Simulation memristor of rare earth element doped amorphous tungsten oxide film and preparation method of simulation memristor

By doping amorphous tungsten oxide film with rare earth elements as the storage layer of simulated memristors, the reliability problem of simulated memristors in neuromorphic systems is solved, and the simulated resistance change performance with high symmetry and wide dynamic regulation range is achieved. , suitable for nonvolatile memory and in-memory computing.

CN118946248APending Publication Date: 2024-11-12SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410992294.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The large-scale application of existing simulated memristors on neuromorphic systems is limited by their reliability issues such as degraded durability and retention performance, read/write noise and interference, and the lack of high symmetry, high linearity and width High-performance analog memristor for dynamic regulation range.

Method used

Rare earth element-doped amorphous tungsten oxide film is used as the storage layer for simulated memristors. Rare earth is realized by depositing conductive films on the substrate as the bottom electrode and the top electrode, combined with physical vapor deposition and magnetron sputtering or laser deposition technology. The uniform doping of elements regulates the electrical properties of the resistive change layer.

Benefits of technology

It realizes analog resistance change performance with high symmetry, high linearity and large dynamic regulation range, improves the reliability and stability of analog memristors, and has broad application prospects in the fields of nonvolatile memory and in-memory computing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946248A_ABST
    Figure CN118946248A_ABST
Patent Text Reader

Abstract

The invention discloses a simulation memristor of a rare earth element doped amorphous tungsten oxide thin film and a preparation method thereof, and belongs to the technical field of nonvolatile memorizers, and the preparation method comprises the following steps: depositing a conductive thin film on a substrate as a bottom electrode thin film of the simulation memristor; then, a rare earth element doped amorphous tungsten oxide film is deposited on the bottom electrode film to serve as a storage layer for simulating the memristor; and finally, depositing a conductive thin film on the storage layer to serve as a top electrode thin film for simulating the memristor. And obtaining the analog memristor of the rare earth element doped amorphous tungsten oxide film. The rare earth element doped and modified amorphous tungsten oxide thin film is used as a storage layer of the analog memristor, the analog resistance change performance with high symmetry, high linearity and large dynamic regulation and control range is realized, the analog resistance change performance is stable, the cost is low, the preparation process is compatible with the COMS process, large-scale production is facilitated, and the method is suitable for large-scale production. The method has an excellent application prospect in the technical field of in-memory calculation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of non-volatile memory, and in particular relates to an analog memristor of a rare earth element doped amorphous tungsten oxide film and a preparation method thereof. Background Art

[0002] A memristor is a circuit element whose resistance value can change with the change of charge or voltage passing through it, and this change has memory. Memristors have broad application prospects and advantages in future electronic devices and systems due to their non-volatility, high storage density, low power consumption, fast read and write speeds, and versatility. In particular, analog non-volatile memory devices capable of multiple states, like memristors, are expected to realize new energy-saving technologies such as in-memory computing and neuromorphic computing, subverting traditional graphics GPU-based neural network accelerators.

[0003] With the demand for new energy-saving hardware in artificial intelligence, analog memristors, which have emerged in neuromorphic computing systems based on analog resistive switches, have attracted widespread attention in recent years. Unlike the more studied binary digital memristor characteristics, analog memristors have the ability to continuously controllable conductance tuning. Although the research on analog memristors has achieved important results, there are still few large-scale studies on neuromorphic systems. The main bottleneck is the reliability problem of analog memristors, such as durability and retention performance degradation, read / write noise and interference. Due to the complexity of the resistive switch mechanism, it is challenging to conduct in-depth research on the root causes of its reliability degradation and propose corresponding optimization methods. Therefore, it is of great significance to realize analog memristors with high symmetry, high linearity and wide dynamic control range. In response to the above problems, one of the main strategies is to modify and regulate the mainstream memristor storage materials to achieve high-performance analog memristor devices. Rare earth element doping of oxide films is a commonly used material modification technology. By doping with rare earth elements, the physical and chemical properties of oxide films, such as optical, electrical, magnetic and structural properties, can be significantly improved. In particular, by selecting appropriate rare earth elements and doping methods, the conductivity, dielectricity and semiconductor properties of the resistive film can be precisely controlled, thereby achieving high-performance analog resistive performance.

