Simple and efficient gas-phase atmosphere perovskite annealing method

By pasting tape on the perovskite film and applying pressure to perform gas-phase atmosphere annealing, the problems of impurities, different grain sizes and poor flatness in the halide perovskite films in the prior art are solved, and grain uniformity is achieved The improvement of peace and flatness reduces costs and is suitable for commercial applications.

CN118946229APending Publication Date: 2024-11-12TSINGHUA UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411026133.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing halide perovskite annealing method has poor effect, resulting in many impurities in the film, different grain sizes, poor flatness, and high costs, making it difficult to meet commercial needs.

Method used

The gas-phase atmosphere annealing method is adopted, and by pasting polyimide tape on the perovskite film and applying pressure, the overall high-temperature annealing is formed to form a solvent vapor-phase atmosphere, reducing the impurity conversion activation energy, promoting grain growth and flatness, and removing impurities.

Benefits of technology

It has achieved improved grain size uniformity, improved film flatness, and reduced impurities, reducing costs, and is suitable for use in devices such as solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946229A_ABST
    Figure CN118946229A_ABST
Patent Text Reader

Abstract

The invention relates to a simple and efficient gas-phase atmosphere perovskite annealing method, which comprises the following steps of: placing a perovskite precursor solution on a substrate to form a perovskite thin film, attaching a polyimide adhesive tape to the thin film and applying pressure before an annealing step, and then integrally annealing under a perovskite annealing condition. According to the method, the perovskite material is annealed by creating a gas-phase atmosphere through a relatively simple method, so that the cost is reduced, the growth of crystal grains is promoted, impurities are reduced, the flatness of the perovskite film is improved, and the commercialization requirement can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of halide perovskite thin films and relates to a simple and efficient gas phase atmosphere perovskite annealing method. Background Art

[0002] Halide perovskites have excellent optical / X-ray absorption coefficients, long carrier lifetimes, high defect tolerance, and low-temperature processes, making them very suitable as semiconductor active layer materials in solar cells, light-emitting diodes, lasers, photodetectors, and X-ray detectors. The annealing step of semiconductor materials after preparation can effectively activate performance, reduce impurities, and improve the lattice, which has a crucial impact on device characteristics. In different preparation processes, the perovskite annealing temperature ranges from 100°C to 300°C, the environment ranges from atmospheric environment to vacuum or nitrogen environment, and the time ranges from 30s to 10min.

[0003] The existing annealing methods have poor annealing effects, which are specifically reflected in the three aspects of impurities, grain size, and flatness of the halide perovskite film obtained by annealing.

[0004] There are two main types of impurities in perovskite films. One is introduced by impure raw materials for perovskite preparation. It usually does not participate in any reaction, but its content is extremely low and can be basically ignored. The other is incompletely converted perovskite raw materials or perovskites in other crystalline phases. The perovskite raw materials or perovskites in other crystalline phases may re-react during the annealing process and be converted into the target perovskite material, thereby removing impurities and increasing the yield of the target perovskite. However, since the impurities are relatively dispersed and the reaction needs to overcome a certain activation energy, the conversion is more difficult or inefficient.

[0005] The grains in perovskite films are often large and small, and their sizes vary. During the annealing process, the grains may grow again, but the result is often that the large grains become larger and the small grains become smaller. Although this may lead to a larger average size, the variance of the overall grain size may be larger.

[0006] In the existing annealing method, the secondary growth of grains during the annealing process may grow along the substrate plane and in two directions perpendicular to the substrate, resulting in a thicker film at large grains and significantly thinner film at small grains. The film flatness may be deteriorated due to the annealing step.

[0007] CN 106128954 A discloses a method for improving the crystallinity of perovskite, which performs annealing in a dimethyl sulfoxide solvent atmosphere to improve the crystallinity of the perovskite film. However, this method has a long annealing time and does not solve the problems of impurities and flatness in the perovskite film.

[0008] Therefore, it is very necessary to develop a simple, easy and efficient annealing method for halide perovskites. Summary of the invention

[0009] Problem that the invention aims to solve

[0010] The present invention aims to provide a simple and efficient gas-phase atmosphere perovskite annealing method, which can promote grain growth, reduce impurities and improve the flatness of the perovskite film while reducing costs.

