Composition, preparation method and application of composition in battery slurry

By using silver powder, glass powder and organic carrier compositions in TOPCon batteries, adjusting the glass powder formula and adding inorganic additives, the problem of high porosity caused by low silver content is solved, the battery's acid and water resistance is improved, and the economy is achieved Take into account both benefits and good performance.

CN119092176APending Publication Date: 2024-12-06ZHEJIANG GUANGDA ELECTRONICS TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411179657.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

After reducing the silver content, existing TOPCon batteries are difficult to take into account both economic benefits and good battery performance, especially under sintering conditions, which lead to hidden dangers such as high porosity, water resistance, welding resistance and acid resistance.

Method used

A composition is adopted, including silver powder, glass powder and an organic carrier. The glass powder is composed of a network forming body and a network modification body. The network forming body is selected from metal oxides such as Te, Pb, Bi, Si, etc., and the network modification body is an alkali metal. The second system glass powder contains Ti, Zr, W, and the glass transition temperature is between 450°C and 600°C. By adjusting the glass powder formula and adding inorganic additives, the sintering and adhesion properties of the silver powder are improved.

Benefits of technology

It effectively reduces the excessive pore problems caused by low silver content, improves the acid and water resistance of the battery, ensures the economic benefits and good performance of the battery, and meets the reliability requirements of battery preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092176A_ABST
    Figure CN119092176A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of solar cells, and particularly relates to a composition, a preparation method and application of the composition in battery slurry. The invention provides a composition. The composition comprises silver powder, glass powder and an organic carrier, the glass powder comprises first system glass powder and second system glass powder, and the first system glass powder is composed of a network former and a network modifier; the second system glass powder contains any one or more of Ti, Zr and W. The invention also provides a preparation method of the composition. The invention also provides application of the composition or a product obtained by the preparation method in battery slurry. In the application, the problem of excessive pores caused by low silver content is improved through formula design of the glass powder and adjustment of the use amount of the glass powder, and further experimental determination shows that the prepared composition has good electrical properties, good acid and water resistance and improved welding resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of solar cells, and in particular relates to a composition, a preparation method and an application thereof in a battery slurry. Background Art

[0002] TOPCon (Tunnel Oxide Passivated Contact) battery is a type of passivated contact battery. Its core feature is to prepare an ultra-thin layer of silicon oxide on the back of the battery, and then deposit a thin layer of doped silicon. The two together form a passivated contact structure. This structure uses the quantum tunneling effect to allow majority carriers to tunnel while blocking minority carriers from penetrating, effectively reducing surface recombination and metal contact recombination, thereby improving the conversion efficiency of the battery.

[0003] In order to make the TOPCon cell have better efficiency, the front slurry and the back slurry need to be sintered under the sintering conditions that achieve the best minority carrier lifetime of the TOPCon cell. In the sintering process, silver powder has an important impact on the slurry and the cost of the single cell. In order to reasonably control the cost and ensure the reliability of the battery, reducing the silver content is a conventional consideration for reducing costs and increasing efficiency. However, if the silver content is directly reduced, after sintering, it is difficult for the grid lines to form a dense whole. The excessively high porosity poses a considerable risk to the water resistance, solder resistance, acid resistance, peeling resistance and long-term reliability of the cell. In addition, during the welding process of photovoltaic modules, the excessively high porosity of the fine grid lines will cause the welding resistance of the fine grid lines to deteriorate, resulting in EL failure defects at the corresponding fine grid lines after string welding.

[0004] Therefore, developing a composition, a preparation method and its application in battery slurry to solve the technical defects in the prior art that it is difficult to balance the economic benefits of battery preparation and good battery performance has become an urgent problem to be solved by those skilled in the art. Summary of the invention

[0005] Based on this, it is necessary to provide a composition, a preparation method and its application in battery slurry to address the technical defects in existing technologies that make it difficult to balance the economic benefits of battery preparation and good battery performance.