[0004] Currently, the large-scale application of analog memristors in neuromorphic systems is limited by reliability issues such as degradation of durability and retention performance, read / write noise and interference, and the lack of high-performance analog memristors with high symmetry, high linearity, and wide dynamic range. There are no reports on the use of amorphous tungsten oxide thin films as memristor storage layers and the controllable doping of rare earth elements to achieve high-performance analog memristors. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing an analog memristor of amorphous tungsten oxide film doped with rare earth elements, so as to solve the technical problems that the existing analog memristors lack high symmetry, high linearity and wide dynamic control range.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention discloses a method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide film, comprising:

[0008] First, a conductive film is deposited on a substrate as a bottom electrode film of an analog memristor; then, an amorphous tungsten oxide film doped with rare earth elements is deposited on the bottom electrode film as a storage layer of the analog memristor; finally, a conductive film is deposited on the storage layer as a top electrode film of the analog memristor; and an analog memristor of amorphous tungsten oxide film doped with rare earth elements is obtained.

[0009] Preferably, the conductive film is deposited on the substrate by physical vapor deposition.

[0010] Preferably, the substrate is a highly insulating and flat glass or intrinsic silicon wafer.

[0011] Preferably, the conductive film is any one of ITO, FTO, Au, Pt, W and TiN having low electrochemical activity.

[0012] Preferably, the thickness of the conductive film is 60-300 nanometers.

[0013] Preferably, the target material is sputtered or laser-bombarded by physical vapor deposition, magnetron sputtering or laser deposition, so that the rare earth element is uniformly doped in the amorphous tungsten oxide film to obtain a rare earth element-doped amorphous tungsten oxide film.

[0014] Preferably, the rare earth element is uniformly doped into the amorphous tungsten oxide film by co-sputtering or laser bombarding of a tungsten-based target and a rare earth element target, thereby obtaining a rare earth element-doped amorphous tungsten oxide film.

[0015] Preferably, in the rare earth element doped amorphous tungsten oxide film, the doped rare earth element is any one of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium and erbium; the thickness of the rare earth element doped amorphous tungsten oxide film is 20-200 nanometers.

[0016] Preferably, the conditions for depositing amorphous tungsten oxide film doped with rare earth elements on the bottom electrode film are: deposition at 50-300°C for 5-25 minutes in an argon and oxygen atmosphere; the argon flow rate is 10-40sccm; the oxygen flow rate is 5-20sccm; and the deposition power is 50-200 watts.

[0017] The invention also discloses a rare earth element doped amorphous tungsten oxide film analog memristor, which is prepared by the above preparation method and comprises, from bottom to top, a bottom electrode, an amorphous tungsten oxide film uniformly doped with rare earth elements and a top electrode.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention discloses a method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide film, wherein the amorphous tungsten oxide film modified by rare earth element doping is used as the storage layer of the analog memristor, and an analog resistive switching performance with high symmetry, high linearity and a large dynamic control range is achieved, and the analog memristor has broad application prospects in the fields of non-volatile memory and in-memory computing. The currently reported memristors have certain limitations in achieving analog memristive performance with high symmetry, high linearity and a large dynamic control range. Amorphous tungsten oxide is an ideal storage material for the resistive switching layer of a memristor device due to its excellent electrical and physical properties. Although it has significant advantages in digital memristors, it has problems in analog resistive switching performance. Therefore, the present invention dopes an amorphous tungsten oxide film with rare earth elements, thereby regulating the oxygen vacancies in the resistive switching layer, and obtaining a memristor with excellent analog resistive switching performance.

[0020] Furthermore, choosing highly insulating and highly flat glass as the substrate provides the possibility for later light-controlled adjustment of the analog memristor performance; choosing highly insulating and highly flat intrinsic silicon wafers as the substrate is compatible with the current mainstream COMS process, which facilitates rapid large-scale tape-out on current mainstream chip devices and realizes rapid large-scale preparation.

[0021] Furthermore, physical vapor deposition is used to deposit the bottom and top conductive films of the device. This method has high controllability, low cost, economy and environmental protection, and the prepared conductive film is of high quality. One of ITO, FTO, Au, Pt, W and TiN with low electrochemical activity is selected as the electrode material to reduce the influence of the electrode on the resistive switching performance, so that the simulated resistive switching performance of the device is more stable.

