Graphene nanobelt-based synaptic transistor with adjustable plasticity and preparation method of graphene nanobelt-based synaptic transistor
By preparing nanowire masks and oxygen plasma etching technology on the graphene surface, the width of graphene nanoribbons is regulated, and the problem of small synaptic plasticity regulation range of graphene-based synaptic devices is solved, achieving wider plasticity regulation and application, and simple and low-cost process.
Patent Information
- Application Number
- CN202411008437.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The range of synaptic plasticity regulation of graphene-based artificial synaptic devices is limited by their zero band gap properties, which limits their application in neuromorphic calculations.
By introducing digital controlled nanoprinting technology to prepare nanowire masks on the graphene surface, and using oxygen plasma etching technology to prepare graphene nanobands with adjustable widths, regulating the band gap of graphene, and achieving effective regulation of synaptic plasticity .
The plasticity regulation range of graphene nanoband-based artificial synaptic devices has been expanded, overcome the inherent limitations of graphene zero band gap, and promotes its application in the field of neuromorphic electronics. It has low cost and simple technology, which is suitable for large-scale preparation.
Smart Images

Figure CN118946254A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor devices, and in particular relates to a graphene nanoribbon-based synaptic transistor with adjustable plasticity and a preparation method thereof. Background Art
[0002] Led by computer and information technology, a new generation of digital technologies such as the Internet of Things, cloud computing, big data, and artificial intelligence have rapidly emerged and become a powerful driving force for modernization. At the same time, the massive amount of data generated every day in the era of big data has put forward higher requirements on the data processing capabilities of computers. However, in traditional computers based on the von Neumann architecture, the storage unit and the computing unit are separated from each other. When processing information, a large amount of data needs to be transferred between the central processing unit and the storage unit, which greatly limits the data processing speed. The human brain contains about 10 11 Neurons are interconnected to form a highly interconnected neural network, which can store and process large amounts of data in parallel. This has attracted more and more attention to neuromorphic computing that simulates the structure and function of the human brain. Among them, synapses are important structures that connect two neurons, responsible for the storage and transmission of information, and are an important part of biological neural networks. Therefore, artificial synaptic devices that can simulate neural functions such as synaptic plasticity of biological synapses are of great significance to the successful construction of neuromorphic computing systems.
[0003] With the rapid development of materials science, more and more new materials are also used in the construction of artificial synaptic devices, which greatly promotes the related research of artificial synaptic devices. Among them, graphene has attracted widespread attention and research interest worldwide since its first successful preparation. Graphene has excellent electrical properties and is an ideal material for manufacturing electronic components. However, due to the material properties of graphene itself with zero bandgap, when applied to artificial synaptic devices, the switching ratio of the device is relatively low, resulting in a small plasticity adjustment range of artificial synaptic devices, which limits the practical application of graphene-based artificial synaptic devices.
[0004] Among the known technical solutions, Tian et al. described a synaptic device based on a double-layer graphene film in their 2015 study ("Graphene Dynamic Synapse with Modulatable Plasticity", Nano Letters 2015, 15, 8013-8019). The device utilizes the intrinsic properties of graphene and adjusts the carrier density of graphene to achieve the regulation of synaptic plasticity. However, due to the zero bandgap characteristics of graphene, the switching ratio of the device is relatively low, only 1-2. Another related technical solution is patent CN110289317A ("Ferroelectric graphene transistor and complementary synaptic device and regulation method based thereon"). The patent discloses a ferroelectric graphene transistor, which realizes a three-terminal adjustable synaptic transistor by applying a ferroelectric thin film dielectric to the graphene channel. However, although the technology has improved the switching ratio, it still has the inherent problem of being limited by the zero bandgap characteristics of graphene, and the switching ratio is not enough to reach a higher level. Moreover, the synaptic plasticity regulation range of the patent is relatively small, and it is impossible to achieve a wider range of plastic regulation of synaptic devices, which limits its application in neuromorphic computing. Therefore, it is urgent to find a suitable graphene band gap regulation method to improve the plastic regulation range of graphene-based artificial synaptic devices. Summary of the invention
[0005] The purpose of the present invention is to provide a graphene nanoribbon-based synaptic transistor with adjustable plasticity and a method for preparing the same, in order to effectively adjust the plasticity of the device, in view of the fact that the current graphene electronic devices are limited by their zero-bandgap semi-metallic characteristics and the synaptic plasticity adjustment range of the devices is small. The method introduces digitally controllable nano-printing technology to prepare nanowire masks on the graphene surface in a large area, quickly and at low cost, and then prepares graphene nanoribbons with adjustable width by oxygen plasma etching technology. The present invention can effectively regulate the bandgap of graphene, so that it exhibits different electrical properties in applications, overcomes the inherent limitations of graphene zero-bandgap, promotes the practical application of graphene nanoribbons in the field of neuromorphic electronics, enriches the application field of graphene materials, and can obtain graphene nanoribbon-based artificial synaptic devices with a large plasticity adjustment range.
