area on the basic copper layer, and combines the film positive film to ensure that the hard dry film completely covers the non-pad area, ensures effective electroplating of the pad area, and at the same time ensures the pad height, thereby ensuring that the pad shape, size and position meet the design requirements, so that the pad accuracy is guaranteed; and uses the photosensitive dry film and the hard dry film in combination to ensure the consistency of the pad area position, further ensuring the stability of the bonding between the pad and the insulating substrate.

[0086] Many specific details are described in the above description to facilitate a full understanding of the present invention. However, the above description is only a preferred embodiment of the present invention. The present invention can be implemented in many other ways different from those described herein, so the present invention is not limited to the specific implementation disclosed above. At the same time, any person familiar with the art can make many possible changes and modifications to the technical solution of the present invention using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.

Claims

1. A method for manufacturing a package substrate core board, characterized in that: The core board comprises an insulating substrate (100), a plurality of copper pillars (101) penetrating the insulating substrate (100), and a plurality of solder pads arranged on two side surfaces of the insulating substrate (100); The pads comprise a first pad (102) and a second pad (103); the first pads (102) are respectively provided at both ends of the copper column (101); and at least a portion of the two first pads (102) facing the copper column (101) are attached to corresponding side surfaces of the insulating substrate (100); and the bottom of the second pad (103) is attached to the insulating substrate (100); The manufacturing method of the core plate comprises: Step 1: cutting a material to provide a double-sided copper-clad laminate, wherein the double-sided copper-clad laminate comprises an insulating substrate (100) and conductive copper layers (200) respectively arranged on two side surfaces of the insulating substrate (100); Step 2: a first copper reduction process is performed to etch the conductive copper layer (200) on both sides of the double-sided copper clad laminate to form thin copper layers (300) on both sides thereof; Step 3: drilling, using a mechanical drilling method to form a through hole (400) on the double-sided copper-clad board, wherein the through hole (400) penetrates the three-layer structure of the thin copper layer (300), the insulating substrate (100), and the thin copper layer (300); Step 4: Copper deposition and flash plating, the whole board is sequentially subjected to chemical copper deposition and electroplating processes to deposit a certain thickness of surface copper layer (500) on the thin copper layers (300) on both sides of the double-sided copper clad board to form composite copper layers (A) respectively, and at the same time, a certain thickness of conductive copper layer (B) is deposited on the inner wall surface of the through hole (400) to achieve connectivity between the composite copper layers (A) on both sides; Step 5: One-time graphic transfer, including film negative and photosensitive dry film (C), A photosensitive dry film (C) and a negative film are sequentially arranged on the outer side of the composite copper layer (A) of the double-sided copper clad laminate, and a pad area (600) covered by the photosensitive dry film (C) and a copper leakage area (700) not covered by the photosensitive dry film (C) are obtained by exposure and development; The photosensitive dry film has a thickness of 30-50 μm and is pressed onto the outer surface of the composite copper layer by a laminating machine at a speed of 2.8 m per minute and a roller temperature of 100-120° C. Step 6: secondary copper reduction, etching the surface copper layer (500) of the copper leakage area (700) until the thin copper layer (300) at the corresponding position is exposed, and removing the photosensitive dry film (C) covering the pad area (600) with a film stripping liquid to obtain a semi-finished core board; Step 7: Secondary graphic transfer, including film positive and hard dry film CD), The hard dry film (CD) and the positive film are sequentially arranged on the outer surface of the semi-finished core board, and through exposure and development, the thin copper layer (300) on the semi-finished core board is covered by the hard dry film (CD), and the pad area (600) is exposed; The hard dry film has a thickness of 70-90 um and is pressed onto the outer surface of the semi-finished core plate by a laminating machine at a speed of 2 m per minute and a roller temperature of 100-120° C. Step 8: pattern electroplating, the exposed through holes (400) and the pad areas (600) on the core board semi-finished product obtained in step 7 are filled with copper by electroplating to form the copper pillars (101) and pads on the insulating substrate (100); Step 9: grinding and film stripping, after removing part of the electroplated copper layer formed on both sides of the semi-finished core board through a ceramic grinding process, remove the hard dry film CD) covering the thin copper layer (300) to form a pad that meets the height and diameter design requirements; Step 10: reducing copper three times, flash etching the thin copper layer (300) other than the pad on the semi-finished core board until the insulating substrate (100) at the corresponding position is exposed, thereby obtaining the core board; Step 11: Inspection before warehousing: by optical scanning, the circuit pattern produced in step 10 is compared with the design pattern, and the circuit pattern is checked and corrected; the circuit pattern is tested by peel strength test using IPC-TM-650 test method, and the bonding strength between the first pad on the core board and the insulating substrate and the copper column, and the bonding strength between the second pad and the insulating substrate, are tested; After passing the test, the products will be divided into panels, packaged and stored according to the design requirements.