[0022] Furthermore, the thickness of the bottom and top conductive films of the analog memristor is between 60 and 300 nanometers. The thickness of the electrode is one of the factors affecting the reliability of the device. An electrode that is too thin below 60 nanometers will reduce the stability of the device. An electrode that is over 600 nanometers will cause excessive internal stress between the electrode and the resistive switching layer, resulting in poor stability of the interface. Therefore, 60-300 nanometers is the most suitable.

[0023] Furthermore, magnetron sputtering is used to prepare the resistive layer film. The sputtering method has the advantages of low cost, high reliability, and high quality of the prepared film. In particular, the prepared dielectric film has very high controllability. Laser deposition is used to bombard the target material with laser. The laser bombardment power is high and the prepared film composition selectivity is high. It is also one of the important methods for preparing dielectric films.

[0024] Furthermore, the rare earth elements are uniformly doped in the amorphous tungsten oxide film by co-sputtering or laser bombarding of tungsten-based targets and rare earth element targets. Co-sputtering is the best strategy to achieve uniform doping in physical vapor deposition coating technology. By stably controlling the sputtering power and other parameters of each target, the concentration and uniformity of doping can be precisely controlled, thereby achieving uniform doping of rare earth elements in the amorphous tungsten oxide film.

[0025] Furthermore, the doped rare earth element is any one of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium and erbium. The amorphous tungsten oxide film doped with the above rare earth elements can effectively regulate the electrical properties of the film and has high stability, thereby effectively regulating the analog resistive switching performance of the memristor.

[0026] Furthermore, the target materials are high-purity metal rare earth target materials and tungsten target materials. High-purity metal rare earth target materials can introduce less impurities; metal rare earth target materials can effectively control the concentration of oxygen vacancies in the film by adjusting the oxygen composition ratio, growth power and other parameters during the film preparation process, thereby achieving the regulation of the resistive switching layer to remove the conductive filaments and achieving excellent simulated resistive switching performance.

[0027] Furthermore, when the deposition temperature of the resistive layer is lower than 50°C, the flatness of the prepared film is reduced, affecting the performance of the memristor. When the temperature of the grown film exceeds 300°C, the defect concentration of the film is reduced, thereby reducing the analog resistive performance of the memristor. When the flow rate of argon gas is in the range of 10-40sccm, too low a flow rate will result in sputtering failure and film deposition failure. When the flow rate of argon gas is too high, the working gas pressure will be reduced, and the quality of the grown resistive layer film will be reduced. When the flow rate of oxygen gas is in the range of 5-20sccm, too high a flow rate of oxygen gas will result in poor conductivity. The defect concentration of amorphous tungsten oxide is too high, while that of amorphous tungsten oxide is too low. Both of them will affect the resistive switching performance of the memristor. The deposition time is between 5 and 25 minutes. If the deposition time is less than 5 minutes, the film thickness is too thin, and the memristor is easily broken down. If the deposition time is more than 25 minutes, the film thickness is too thick, and the analog resistive switching performance of the memristor deteriorates. The power is between 50 and 200 watts. If the power is too low, the film growth is too slow. If the power is more than 200 watts, the flatness of the film is reduced, thus affecting the performance of the constructed memristor.

[0028] Furthermore, the thickness of the rare earth element uniformly doped amorphous tungsten oxide film is between 20-200 nanometers. If the film thickness is too thin (less than 20 nanometers), the prepared memristor is easily broken down; if the film thickness is too thick (more than 200 nanometers), the analog resistive switching performance of the memristor deteriorates.

[0029] The present invention also discloses an analog memristor of a rare earth element-doped amorphous tungsten oxide thin film prepared by the above preparation method, which has the advantages of stable analog resistive switching performance, low cost, and a preparation process compatible with a COMS process, is conducive to large-scale production, and has excellent application prospects in market fields such as in-memory computing. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic structural diagram of the analog memristor of the rare earth element doped amorphous tungsten oxide film disclosed in the present invention;

[0031] Figure 2 This is the XRD pattern of the yttrium-doped amorphous tungsten oxide film prepared in Example 1 of the present invention;

[0032] Figure 3 The voltage-current curve of the yttrium-doped amorphous tungsten oxide thin film analog memristor prepared in Example 1 of the present invention;

[0033] Figure 4 This is a cycle characteristic curve diagram of the yttrium-doped amorphous tungsten oxide thin film analog memristor prepared in Example 1 of the present invention;

[0034] Figure 5 The voltage-current curves of the yttrium-doped amorphous tungsten oxide thin film analog memristor prepared in Example 1 of the present invention under different limiting current conditions. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0036] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0037] In the present invention, unless otherwise specified, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution.