[0006] The present application provides a composition, the raw materials of the composition comprising: silver powder, glass powder and an organic carrier;

[0007] The glass powder includes a first system glass powder and a second system glass powder, the first system glass powder is composed of a network former and a network modifier, the network former is selected from metal oxides containing any one or more of Te, Pb, Bi, Si and Zn, and the network modifier is an alkali metal oxide and / or an alkaline earth metal oxide; the second system glass powder contains any one or more of Ti, Zr and W, and the glass transition temperature Tg of the second system glass powder is between 450°C and 600°C.

[0008] In one of the embodiments, in terms of mass percentage, for every 100% of the glass powder, the glass powder includes: 55% to 90% of the first system glass powder and 10% to 45% of the second system glass powder.

[0009] In one embodiment, the raw materials of the composition include: 65-85 parts of silver powder, 3-15 parts of glass powder and 11-25 parts of organic carrier.

[0010] In one embodiment, the raw materials of the composition also include: inorganic additives.

[0011] In one embodiment, the raw materials of the composition include: 65-85 parts of silver powder, 3-15 parts of glass powder, 11-25 parts of organic carrier and 1-10 parts of inorganic additive.

[0012] In one embodiment, the inorganic auxiliary agent is a submicron powder, the D50 of the inorganic auxiliary agent is 50nm-1000nm, and the inorganic auxiliary agent is selected from any one or more of aluminum oxide, titanium oxide, silicon oxide, silicon nitride and zirconium oxide.

[0013] The present application also provides a method for preparing the composition comprising any one of the above, the preparation method comprising:

[0014] Step 1, preparing an organic carrier: butyl carbitol, butyl carbitol acetate, diethylene glycol dibutyl ether, tripropylene glycol monomethyl ether and alcohol lipid twelve are mixed for the first time, and then mixed with hydroxyethyl cellulose for the second time, and then polyamide wax is added and mixed for the third time under heating conditions to obtain an organic carrier;

[0015] Step 2, preparing slurry: silver powder and glass powder are pre-mixed, and then mixed with the organic carrier again and stirred. The stirred intermediate product is rolled to disperse and homogenize, and the product is obtained after filtering.

[0016] The present application also provides a method for preparing the composition comprising any one of the above, the preparation method comprising:

[0017] Step 1, preparing an organic carrier: butyl carbitol, butyl carbitol acetate, diethylene glycol dibutyl ether, tripropylene glycol monomethyl ether and alcohol lipid twelve are mixed for the first time, and then mixed with hydroxyethyl cellulose for the second time, and then polyamide wax is added and mixed for the third time under heating conditions to obtain an organic carrier;

[0018] Step 2, mixing the inorganic additive: the organic carrier and the inorganic additive are mixed for the fourth time to obtain an organic-inorganic mixed system;

[0019] Step 3, preparing slurry: After pre-mixing the silver powder and the glass powder, mix them again with the organic-inorganic mixed system and stir, roll the stirred intermediate product to disperse and homogenize it, and obtain the product after filtering.

[0020] The present application also provides an application of the composition described in any one of the above or the product obtained by the preparation method described in any one of the above in battery slurry.

[0021] In summary, the present application provides a composition, including: silver powder, glass powder and organic carrier; the glass powder includes a first system glass powder and a second system glass powder, the first system glass powder is composed of a network former and a network modifier, the network former is selected from any one or more metal oxides containing Te, Pb, Bi, Si and Zn, and the network modifier is an alkali metal oxide and / or an alkaline earth metal oxide; the second system glass powder contains any one or more of Ti, Zr and W, and the glass transition temperature Tg of the second system glass powder is between 450°C and 600°C. The present application also provides a method for preparing the above composition, and the present application also provides an application of the above composition or the product obtained by the above preparation method in battery slurry. In the technical solution provided by the present application, the problem of excessive pores caused by low silver content is improved by adjusting the formula of the glass powder, and further experimental measurements show that the prepared composition has good electrical properties and good acid and water resistance. A composition, a preparation method and its application in battery slurry provided in the embodiment of the present application solve the technical defects in the prior art that it is difficult to take into account both the economic benefits of battery preparation and good battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0023] Figure 1A schematic diagram of a preparation process of a composition preparation method in the technical solution provided in the embodiment of the present application;