[0011] Solutions for solving problems

[0012] [1] A gas phase atmosphere perovskite annealing method comprising the following steps:

[0013] (1) After a perovskite film is prepared on a substrate, a polyimide tape is attached to the perovskite film and pressure is applied to seal the perovskite film;

[0014] (2) annealing the sealed perovskite film, polyimide tape and substrate as a whole at a temperature above 80° C. for 3-8 minutes;

[0015] Wherein, the perovskite film is prepared by a perovskite precursor solution; and the pressure is 0.1-10KPa.

[0016] [2] The method according to [1], wherein the pressure is 0.5-2 KPa, preferably 0.5-1 KPa.

[0017] [3] The method according to [1] or [2], wherein the perovskite is a halide perovskite, preferably CH3NH3PbBr3, CH3NH3PbI3, (CH3NH3)3Bi2I9, (NH3)3Bi2I9, CsPbBr3, CsPbI3, Cs2AgBiBr6, Cs3Bi2Br9, CsBiBr4 or Cs3Bi2I9, more preferably Cs2AgBiBr6.

[0018] [4] The method according to any one of [1] to [3], wherein the substrate is a silicon wafer.

[0019] [5] The method according to any one of [1] to [4], wherein in step (2), high temperature annealing is performed at a temperature of 80-300° C. for 4-6 minutes.

[0020] [6] A method for preparing a perovskite film by gas phase atmosphere annealing, comprising the following steps:

[0021] (a) taking corresponding precursor substances according to the ratio of perovskite elements, dissolving them in a solvent, heating, stirring, and dissolving them to obtain a perovskite precursor solution;

[0022] (b) placing the perovskite precursor solution prepared in step (a) on a substrate to form a liquid film, and converting the liquid film into a perovskite film;

[0023] (c) annealing the perovskite film prepared in step (b) according to the gas phase atmosphere perovskite annealing method described in any one of [1] to [5], removing the polyimide tape, and obtaining a gas phase atmosphere annealed perovskite film.

[0024] [7] The preparation method according to [6], wherein in step (a), the solvent is DMSO.

[0025] [8] The preparation method according to [6] or [7], wherein in step (b), the perovskite precursor solution is formed into a liquid film by spin coating, blade coating or spray coating.

[0026] [9] The preparation method according to any one of [6] to [8], wherein in step (b), the liquid film is converted into a perovskite film by an anti-solvent method, a natural volatilization method, a vacuum volatilization method, a low-temperature volatilization method or a heating crystallization method.

[0027]

[10] A gas phase atmosphere annealed perovskite film, which is prepared by the preparation method described in any one of [6]-[9].

[0028] Effects of the Invention

[0029] The technical effects of the present invention are embodied in the following aspects:

[0030] (1) Through the airtightness of the tape and the application of pressure, the perovskite is placed in a sealed condition, which can retain a small amount of solvent remaining in the spin-coated film to a limited extent, forming a solvent gas phase atmosphere, reducing the activation energy of the conversion of the impurity phase perovskite to the target phase perovskite, and dissolving smaller grains, promoting the regrowth of large grains, and improving the size uniformity of the grains;

[0031] (2) The presence of the tape can limit the growth space of the perovskite grains perpendicular to the substrate surface, prompting the grains to grow more horizontally along the substrate, thereby improving the flatness of the film;

[0032] (3) After annealing, the tape is removed without introducing new impurities, and the impurities in the perovskite raw material are absorbed and removed along with the tape, thereby reducing the impurity content in the perovskite film;

[0033] (4) The annealing method of the present invention has simple steps, is easy to operate, does not require the use of special equipment or materials, and has low cost.

[0034] In summary, the present invention creates a gas phase atmosphere to anneal the perovskite material through a relatively simple method, which can promote grain growth, reduce impurities, and improve flatness while reducing costs, thereby meeting commercial needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of perovskite films obtained by the annealing method of the present invention (upper route) and the traditional annealing method (lower route).

[0036] Figure 2 The top views are scanning electron microscope images of the gas phase atmosphere annealed perovskite film prepared in the embodiment and the perovskite film prepared in the comparative example at different scales.