[0006] The technical solution of the present invention is:
[0007] A graphene nanoribbon-based synaptic transistor with adjustable plasticity, wherein the structure of the synaptic transistor comprises a substrate, a semiconductor layer, a source-drain electrode and an ion-glued gate dielectric layer from bottom to top;
[0008] Wherein, the substrate is a silicon wafer (Si / SiO2) substrate with an oxide layer grown thereon;
[0009] The semiconductor is a graphene nanoribbon array with adjustable width; the graphene nanoribbon width ranges from 100 to 800 nm, the thickness ranges from 0.7 to 2.5 nm, the length ranges from 10 to 15 mm, and the spacing between the nanoribbons ranges from 100 to 2000 μm;
[0010] The source and drain electrodes are evaporated gold electrodes with a thickness of 40 to 80 nm;
[0011] The material of the ion glue grid dielectric layer is [PVDF-HFP] [EMIM-TFSI], and the thickness is 100 to 500 μm;
[0012] The method for preparing the graphene nanoribbon-based synaptic transistor with adjustable plasticity comprises the following steps:
[0013] (1) etching the back side of the copper foil with graphene films grown on both sides with oxygen plasma to remove the poor quality graphene on the back side of the copper foil and retain the graphene film on the front side of the copper foil;
[0014] Among them, the oxygen flow rate is 50-80sccm, the RF power is 30-60W, and the etching time is 10-60s;
[0015] (2) spin coating a polymethyl methacrylate (PMMA) solution onto the front surface of the copper foil on which the graphene film is grown, to obtain a graphene / PMMA film attached to the surface of the copper foil;
[0016] The mass solubility of the PMMA solution is 2-10%, the solvent is chlorobenzene, the spin coating speed of the PMMA solution is 3000-5000 r / min, and the spin coating time is 40-60 s;
[0017] (3) etching the copper foil substrate to which the graphene / PMMA film is attached in step (2) by wet etching, i.e., by immersing the copper foil substrate in an ammonium persulfate solution to obtain a polymer-supported graphene / PMMA film;
[0018] The etching time of the copper foil is 2 to 8 hours, and the etching solution is an ammonium persulfate ((NH4)2S2O8) solution with a solubility of 0.1 to 1 mol / L;
[0019] (4) using a clean Si / SiO2 substrate to fish out and dry the graphene / PMMA film obtained in step (4) to obtain a graphene / PMMA film attached to the substrate; then placing it in acetone, a mixed organic solvent, and an isopropanol solution in turn to remove PMMA, thereby obtaining a single-layer graphene film attached to the Si / SiO2 substrate;
[0020] The mixed organic solvent is acetone and isopropanol, and the volume ratio of the two is 1:1;
[0021] (5) using an electrofluidic printing device to print a polyvinyl carbazole (PVK) precursor solution onto the surface of the graphene film obtained in step (4) to form a PVK nanowire mask;
[0022] The mass solubility of the PVK precursor solution is 2% to 10%, and the solvent is styrene; the working voltage is 4000 to 5000 V, and the working distance is 2 to 3 mm. The lateral movement distance of the substrate is set to 160 to 200 mm, the lateral movement speed is 200 to 600 mm / s, the longitudinal movement distance is 0.1 to 0.5 mm, and the speed is 0.6 to 2 mm / s;
[0023] (6) using a mask, evaporating metal electrodes with a thickness of 40 to 80 nm and a spacing of 100 to 200 μm on the surface of the PVK nanowire array obtained in step (5) as source and drain electrodes; wherein the metal is gold, aluminum or silver;
[0024] (7) using oxygen plasma etching technology to etch away the graphene not protected by the nanowire mask, and then removing the nanowire mask by ultrasound to prepare a graphene nanoribbon array;
[0025] (8) The ion glue gate dielectric layer is attached to the graphene nanoribbon array between the source and drain electrodes, and finally a graphene nanoribbon-based synaptic transistor with adjustable plasticity is prepared.