[0024] Figure 2 Another schematic diagram of a preparation process of a composition preparation method in the technical solution provided in an embodiment of the present application. DETAILED DESCRIPTION

[0025] The embodiments of the present application provide a composition, a preparation method and application thereof in battery slurry, which are used to solve the technical defects in the prior art that it is difficult to balance the economic benefits of battery preparation and good battery performance.

[0026] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings and examples. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0027] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0028] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0029] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0030] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0031] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.

[0032] The following will be combined Figure 1 and Figure 2 The following examples are provided to further illustrate a composition, a preparation method and an application thereof in battery slurry provided in the present application.

[0033] Example 1

[0034] This embodiment is a specific embodiment of preparing the composition product 1.

[0035] In this embodiment, the raw materials of the product 1 include, by mass percentage, 83% silver powder, 3.6% first system glass powder 1 , 1% second system glass powder 1 , and 12.4% organic vehicle 1 .

[0036] In this embodiment, the first system glass powder 1 is: according to the molecular molar percentage of oxides, the sum of TeO2, PbO, Bi2O3, ZnO, WO3, SiO2, TiO2, Al2O3 and ZrO2 is 10% to 80%; the sum of Na2O, Li2O, K2O, MgO, CaO and BaO is 10-20%, and Tg<350°C; the second system glass powder 1 is: according to the molecular molar percentage of oxides, the sum of PbO, Bi2O3, Li2O, BaO, ZnO and their corresponding halides is 10% to 30%, the sum of TiO2, SiO2, B2O3, Al2O3, ZrO2 and WO3 is 70 to 90%, and Tg≥450°C.

[0037] 1.1 Preparation of organic slurry

[0038] In terms of mass percentage (the total content of the organic carrier is 100%), 10% butyl carbitol, 60% butyl carbitol acetate, 5% diethylene glycol dibutyl ether, 10% tripropylene glycol monomethyl ether and 10% alcohol lipid twelve are weighed and mixed for the first time. After the former is mixed evenly, it is mixed for the second time with 7% hydroxyethyl cellulose, and then 3% polyamide wax is added, heated to 80°C, and mixed for the third time and stirred for 60 minutes, and cooled to room temperature to obtain an organic carrier 1.

[0039] 1.2 Preparation of slurry

[0040] After the silver powder and the glass powder 1 are pre-mixed, the mixed system is added to the organic carrier 1, mixed with the organic carrier 1 again and stirred for 120 minutes. The stirred intermediate product is rolled on a three-roll mill for 6 times to further disperse and homogenize. When the scraper fineness is less than 5 μm, it is filtered with a 400-mesh filter cloth to obtain product 1.

[0041] Example 2

[0042] This embodiment is a specific embodiment of preparing the composite product 2.

[0043] In this embodiment, the raw materials of the product 2 include, by mass percentage, 81% silver powder, 3.6% first system glass powder 2, 1% second system glass powder 2, 12.4% organic vehicle 2 and 2% inorganic auxiliary agent 2.

[0044] In this embodiment, the first system glass powder 2 is: according to the molecular molar percentage of oxides, the sum of TeO2, PbO, Bi2O3, ZnO, WO3, SiO2, TiO2, Al2O3 and ZrO2 is 10% to 80%; the sum of Na2O, Li2O, K2O, MgO, CaO and BaO is 10-20%, Tg<350°C; the second system glass powder 2 is: according to the molecular molar percentage of oxides, the sum of PbO, Bi2O3, Li2O, BaO, ZnO and their corresponding halides is 10% to 30%, the sum of TiO2, SiO2, B2O3, Al2O3, ZrO2 and WO3 is 70-90%, Tg≥450°C. The inorganic additive 2 is a submicron inorganic additive, specifically a titanium dioxide powder of 100-1.2um.