[0037] Figure 3 Transverse images of scanning electron microscope images of the gas phase atmosphere annealed perovskite film prepared in the embodiment and the perovskite film prepared in the comparative example.

[0038] Figure 4 Statistical graphs of particle size distribution of the gas phase atmosphere annealed perovskite film prepared in the example and the comparative example. DETAILED DESCRIPTION

[0039] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.

[0040] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.

[0041] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0042] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0043] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0044] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0045] In the present specification, when "normal temperature" or "room temperature" is used, the temperature may be 15°C to 30°C, further 15°C to 25°C, for example, 20°C.

[0046] The existing halide perovskite annealing method uses a hot plate or an oven to heat the prepared halide perovskite material at 100°C, 280°C or 300°C for 30s to 10min in an environment such as atmosphere, nitrogen or vacuum. The annealing effect is poor, which is specifically reflected in the fact that the halide perovskite film obtained by annealing has more impurities, different grain sizes, and poor film flatness.

[0047] The present invention provides a perovskite annealing method in a gas phase atmosphere, wherein a perovskite precursor solution is spin-coated on a substrate to form a preliminary perovskite film, and then immediately before the annealing step, a tape (such as a polyimide tape) with stable chemical properties, high temperature resistance, and low residual adhesive is closely attached to the film, and then the whole is annealed under the perovskite film annealing conditions. Through the air tightness of the tape and the application of pressure, a small amount of solvent remaining in the spin-coated film can be limitedly retained to form a solvent gas phase atmosphere, reduce the activation energy of the impurity phase perovskite to the target phase perovskite conversion, and dissolve smaller grains, promote the growth of large grains again, and improve the size uniformity of the grains. And the presence of the tape can limit the growth space of the perovskite grains perpendicular to the substrate surface, and promote the grains to grow again more horizontally along the substrate, thereby improving the flatness of the film. After the annealing is completed, the tape is removed, and new impurities can be introduced without absorbing the impurities carried by the perovskite raw material, and removed together with the tape, thereby reducing the impurity content in the perovskite film.

[0048] <Gas atmosphere perovskite annealing method>

[0049] Specifically, the present invention provides a gas phase atmosphere perovskite annealing method, which comprises the following steps:

[0050] (1) After a perovskite film is prepared on a substrate, a polyimide (PI) tape is attached to the perovskite film and pressure is applied to seal the perovskite film;

[0051] (2) annealing the sealed perovskite film, polyimide tape and substrate as a whole at a temperature above 80° C. for 3-8 minutes;

[0052] Wherein, the perovskite film is prepared by a perovskite precursor solution; and the pressure is 0.1-10KPa.

[0053] In step (1), the pressure is applied mainly to make the polyimide tape and the perovskite film fit more closely, and to limit the growth of the perovskite grains in a direction perpendicular to the substrate, thereby improving the flatness of the film. In some embodiments, in step (1), if no pressure is applied, the flatness of the film will be relatively poor.

[0054] In some specific embodiments, the pressure is 0.5-2 KPa, preferably 0.5-1 KPa, such as 0.5, 0.6, 0.8, 1 KPa.

[0055] In some specific embodiments, the perovskite is a halide perovskite. The types of perovskites include, but are not limited to, CH3NH3PbBr3, CH3NH3PbI3, (CH3NH3)3Bi2I9, (NH3)3Bi2I9, CsPbBr3, CsPbI3, Cs2AgBiBr6, Cs3Bi2Br9, CsBiBr4 or Cs3Bi2I9. In some preferred embodiments, the perovskite is Cs2AgBiBr6.

[0056] In some specific embodiments, the substrate is made of silicon material, for example, the substrate is a silicon wafer.

[0057] The annealing conditions in step (2) can be arbitrarily adapted to the type of perovskite at a temperature above 80 degrees by any heating instrument or device, as well as the length of annealing time of the perovskite. In some specific embodiments, in step (2), the sealed perovskite film, polyimide tape and substrate are annealed at a temperature of 80-300°C for 4-6 minutes.