[0026] Also included are the substrate pre-treatment steps:
[0027] Substrate cleaning: The Si / SiO2 substrate was ultrasonically cleaned with deionized water, acetone, and isopropanol for 30 min, and then its surface was blown dry with nitrogen (N2) for later use;
[0028] The PVK nanowire mask described in step (5) is a PVK nanowire array with controllable diameter (100-800 nm) and adjustable spacing (50-300 μm).
[0029] During the oxygen plasma etching process described in step (7), the oxygen flow rate is 30 to 100 sccm, the etching power is 20 to 80 W, and the etching time is 5 to 60 s.
[0030] The preparation method of the ionic glue grid dielectric layer described in step (8) is as follows: [PVDF-HFP][EMIM-TFSI] ionic liquid and acetone are mixed and stirred in a mass ratio of 1:3 to 5:7, and after the mixed solution is fully dissolved, it is drop-coated on a clean glass slide, and after drying, an ionic glue film is obtained, and its thickness is 100 to 500 μm.
[0031] The essential features of the present invention are:
[0032] The present invention ensures the large-area, rapid and low-cost preparation of nanowire masks on the graphene surface by introducing digitally controllable nano-printing technology; the diameter of the nanowire mask is adjustable, and further combined with oxygen plasma etching technology, graphene nanoribbons of different widths can be prepared, thereby regulating the band gap width of the graphene nanoribbons; the adjustable graphene nanoribbon band gap ensures that the synaptic transistor device based on the graphene nanoribbon has adjustable synaptic plasticity; by exploring the relationship between the width of the graphene nanoribbon and the plasticity of the synaptic device, it is ensured that a graphene nanoribbon-based artificial synaptic device with a large plasticity adjustment range is obtained.
[0033] The beneficial effects of the invention are:
[0034] (1) The method for preparing graphene nanoribbons provided by the present invention has the advantages of low cost and simple process, compared with traditional graphene nanoribbon preparation processes such as photolithography which require expensive equipment and complicated process flows;
[0035] (2) The present invention achieves controllable preparation of graphene nanoribbon width by regulating the diameter of the nanowire mask, thereby regulating the band gap of the graphene nanoribbon. By using oxygen plasma etching technology combined with high-precision nanoprinting technology, the width of the graphene nanoribbon can be controlled within the range of 100 to 800 nanometers. ;
[0036] (3) The present invention explores the regulatory effect of graphene nanoribbon width on its synaptic plasticity. By optimizing the device performance through the changes in EPSC at different widths corresponding to different voltages, pulse numbers, and different etching times, a graphene nanoribbon-based artificial synaptic device with a large plasticity regulation range is obtained.
[0037] (4) Combined with digitally controllable nanowire printing technology, large-scale preparation of graphene-based nanoribbon synaptic devices can be achieved, which is beneficial to device integration. By optimizing printing parameters, uniform nanowire masks can be prepared on large-area substrates in a short time, thereby greatly improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a schematic diagram of the structure of the graphene nanoribbon-based synaptic transistor with adjustable plasticity according to the present invention.
[0039] Figure 2 This is the pulse amplitude dependent plasticity (SVDP) of the graphene nanoribbon-based synaptic transistor obtained in Example 1. The read voltage is 0.2 V, and the gate voltage ranges from -5 to 5 V (each increase is 0.5 V).
[0040] Figure 3is the excitatory postsynaptic current (EPSC) of the graphene nanoribbon-based synaptic transistor obtained in Example 1. The pulse amplitude is 4V and the read voltage is 0.2V.
[0041] Figure 4 This is the pulse number dependent plasticity (SNDP) of the graphene nanoribbon-based synaptic transistor obtained in Example 1. The pulse numbers are 5, 10, 20, 30, 50, and 100, respectively, the pulse amplitude is 4V, and the read voltage is 0.2V.