[0045] 2.1 Preparation of organic slurry

[0046] In terms of mass percentage (the total content of the organic carrier is 100%), 10% butyl carbitol, 60% butyl carbitol acetate, 5% diethylene glycol dibutyl ether, 10% tripropylene glycol monomethyl ether and 10% alcohol lipid twelve are weighed and mixed for the first time. After the former is mixed evenly, it is mixed for the second time with 7% hydroxyethyl cellulose, and then 3% polyamide wax is added, heated to 80°C, and mixed for the third time and stirred for 60 minutes, and cooled to room temperature to obtain an organic carrier 2.

[0047] 2.2 Mixed Inorganic Additives

[0048] The organic carrier 2 and the inorganic auxiliary agent 2 are mixed for the fourth time, and after being mixed evenly, an organic-inorganic mixed system 2 is obtained.

[0049] 2.3 Preparation of slurry

[0050] After the silver powder and the glass powder 2 are pre-mixed, the mixed system is added to the organic-inorganic mixed system 2, mixed again and stirred for 120 minutes, and the stirred intermediate product is rolled on a three-roll mill for 6 times to further disperse and homogenize. When the scraper fineness is less than 5μm, it is filtered with a 400-mesh filter cloth to obtain product 2.

[0051] Example 3

[0052] This embodiment is a specific embodiment of preparing composition product 3.

[0053] In this embodiment, the raw materials of the product 3 include, by mass percentage, 79% silver powder, 4.4% first system glass powder 3, 2% second system glass powder 3, 11.6% organic carrier 3 and 1% inorganic auxiliary agent 3.

[0054] In this embodiment, the first system glass powder 3 is: according to the molecular molar percentage of the oxides, the sum of TeO2, PbO, Bi2O3, ZnO, WO3, SiO2, TiO2, Al2O3 and ZrO2 is 10% to 80%; the sum of Na2O, Li2O, K2O, MgO, CaO and BaO is 10-20%, and Tg<350°C; the second system glass powder 3 is: according to the molecular molar percentage of the oxides, the sum of PbO, Bi2O3, Li2O, BaO, ZnO and their corresponding halides is 10% to 30%, the sum of TiO2, SiO2, B2O3, Al2O3, ZrO2 and WO3 is 70 to 90%, and Tg≥450°C. The inorganic additive is a submicron powder, and the D50 of the inorganic additive is 50nm-1000nm. The inorganic additive is a submicron spherical inorganic additive, specifically, an alumina powder of 50-500nm.

[0055] 3.1 Preparation of organic slurry

[0056] In terms of mass percentage (the total content of the organic carrier is 100%), 10% butyl carbitol, 60% butyl carbitol acetate, 5% diethylene glycol dibutyl ether, 10% tripropylene glycol monomethyl ether and 10% alcohol lipid twelve are weighed and mixed for the first time. After the former is mixed evenly, it is mixed with 7% hydroxyethyl cellulose for the second time, and then 3% polyamide wax is added, heated to 80°C, and mixed for the third time and stirred for 60 minutes, and cooled to room temperature to obtain organic carrier 3.

[0057] 3.2 Mixed Inorganic Additives

[0058] The organic carrier 3 and the inorganic auxiliary agent 3 are mixed for the fourth time, and after being mixed evenly, an organic-inorganic mixed system 3 is obtained.

[0059] 3.3 Preparation of slurry

[0060] After the silver powder and the glass powder 3 are pre-mixed, the mixed system is added to the organic-inorganic mixed system 3, mixed again and stirred for 120 minutes, and the stirred intermediate product is rolled on a three-roll mill for 6 times to further disperse and homogenize. When the scraper fineness is less than 5μm, it is filtered with a 400-mesh filter cloth to obtain product 3.