2. The method for manufacturing a package substrate core board according to claim 1, characterized in that: The conductive copper layer (200) has a thickness of 15-18 μm, and the thin copper layer has a thickness of 3-8 μm; In addition, before the first copper reduction, the double-sided copper clad laminate is placed in an oven at a controlled temperature of 180° C. and baked for 60 minutes to eliminate the internal stress of the double-sided copper clad laminate.

3. The method for manufacturing a package substrate core board according to claim 2, characterized in that: The diameter of the through hole (400) is consistent with that of the copper column (101), which is 0.1-0.12 mm. The drilling speed is 185,000 revolutions per minute, the feed speed is 1.5 m per minute, and the retraction speed is 296 mm per second. After drilling, a degumming process is used to remove residual glue in the through hole (400), and then copper electroplating is performed to deposit a copper layer with a thickness of 2-4 μm in the through hole (400), so that a copper layer is formed on the bare surface of the insulating substrate in the through hole (400); Among them, the degumming rate is 0.25-0.4 mg per square centimeter, the copper deposition rate is 0.3-0.8 um, and the micro-etching rate is 0.4-1.2 um.

4. The method for manufacturing a package substrate core board according to claim 3, characterized in that: In step 4, the flash plating parameters are 6 amps per square foot and the time is 40 minutes; After flash plating, the thickness of the conductive copper layer (B) in the through hole (400) is 2-4 μm; the thickness of the surface copper layer (500) is 2-4 μm, so that the thickness of the composite copper layer (A) is 5-12 μm.

5. The method for manufacturing a package substrate core board according to claim 4, characterized in that: In step 5, before providing the photosensitive dry film (C), a flash etching process is used, and the surface of the composite copper layer (A) and the conductive copper layer (B) formed in step 4 is micro-etched by 0.5 μm at an etching rate of 0.5-1.2 μm per minute to remove the oxide layer formed on the surface of the copper layer; In addition, in step 5, an LDI exposure machine is used for exposure with an exposure energy of 110 mJ / cm2, a development speed of 3-4.5 m / min, and a development point of 50-60%.

6. The method for manufacturing a package substrate core board according to claim 5, characterized in that: In step 7, an LDI exposure machine is used to perform exposure and development with an exposure energy of 280 mJ / cm2, a development speed of 1-2 m / min, and a development point of 50-60%.

7. The method for manufacturing a package substrate core board according to claim 6, characterized in that: In step 10, a flash etching process is used to etch the thin copper layer (300) other than the pad on the semi-finished core board at a speed of 5 m per minute and a temperature of 25-35° C. until the insulating substrate (100) at the corresponding position is completely exposed.

8. The method for manufacturing a package substrate core board according to claim 7, characterized in that: The pads on the core board include any one or more of a cross shape, a square shape, and a circle shape. The first pad is a circular structure coaxially arranged with the copper column, and its diameter is 0.145-0.175 mm. The second pad is a cross-shaped or square structure, and its width is 0.09-0.11 mm.

Citation Information

Cited By