[0038] In the present invention, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.

[0039] In the present invention, unless otherwise specified, percentage (%) or part refers to the weight percentage or weight part relative to the composition.

[0040] In the present invention, unless otherwise specified, the components or preferred components involved can be combined with each other to form a new technical solution.

[0041] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "6-22" means that all real numbers between "6-22" have been listed in this document, and "6-22" is just an abbreviation of these numerical combinations.

[0042] The “range” disclosed in the present invention is in the form of a lower limit and an upper limit, which can be one or more lower limits, and one or more upper limits, respectively.

[0043] In the present invention, the term "and / or" used herein refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0044] In the present invention, unless otherwise specified, each reaction or operation step can be carried out sequentially or in accordance with the sequence. Preferably, the reaction method herein is carried out sequentially.

[0045] Unless otherwise specified, the professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content may also be applied to the present invention.

[0046] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0047] The present invention discloses a method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide film, comprising: depositing a conductive film on a suitable substrate as a bottom electrode film of the analog memristor; depositing a rare earth element doped amorphous tungsten oxide film on the bottom electrode film as a storage layer of the analog memristor; and depositing a conductive film on the storage layer as a top electrode of the analog memristor, to prepare an analog memristor based on the rare earth element doped amorphous tungsten oxide film.

[0048] Specifically, the substrate is a highly insulating and flat glass or an intrinsic silicon wafer.

[0049] Specifically, physical vapor deposition is used to deposit one of ITO, FTO, Au, Pt, W and TiN with low electrochemical activity as the bottom conductive film and the top conductive film of the analog memristor.

[0050] Furthermore, the thickness of the bottom conductive film and the top conductive film are both in the range of 60-300 nanometers.

[0051] Specifically, the target material is sputtered or laser bombarded by magnetron sputtering or laser deposition.

[0052] Specifically, a tungsten-based target material and a rare earth element target material are co-sputtered or laser-bombarded to achieve uniform doping of the rare earth element into the amorphous tungsten oxide film.

[0053] Specifically, the doped rare earth element is any one of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium and erbium.

[0054] Specifically, the target material is a high-purity metal rare earth target material and a tungsten target material.

[0055] Specifically, the deposition temperature of the storage layer is between 50-300° C.; the flow rates of argon and oxygen are 10-40 sccm and 5-20 sccm respectively; the deposition time is 5-25 minutes; and the power is 50-200 watts.

[0056] Specifically, the thickness of the rare earth element doped amorphous tungsten oxide film is 20-200 nanometers.

[0057] The present invention provides an analog memristor based on rare earth element doped amorphous tungsten oxide film, the structure of the device is a high flat substrate, a bottom conductive electrode, an yttrium doped amorphous tungsten oxide film analog resistive storage layer and a top conductive electrode from bottom to top, belonging to the field of non-volatile memory. The preparation method of the present invention, relative to the digital switching characteristics of the undoped tungsten oxide film memristor, the rare earth element doped tungsten oxide film memristor has stable analog resistive switching performance, and the analog memristive characteristics of the device are achieved by controlling the forward and reverse cut-off voltages.

[0058] See also Figure 1 This is a schematic diagram of the structure of the simulated memristor of the rare earth element doped amorphous tungsten oxide film disclosed in the present invention; as can be seen from the figure, from bottom to top it includes a highly flat substrate, a bottom electrode, a rare earth element doped amorphous tungsten oxide film simulated resistive storage layer and a top electrode, and the top electrode and the bottom electrode are connected through the rare earth element doped amorphous tungsten oxide film.