[0061] Example 4

[0062] This embodiment is a specific embodiment of preparing composite product 4.

[0063] In this embodiment, the raw materials of product 4 include, by mass percentage: 79% silver powder, 4.4% first system glass powder 4, 11.6% organic carrier 4 and 5% inorganic additive 4; in this embodiment, the first system glass powder 4 is: by molecular molar percentage of oxides, the sum of TeO2, PbO, Bi2O3, ZnO, WO3, SiO2, TiO2, Al2O3 and ZrO2 is 10% to 80%; the sum of Na2O, Li2O, K2O, MgO, CaO and BaO is 10-20%, Tg<350°C. The D50 of the inorganic additive is 50nm to 1000nm, and the inorganic additive 4 is a submicron spherical inorganic additive, specifically 50-500nm alumina powder.

[0064] 4.1 Preparation of organic slurry

[0065] In terms of mass percentage (the total content of the organic carrier is 100%), 10% butyl carbitol, 60% butyl carbitol acetate, 5% diethylene glycol dibutyl ether, 10% tripropylene glycol monomethyl ether and 10% alcohol lipid twelve are weighed and mixed for the first time. After the former is mixed evenly, it is mixed with 7% hydroxyethyl cellulose for the second time, and then 3% polyamide wax is added, heated to 80°C, and mixed for the third time and stirred for 60 minutes, and cooled to room temperature to obtain organic carrier 4.

[0066] 4.2 Mixed Inorganic Additives

[0067] The organic carrier and the inorganic auxiliary agent are mixed for the fourth time, and after being mixed evenly, an organic-inorganic mixed system 4 is obtained.

[0068] 4.3 Preparation of slurry

[0069] After the silver powder and the glass powder 4 are pre-mixed, the mixed system is added to the organic-inorganic mixed system 4, mixed again and stirred for 120 minutes, and the stirred intermediate product is rolled on a three-roll mill for 6 times to further disperse and homogenize. When the scraper fineness is less than 5μm, it is filtered with a 400-mesh filter cloth to obtain product 4.

[0070] Example 5

[0071] This embodiment is a specific embodiment of preparing the composite product 5.

[0072] In this embodiment, the raw materials of the product 5 include, by mass percentage, 77% silver powder, 6.3% first system glass powder 5, 4.1% second system glass powder 5, 11.6% organic carrier 5 and 1% inorganic additive 5; in this embodiment, the first system glass powder 5 is: by molecular molar percentage of oxides, the sum of TeO2, PbO, Bi2O3, ZnO, WO3, SiO2, TiO2, Al2O3 and ZrO2 is between 10% and 80%. 0%; the sum of Na2O, Li2O, K2O, MgO, CaO and BaO is 10-20%, Tg<350℃; the second system glass powder 5 is: the sum of PbO, Bi2O3, Li2O, BaO, ZnO and their corresponding halides is 10% to 30% according to the molecular molar percentage of the oxides, the sum of TiO2, SiO2, B2O3, Al2O3, ZrO2 and WO3 is 70-90%, Tg≥450℃. The inorganic additive is a submicron powder, the D50 of the inorganic additive is 50nm to 1000nm, and the inorganic additive 5 is a submicron spherical inorganic additive, specifically a 50-500nm silica powder.

[0073] 5.1 Preparation of organic slurry

[0074] In terms of mass percentage (the total content of the organic carrier is 100%), 10% butyl carbitol, 60% butyl carbitol acetate, 5% diethylene glycol dibutyl ether, 10% tripropylene glycol monomethyl ether and 10% alcohol lipid twelve are weighed and mixed for the first time. After the former is mixed evenly, it is mixed with 7% hydroxyethyl cellulose for the second time, and then 3% polyamide wax is added, heated to 80°C, and mixed for the third time and stirred for 60 minutes, and cooled to room temperature to obtain an organic carrier 5.