[0058] <Method for preparing perovskite thin film by gas phase atmosphere annealing>

[0059] The present invention also provides a method for preparing a gas phase atmosphere annealed perovskite film, which comprises the following steps:

[0060] (a) taking corresponding precursor substances according to the ratio of perovskite elements, dissolving them in a solvent, heating, stirring, and dissolving them to obtain a perovskite precursor solution;

[0061] (b) placing the perovskite precursor solution prepared in step (a) on a substrate to form a liquid film, and converting the liquid film into a perovskite film;

[0062] (c) annealing the perovskite film prepared in step (b) according to the above-mentioned <gas phase atmosphere perovskite annealing method>, removing the polyimide tape, and obtaining a gas phase atmosphere annealed perovskite film.

[0063] In some specific embodiments, the perovskite is a halide perovskite. The types of perovskites include, but are not limited to, CH3NH3PbBr3, CH3NH3PbI3, (CH3NH3)3Bi2I9, (NH3)3Bi2I9, CsPbBr3, CsPbI3, Cs2AgBiBr6, Cs3Bi2Br9, CsBiBr4 or Cs3Bi2I9. In some preferred embodiments, the perovskite is Cs2AgBiBr6.

[0064] The solvent in step (a) is not particularly limited, as long as it can dissolve the precursor material. In some specific embodiments, the solvent is DMSO (dimethyl sulfoxide).

[0065] In some specific embodiments, the substrate is made of silicon material, for example, the substrate is a silicon wafer.

[0066] In some specific embodiments, in step (b), the perovskite precursor solution is formed into a liquid film by spin coating (e.g., spin coating in which the liquid is dispersed by centrifugal force), scraping (e.g., scraping in which the liquid is dispersed by a scraper), or spraying (e.g., spraying by atomizing the precursor solution).

[0067] In some specific embodiments, in step (b), the liquid film is converted into a perovskite film by an anti-solvent method (the solvent may be ethanol or isopropanol), a natural volatilization method, a vacuum volatilization method, a low-temperature volatilization method, or a heating crystallization method.

[0068] <Perovskite thin film annealed in gas phase atmosphere>

[0069] In addition, the present invention also provides a gas phase atmosphere annealed perovskite film, which is prepared by the above <Preparation method of gas phase atmosphere annealed perovskite film>. The gas phase atmosphere annealed perovskite film prepared by the present invention has high flatness, uniform grain size, and less impurities, and has very excellent performance, and is very suitable for use in solar cells, light emitting diodes, lasers, photodetectors, X-ray detectors and other devices.

[0070] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0071] Example

[0072] (1) Preparation of precursor solution

[0073] According to the ratio of perovskite elements, the corresponding precursor substances are weighed and dissolved in the solvent, heated, stirred, and dissolved to obtain a perovskite precursor solution. Taking cesium silver bismuth bromide perovskite (Cs2AgBiBr6) as an example, 1171.5 mg of cesium bromide (CsBr) powder, 517 mg of silver bromide (AgBr) powder, and 1237.5 mg of bismuth bromide (BiBr3) powder are weighed, dissolved in 5 mL of dimethyl sulfoxide (DMSO), heated to 120°C, and stirred with a magnetic stirrer until completely dissolved to obtain a perovskite precursor solution with a concentration of 0.55 mol / L.

[0074] (2) Preparation of preliminary perovskite films

[0075] The precursor solution prepared in step (1) is formed into a film on a substrate. By spin coating, a silicon wafer with a silicon material substrate is first prepared, and the hydrophilic and hydrophobic properties of the surface are improved by oxygen plasma treatment. Then, an appropriate amount of the precursor solution is dripped on the substrate, and a spin coating instrument is used to form a liquid film by spin coating at a speed of 700 rpm for 10 seconds followed by 3000 rpm for 40 seconds. In this process, an anti-solvent method (the solvent is ethanol) is used to form a preliminary perovskite film.

[0076] (3) Vapor atmosphere annealing

[0077] After the preliminary perovskite film is prepared, the surface is then sealed by adhering a sealing material. A polyimide (PI) tape is pasted on the preliminary perovskite film and a pressure of 1 KPa is applied. Subsequently, the preliminary perovskite film is annealed at 280°C for 5 minutes along with the substrate and the tape, and then the tape is removed to obtain a gas-phase atmosphere annealed perovskite film. The roadmap is shown in Figure 1 In the upper route, the perovskite film obtained by the annealing method of the present invention has high flatness, uniform grain size, and less impurities, indicating that the annealing method of the present invention has achieved excellent technical effects.