[0059] The present invention discloses a method for preparing a simulated memristor of a rare earth element doped amorphous tungsten oxide thin film, which specifically comprises the following steps:

[0060] S1. Select glass or intrinsic silicon wafer with high insulation and high flatness as substrate, and deposit a conductive film of ITO, FTO, Au, Pt, W and TiN with a thickness of 60-300 nanometers and low electrochemical activity on the substrate by physical vapor deposition as the bottom electrode film of the analog memristor;

[0061] Preferably, the substrate is an intrinsic silicon wafer with high insulation and high flatness.

[0062] Preferably, the bottom electrode is selected to be Pt which has low electrochemical activity.

[0063] Preferably, the thickness of the bottom Pt electrode is 100 nanometers.

[0064] S2. Sputter or laser bombard the target material by magnetron sputtering or laser deposition, and deposit one of the rare earth elements scandium, yttrium, lanthanum, cerium, praseodymium, neodymium and erbium by co-sputtering. The target material for sputtering or laser deposition is a high-purity metal rare earth target and a tungsten target; the deposition temperature is between 50-300°C, the flow rates of argon and oxygen are 10-40sccm and 5-20sccm respectively, the deposition time is 5-25 minutes, and the power is 50-200 watts. Obtain an amorphous tungsten oxide film uniformly doped with rare earth elements as a storage layer for simulating memristor resistance.

[0065] Preferably, the sputtering deposition is performed by magnetron sputtering.

[0066] Preferably, a co-sputtering method of rare earth elements and tungsten target is adopted.

[0067] Preferably, the rare earth element yttrium is doped.

[0068] Preferably, the deposition temperature is 250° C.; the flow rates of argon and oxygen are 30 sccm and 10 sccm respectively; the deposition time is 10 minutes; and the power is 100 watts.

[0069] S3. Deposit a conductive film of ITO, FTO, Au, Pt, W and TiN with a thickness of 60-300 nanometers and low electrochemical activity by physical vapor deposition as the top electrode film of the simulated memristor; obtain a simulated memristor of rare earth element-doped amorphous tungsten oxide film.

[0070] Preferably, the bottom electrode is selected to be Pt which has low electrochemical activity.

[0071] Preferably, the thickness of the bottom Pt electrode is 100 nanometers.

[0072] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings here can usually be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0073] Example 1

[0074] A method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film, comprising:

[0075] 1) A highly insulating and flat intrinsic silicon wafer is selected as the substrate, and a Pt conductive film with a thickness of 100 nanometers and low electrochemical activity is deposited by physical vapor deposition as the bottom electrode film of the analog memristor.

[0076] 2) The target material is sputtered and bombarded by magnetron sputtering, and the rare earth element yttrium is deposited by co-sputtering. The sputtering target material is a high-purity metal rare earth target material and a tungsten target material; the deposition temperature is 250°C, the flow rates of argon and oxygen are 30sccm and 10sccm respectively, the deposition time is 10 minutes, and the power is 100 watts. The amorphous tungsten oxide film uniformly doped with the rare earth element yttrium is realized as the storage layer of the analog memristor, and the thickness of the amorphous tungsten oxide film doped with the rare earth element yttrium is 50 nanometers.

[0077] 3) A W conductive film with a thickness of 100 nanometers and low electrochemical activity is deposited by physical vapor deposition as a top electrode film of the simulated memristor; and a simulated memristor of amorphous tungsten oxide film doped with rare earth elements is obtained.

[0078] The schematic diagram of the structure of the simulated memristor of the rare earth element yttrium-doped amorphous tungsten oxide film constructed in this embodiment 1, the device comprises, from bottom to top, a highly flat substrate, a bottom conductive electrode, a yttrium-doped amorphous tungsten oxide film simulated resistive storage layer and a top conductive electrode.

[0079] See also Figure 2 , is the XRD pattern of the yttrium-doped amorphous tungsten oxide film of the simulated memristor constructed in Example 1. It can be seen that no obvious diffraction peak is observed, indicating that the prepared resistive switching layer film is amorphous.

[0080] See also Figure 3 , is a voltage-current curve diagram of the yttrium-doped amorphous tungsten oxide thin film analog memristor constructed in Example 1. It can be seen that the constructed memristor has a stable bipolar analog resistive switching characteristic, which is conducive to its application in the fields of storage and in-memory computing.

[0081] See also Figure 4 , which is the cycle characteristic curve of the yttrium-doped amorphous tungsten oxide thin film analog memristor constructed in Example 1. It can be seen that the analog memristor has good cycle characteristics and still maintains high stability after nearly 200 cycles.