[0075] 5.2 Mixed Inorganic Additives

[0076] The organic carrier and the inorganic auxiliary agent are mixed for the fourth time, and after being mixed evenly, an organic-inorganic mixed system 5 is obtained.

[0077] 5.3 Preparation of slurry

[0078] After the silver powder and the glass powder 5 are pre-mixed, the mixed system is added to the organic-inorganic mixed system 5, mixed again and stirred for 120 minutes, and the stirred intermediate product is rolled on a three-roll mill for 6 times to further disperse and homogenize. When the scraper fineness is less than 5μm, it is filtered with a 400-mesh filter cloth to obtain product 5.

[0079] Comparative Example 1

[0080] Calculated by mass percentage, the composition includes: 85% silver powder, 2.6% glass material and 12.4% organic carrier.

[0081] In this comparative example, the preparation method comprises the following steps:

[0082] Step 1: Preparation of organic carrier:

[0083] 10% of butyl carbitol, 60% of butyl carbitol acetate, 5% of diethylene glycol dibutyl ether, 5% of tripropylene glycol monomethyl ether, and 10% of alcohol lipid dodecahydrate are weighed by mass percentage and mixed evenly to obtain a mixed solvent, 7% of ethyl cellulose is weighed and added to the mixed solvent, and then 3% of polyamide wax thixotropic agent is added, and then heated to 80° C. while stirring. After the resin is completely dissolved, stirring is continued for 60 minutes, and then cooled to room temperature to obtain an organic carrier.

[0084] Step 2: Prepare electrode slurry:

[0085] Silver powder, glass material and organic carrier are premixed, then added into the organic carrier and stirred for 2 hours, and then the stirred raw materials are rolled 6 times on a three-roll mill to further disperse and homogenize. When the scraper fineness is less than 5 μm, filter with a 400-mesh filter cloth to obtain a reference product.

[0086] The products 1 to 5 prepared in Examples 1 to 5 and the reference product prepared in the comparative example were subjected to relevant tests on battery performance. Please refer to Table 1 for the obtained test results.

[0087] Table 1

[0088]

[0089] In Table 1, Eta is the solar cell conversion efficiency, Voc is the open circuit voltage, Isc is the short circuit current, FF is the fill factor, Rs is the equivalent series resistance, and Rsh is the equivalent parallel resistance.

[0090] It can be concluded from Table 1 that, compared with the reference product prepared in the comparative example, the product prepared by the technical solution provided in the embodiment of the present application has good battery-related parameters and can meet actual practical needs.

[0091] In the technical solution provided by the present application, first, by adjusting the formula of the glass powder, the high Tg glass can improve the wetting and bonding of other components with the silver powder particles. At the same time, the ZrO2, WO3, and TiO2 in the glass powder have good water and acid resistance, thereby further strengthening the reliability risks caused by the reduction of silver content and the reduction of printing deposition weight. The glass powder will soften and liquefy during the sintering process, which will promote the sintering of the silver powder on the one hand, and at the same time, compared with organic additives, it will not produce a large volume of gas to make the structure loose, solving the problem of excessive pores caused by low silver content.

[0092] Second, the use of inorganic powder as an inorganic additive can play a placeholder role in replacing the organic components. After drying and sintering, the inorganic additive will not volatilize like the organic carrier to produce excessive pores.