[0078] Comparative Example

[0079] After the preliminary perovskite film is prepared according to the method of the above embodiment, the substrate is annealed at 280°C for 5 minutes to obtain a perovskite film prepared by a conventional annealing method. Figure 1 In the lower route, the perovskite film produced by the traditional annealing method has poor flatness, uneven grain sizes, and more impurities.

[0080] The scanning electron microscope (SEM) images of the gas phase atmosphere annealed perovskite film prepared in the embodiment and the perovskite film prepared in the comparative example are shown in FIG. Figure 2 and Figure 3 ,in, Figure 2 is a top view, Figure 3 is a cross-sectional view. Figure 2 It can be seen that the perovskite film annealed in gas phase atmosphere has better size, better uniformity and fewer pinholes. Figure 3 It can be seen that, by using the conventional annealing method in the comparative example, the perovskite film is a multilayer film, and by using the gas phase atmosphere annealing method in the embodiment, the perovskite film is a compact single-layer film.

[0081] The particle size distribution statistics of the gas phase atmosphere annealed perovskite film prepared in the embodiment and the perovskite film prepared in the comparative example are shown in FIG. Figure 4 .Depend on Figure 4 It can be seen that by using the gas phase atmosphere annealing method in the embodiment, the size of the perovskite grains is relatively large, with the maximum reaching about 400 nm.

[0082] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.

[0083] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A gas phase atmosphere perovskite annealing method comprising the following steps: (1) After a perovskite film is prepared on a substrate, a polyimide tape is attached to the perovskite film and pressure is applied to seal the perovskite film; (2) annealing the sealed perovskite film, polyimide tape, and substrate at a temperature above 80° C. for 3-8 minutes; in, The perovskite film is prepared from a perovskite precursor solution; and the pressure is 0.1-10 KPa.

2. The method according to claim 1, characterized in that The pressure is 0.5-2KPa, preferably 0.5-1KPa.

3. The method according to claim 1 or 2, characterized in that The perovskite is a halide perovskite, preferably CH3NH3PbBr3, CH3NH3PbI3, (CH3NH3)3Bi2I9, (NH3)3Bi2I9, CsPbBr3, CsPbI3, Cs2AgBiBr6, Cs3Bi2Br9, CsBiBr4 or Cs3Bi2I9, more preferably Cs2AgBiBr6.

4. The method according to any one of claims 1 to 3, characterized in that The substrate is a silicon wafer.

5. The method according to any one of claims 1 to 4, characterized in that In step (2), high temperature annealing is performed at a temperature of 80-300° C. for 4-6 minutes.

6. A method for preparing a perovskite film by gas phase atmosphere annealing, comprising the following steps: (a) taking a corresponding precursor material according to the ratio of perovskite elements, dissolving it in a solvent, heating, stirring, and dissolving it to obtain a perovskite precursor solution; (b) placing the perovskite precursor solution prepared in step (a) on a substrate to form a liquid film, and converting the liquid film into a perovskite thin film; (c) annealing the perovskite film prepared in step (b) according to the vapor atmosphere perovskite annealing method according to any one of claims 1 to 5, removing the polyimide tape, and obtaining a vapor atmosphere annealed perovskite film.

7. The preparation method according to claim 6, characterized in that In step (a), the solvent is DMSO.

8. The preparation method according to claim 6 or 7, characterized in that In step (b), the perovskite precursor solution is formed into a liquid film by spin coating, doctor blade coating or spray coating.

9. The preparation method according to any one of claims 6 to 8, characterized in that In step (b), the liquid film is converted into a perovskite film by an anti-solvent method, a natural volatilization method, a vacuum volatilization method, a low-temperature volatilization method or a heating crystallization method.

10. A gas phase atmosphere annealed perovskite film, prepared by the preparation method according to any one of claims 6 to 9.

Citation Information

Cited By

  • Gas phase annealing method and annealing device for perovskite thin film

    CN122555363A