[0082] See also Figure 5 , which is a voltage-current curve of the yttrium-doped amorphous tungsten oxide thin film analog memristor under different limiting currents constructed in Example 1. It can be seen that good analog memory characteristics are exhibited under different limiting currents, indicating that the memristor has excellent analog resistive switching performance.

[0083] Example 2

[0084] A method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film, comprising:

[0085] 1) Highly insulating and highly flat glass is selected as the substrate, and a 100-nanometer-thick ITO conductive film with low electrochemical activity is deposited by physical vapor deposition as the bottom electrode film of the analog memristor.

[0086] 2) The target material is laser bombarded by laser deposition, and the rare earth element scandium is deposited by co-laser bombardment. The bombardment target materials are high-purity metal rare earth target and tungsten target; the deposition temperature is 250°C, the flow rates of argon and oxygen are 30sccm and 10sccm respectively, the deposition time is 10 minutes, and the power is 100 watts. An amorphous tungsten oxide film uniformly doped with the rare earth element scandium is obtained as the storage layer of the simulated memristor, and the thickness of the amorphous tungsten oxide film doped with the rare earth element scandium is 50 nanometers.

[0087] 3) Using physical vapor deposition to deposit an ITO conductive film with a thickness of 100 nanometers and low electrochemical activity as a top electrode film of the simulated memristor; obtaining a simulated memristor of amorphous tungsten oxide film doped with rare earth elements.

[0088] Compared with Example 1, the analog memristor prepared in Example 2 uses scandium as the doping element, the bottom electrode and the top electrode are ITO, and the deposition of the analog resistive layer is carried out by laser deposition. Compared with sputtering, the uniformity of the film needs to be improved, resulting in the performance of the constructed analog memristor needs to be further improved.

[0089] Example 3

[0090] A method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film, comprising:

[0091] 1) A highly insulating and flat intrinsic silicon wafer was selected as the substrate, and a 60-nanometer-thick FTO conductive film with low electrochemical activity was deposited by physical vapor deposition as the bottom electrode film of the simulated memristor.

[0092] 2) The target material is sputtered and bombarded by magnetron sputtering, and the rare earth element lanthanum is deposited by co-sputtering. The sputtering target material is a high-purity metal rare earth target material and a tungsten target material; the deposition temperature is 50°C, the flow rates of argon and oxygen are 30ccm and 10ccm respectively, the deposition time is 10 minutes, and the power is 100 watts. An amorphous tungsten oxide film uniformly doped with the rare earth element lanthanum is obtained as the storage layer of the simulated memristor, and the thickness of the amorphous tungsten oxide film doped with the rare earth element lanthanum is 50 nanometers.

[0093] 3) A 60-nanometer-thick FTO conductive film with low electrochemical activity is deposited by physical vapor deposition as a top electrode film of the simulated memristor; and a simulated memristor of amorphous tungsten oxide film doped with rare earth elements is obtained.

[0094] Compared with Example 1, the analog memristor prepared in Example 3 uses lanthanum as the doping element, the bottom electrode and the top electrode are FTO, the substrate temperature is low, the thickness of the electrode is thin, and the lower deposition temperature leads to a decrease in the intrinsic defect concentration of the film, and the analog resistive switching performance needs to be improved.

[0095] Example 4

[0096] A method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film, comprising:

[0097] 1) A highly insulating and flat intrinsic silicon wafer is selected as the substrate, and a 300-nanometer-thick Au conductive film with low electrochemical activity is deposited by physical vapor deposition as the bottom electrode film of the analog memristor.

[0098] 2) The target material is sputtered and bombarded by magnetron sputtering, and the rare earth element cerium is deposited by co-sputtering. The sputtering target material is a high-purity metal rare earth target material and a tungsten target material; the deposition temperature is 300°C, the flow rates of argon and oxygen are 30ccm and 10ccm respectively, the deposition time is 10 minutes, and the power is 100 watts. An amorphous tungsten oxide film uniformly doped with the rare earth element cerium is obtained as a storage layer of the simulated memristor, and the thickness of the amorphous tungsten oxide film doped with the rare earth element cerium is 50 nanometers.