[0093] In summary, the present application provides a composition, including: silver powder, glass powder and organic carrier; the glass powder includes a first system glass powder and a second system glass powder, the first system glass powder is composed of a network former and a network modifier, the network former is selected from any one or more metal oxides containing Te, Pb, Bi, Si and Zn, and the network modifier is an alkali metal oxide and / or an alkaline earth metal oxide; the second system glass powder contains any one or more of Ti, Zr and W, and the glass transition temperature Tg of the second system glass powder is between 450°C and 600°C. The present application also provides a method for preparing the above composition, and the present application also provides an application of the above composition or the product obtained by the above preparation method in battery slurry. In the technical solution provided by the present application, the problem of excessive pores caused by low silver content is improved by adjusting the formula of the glass powder, and further experimental measurements show that the prepared composition has good electrical properties and good acid and water resistance. A composition, a preparation method and its application in battery slurry provided in the embodiment of the present application solve the technical defects in the prior art that it is difficult to take into account both the economic benefits of battery preparation and good battery performance.

[0094] The technical features of the above-mentioned embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. At the same time, other implementation methods can be derived from the above-mentioned embodiments, so that structural and logical replacements and changes can be made without departing from the scope of this disclosure.

[0095] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A composition, It is characterized in that The raw materials of the composition include: silver powder, glass powder and organic carrier; The glass powder includes a first system glass powder and a second system glass powder, the first system glass powder is composed of a network former and a network modifier, the network former is selected from metal oxides containing any one or more of Te, Pb, Bi, Si and Zn, and the network modifier is an alkali metal oxide and / or an alkaline earth metal oxide; the second system glass powder contains any one or more of Ti, Zr and W, and the glass transition temperature Tg of the second system glass powder is between 450°C and 600°C.

2. The composition according to claim 1, It is characterized in that Calculated by mass percentage, every 100% of the glass powder includes 55% to 90% of the first system glass powder and 10% to 45% of the second system glass powder.

3. The composition according to claim 1 or 2, It is characterized in that The raw materials of the composition also include: inorganic auxiliary agent.

4. The composition according to claim 3, It is characterized in that The raw materials of the composition include, by weight, 65 to 85 parts of silver powder, 3 to 15 parts of glass powder, 11 to 25 parts of organic carrier and 0 to 10 parts of inorganic auxiliary agent.

5. The composition according to claim 3 or 4, It is characterized in that The inorganic auxiliary agent is a submicron powder, the D50 of the inorganic auxiliary agent is 50nm-1000nm, and the inorganic auxiliary agent is selected from: any one or more of aluminum oxide, titanium oxide, silicon oxide, silicon nitride and zirconium oxide.

6. A method for preparing the composition according to any one of claims 1, 2 or 4, It is characterized in that The preparation method is: Step 1, preparing an organic carrier: butyl carbitol, butyl carbitol acetate, diethylene glycol dibutyl ether, tripropylene glycol monomethyl ether and alcohol lipid twelve are mixed for the first time, and then mixed with hydroxyethyl cellulose for the second time, and then polyamide wax is added and mixed for the third time under heating conditions to obtain an organic carrier; Step 2, preparing slurry: silver powder and glass powder are pre-mixed, and then mixed with the organic carrier again and stirred. The stirred intermediate product is rolled to disperse and homogenize, and the product is obtained after filtering.

7. A method for preparing the composition according to any one of claims 3 to 5, It is characterized in that The preparation method is: Step 1, preparing an organic carrier: butyl carbitol, butyl carbitol acetate, diethylene glycol dibutyl ether, tripropylene glycol monomethyl ether and alcohol lipid twelve are mixed for the first time, and then mixed with hydroxyethyl cellulose for the second time, and then polyamide wax is added and mixed for the third time under heating conditions to obtain an organic carrier; Step 2, mixing the inorganic additive: the organic carrier and the inorganic additive are mixed for the fourth time to obtain an organic-inorganic mixed system; Step 3, preparing slurry: After pre-mixing the silver powder and the glass powder, mix them again with the organic-inorganic mixed system and stir, roll the stirred intermediate product to disperse and homogenize it, and obtain the product after filtering.

8. Use of the composition according to any one of claims 1 to 5 or the product obtained by the preparation method according to any one of claims 6 or 7 in battery slurry.

Citation Information

Cited By

  • Composition, preparation method therefor and use thereof in battery slurry