[0099] 3) Physical vapor deposition is used to deposit a 300-nanometer-thick Au conductive film with low electrochemical activity as the top electrode film of the simulated memristor; and a simulated memristor of amorphous tungsten oxide film doped with rare earth elements is obtained.

[0100] Compared with Example 1, the analog memristor prepared in Example 4 uses cerium as the doping element, the bottom electrode and the top electrode are FTO, the substrate temperature is high, and the electrode thickness is large. Although the performance of the constructed analog memristor is high, the thicker electrodes waste energy.

[0101] Example 5

[0102] A method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film, comprising:

[0103] 1) A highly insulating and flat intrinsic silicon wafer is selected as the substrate, and a W conductive film with a thickness of 100 nanometers and low electrochemical activity is deposited by physical vapor deposition as the bottom electrode film of the analog memristor.

[0104] 2) The target material is sputtered and bombarded by magnetron sputtering, and the rare earth element praseodymium is deposited by co-sputtering. The sputtering target material is a high-purity metal rare earth target material and a tungsten target material; the deposition temperature is 250°C, the flow rates of argon and oxygen are 10ccm and 5ccm respectively, the deposition time is 5 minutes, and the power is 50 watts. An amorphous tungsten oxide film uniformly doped with rare earth element praseodymium is obtained as the storage layer of the simulated memristor, and the thickness of the amorphous tungsten oxide film doped with rare earth element praseodymium is 20 nanometers.

[0105] 3) A Pt conductive film with a thickness of 100 nanometers and low electrochemical activity is deposited by physical vapor deposition as a top electrode film of the simulated memristor; and a simulated memristor of amorphous tungsten oxide film doped with rare earth elements is obtained.

[0106] Compared with Example 1, the analog memristor prepared in Example 5 uses praseodymium as the doping element, the bottom electrode is W, and the top electrode is Pt. At the same time, the oxygen and argon gas flow rates are small, the film deposition time and power are small, the thickness of the prepared film is small, and the stability of the constructed analog memristor needs to be improved.

[0107] Example 6

[0108] A method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film, comprising:

[0109] 1) A highly insulating and flat intrinsic silicon wafer is selected as the substrate, and a TiN conductive film with a thickness of 100 nanometers and low electrochemical activity is deposited by physical vapor deposition as the bottom electrode film of the analog memristor.

[0110] 2) The target material is sputtered and bombarded by magnetron sputtering, and the rare earth element neodymium is deposited by co-sputtering. The sputtering target material is a high-purity metal rare earth target material and a tungsten target material; the deposition temperature is 250°C, the flow rates of argon and oxygen are 40ccm and 20ccm respectively, the deposition time is 25 minutes, and the power is 200 watts. An amorphous tungsten oxide film uniformly doped with the rare earth element neodymium is obtained as the storage layer of the simulated memristor, and the thickness of the amorphous tungsten oxide film doped with the rare earth element neodymium is 200 nanometers.

[0111] 3) A TiN conductive film with a thickness of 100 nanometers and low electrochemical activity is deposited by physical vapor deposition as a top electrode film of the analog memristor; and an analog memristor of amorphous tungsten oxide film doped with rare earth elements is obtained.

[0112] Compared with Example 1, the analog memristor prepared in Example 6 uses neodymium as the doping element, and the bottom and top electrodes are TiN. At the same time, the oxygen and argon gas flow rates are large, and the film deposition time and power are large. Although the prepared analog memristor has good analog resistive switching performance, its cycle stability needs to be improved.

[0113] Example 7

[0114] A method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film, comprising:

[0115] 1) A highly insulating and flat intrinsic silicon wafer is selected as the substrate, and a Pt conductive film with a thickness of 100 nanometers and low electrochemical activity is deposited by physical vapor deposition as the bottom electrode film of the analog memristor.

[0116] 2) The target material is sputtered and bombarded by magnetron sputtering, and the rare earth element erbium is deposited by co-sputtering. The sputtering target material is a high-purity metal rare earth target material and a tungsten target material; the deposition temperature is 250°C, the flow rates of argon and oxygen are 30ccm and 10ccm respectively, the deposition time is 10 minutes, and the power is 100 watts. An amorphous tungsten oxide film uniformly doped with the rare earth element erbium is obtained as the storage layer of the simulated memristor, and the thickness of the amorphous tungsten oxide film doped with the rare earth element erbium is 50 nanometers.

[0117] 3) A Pt conductive film with a thickness of 100 nanometers and low electrochemical activity is deposited by physical vapor deposition as a top electrode film of the simulated memristor; and a simulated memristor of amorphous tungsten oxide film doped with rare earth elements is obtained.

[0118] The analog memristor prepared in Example 7 uses rare earth erbium as a doping element and a top electrode of Pt. The switching voltage of the resistive switching performance of the prepared device is larger than that of the device in Example 1, resulting in increased power consumption of the device.

[0119] In summary, the analog memristor of a rare earth element doped amorphous tungsten oxide thin film according to the present invention has the following characteristics:

[0120] 1) Amorphous tungsten oxide is an ideal storage material for the resistive switching layer of a memristor due to its excellent electrical and physical properties. Although it has significant advantages in realizing digital memristors, it has problems in analog resistive switching performance. The present invention realizes a device with excellent analog resistive switching performance by doping amorphous tungsten oxide with rare earth elements.

[0121] 2) The method for preparing an analog memristor of a rare earth element-doped amorphous tungsten oxide film proposed in the present invention has the advantages of low cost and compatibility of the preparation process with the COMS process, which is conducive to large-scale production and has excellent application prospects in market fields such as in-memory computing.

[0122] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film, characterized in that: include: First, a conductive film is deposited on a substrate as a bottom electrode film of an analog memristor; Then, a rare earth element doped amorphous tungsten oxide film is deposited on the bottom electrode film as a storage layer of the simulated memristor; finally, a conductive film is deposited on the storage layer as a top electrode film of the simulated memristor; and a simulated memristor of amorphous tungsten oxide film doped with rare earth elements is obtained.

2. The method for preparing the analog memristor of rare earth element doped amorphous tungsten oxide thin film according to claim 1, characterized in that: The conductive film is deposited on the substrate by physical vapor deposition.

3. The method for preparing the analog memristor of rare earth element doped amorphous tungsten oxide thin film according to claim 1, characterized in that: The substrate is highly insulating and flat glass or an intrinsic silicon wafer.

4. The method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film according to claim 1, characterized in that: The conductive film is any one of ITO, FTO, Au, Pt, W and TiN with low electrochemical activity.

5. The method for preparing the analog memristor of rare earth element doped amorphous tungsten oxide thin film according to claim 1, characterized in that: The thickness of the conductive film is 60-300 nanometers.

6. The method for preparing the analog memristor of rare earth element doped amorphous tungsten oxide thin film according to claim 1, characterized in that: The target material is sputtered or laser-bombarded by physical vapor deposition, magnetron sputtering or laser deposition, so that the rare earth element is uniformly doped in the amorphous tungsten oxide film to obtain the rare earth element-doped amorphous tungsten oxide film.

7. The method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film according to claim 1, characterized in that: By co-sputtering or laser bombarding a tungsten-based target and a rare earth element target, the rare earth element is uniformly doped in the amorphous tungsten oxide film to obtain a rare earth element-doped amorphous tungsten oxide film.

8. The method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film according to claim 1, characterized in that: In the rare earth element doped amorphous tungsten oxide film, the doped rare earth element is any one of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium and erbium; the thickness of the rare earth element doped amorphous tungsten oxide film is 20-200 nanometers.

9. The method for preparing an analog memristor of a rare earth element doped amorphous tungsten oxide thin film according to claim 1, characterized in that: The conditions for depositing amorphous tungsten oxide film doped with rare earth elements on the bottom electrode film are: deposition at 50-300°C for 5-25 minutes in an argon and oxygen atmosphere; the argon flow rate is 10-40sccm; the oxygen flow rate is 5-20sccm; and the deposition power is 50-200 watts.

10. An analog memristor of a rare earth element doped amorphous tungsten oxide film, characterized in that: The method is prepared by any one of claims 1 to 9, and comprises, from bottom to top, a bottom electrode, an amorphous tungsten oxide film uniformly doped with rare earth elements, and a top electrode.

Citation Information

Cited By

  • Memristor based on molybdenum-doped vanadium dioxide phase change thin film material and preparation method thereof

    CN119562756A

  • Amorphous tungsten oxide film simulation type resistance change memristor and preparation method and application thereof

    CN119789774A