[0042] Figure 5 The comparison of the excitatory postsynaptic current gain of the graphene nanoribbon-based synaptic transistor under different etching time conditions obtained in Example 2. The etching time is 10s, 20s, and 30s, respectively, the test applied pulse amplitude is 4V, and the reading voltage is 0.2V. DETAILED DESCRIPTION
[0043] The present invention is described below in conjunction with examples, but the present invention is not limited to the scope of the examples.
[0044] The structure of the graphene nanoribbon-based synaptic transistor with adjustable plasticity of the present invention is shown in FIG. Figure 1 As shown, from bottom to top, they are Si / SiO2 substrate, graphene nanoribbon, the two ends of the graphene nanoribbon are source and drain gold electrodes, and the source and drain electrodes are covered with [PVDF-HFP][EMIM-TFSI] ion glue gate dielectric layer;
[0045] Embodiment 1:
[0046] (1) 2×2cm 2 The Si / SiO2 substrate (with an oxide layer thickness of 300 nm) was ultrasonically cleaned with deionized water, acetone, and isopropanol for 30 min, respectively, and then its surface was blown dry with N2;
[0047] (2) Cut the copper foil with 0.35 nm graphene film grown on both sides into small pieces of 1.5×1.5 cm, and perform oxygen plasma etching on the back side thereof, wherein the oxygen flow rate is 50 sccm, the radio frequency power is 30 W, and the etching time is 50 s, to remove the poor quality graphene film grown on the back side of the copper foil, and retain the graphene film on the front side of the copper foil;
[0048] (3) dissolving PMMA in chlorobenzene to prepare a PMMA solution with a mass concentration of 3%;
[0049] (4) spin coating the PMMA solution onto the graphene film surface on the front side of the copper foil (spin coating speed 3000 r / min, time 60 s) to obtain a graphene / PMMA film attached to the surface of the copper foil;
[0050] (5) dissolving (NH4)2S2O8 powder in deionized water to prepare an etching solution with a concentration of 0.3 mol / L, immersing the copper foil substrate to which the graphene / PMMA film is attached in the solution and etching for 4 h, obtaining a polymer-supported graphene / PMMA film floating on the surface of the solution, and then transferring it to deionized water for rinsing;
[0051] (6) using a clean Si / SiO2 substrate to fish out and dry the graphene / PMMA film to obtain a graphene / PMMA film attached to the substrate, and then placing it in acetone, acetone:isopropanol = 1:1, and isopropanol solution in turn to remove PMMA to obtain a graphene film attached to the Si / SiO2 substrate;
[0052] (7) dissolving PVK in styrene to prepare a PVK precursor solution with a mass concentration of 4%;
[0053] (8) Using an electrofluidic printing device (EHD-Jet electrofluidic printing device), the PVK precursor solution is printed onto the surface of the graphene film to form a PVK nanowire mask. The working voltage is 4500V and the working distance is 3mm. The lateral movement distance of the substrate is 180mm, the lateral movement speed is 500mm / s, the longitudinal movement distance is 0.2mm, and the speed is 1mm / s; the diameter of the obtained nanowire is 400nm, the lateral length is 2cm, and the nanowire array spacing is 200μm;
[0054] (9) Using a mask, evaporating gold electrodes with a thickness of 60 nm and a spacing of 100 μm on the surface of the PVK nanowire array as source and drain electrodes;
[0055] (10) using oxygen plasma etching technology to etch away the graphene not protected by the PVK nanowire mask, the power of oxygen plasma etching is 30 W, the oxygen flow rate is 100 sccm, and the etching time is 20 s, and then the nanowire mask is removed by ultrasound to prepare a graphene nanoribbon array attached to the surface of the substrate, wherein the thickness of the nanoribbon is 1.5 nm;
[0056] (11) [PVDF-HFP][EMIM-TFSI] ionic liquid and acetone in a mass ratio of 1:4:7 were mixed and stirred on a magnetic stirrer at 50 °C and 600 r / min. After fully dissolved, the mixed solution was drop-coated on a clean glass slide and dried to obtain a 300 μm thick ionic gel film;
[0057] (12) attaching an ion glue gate dielectric layer to the graphene nanoribbon array between the source and drain electrodes to prepare a graphene nanoribbon-based synaptic transistor device;
[0058] (13) The electrical performance of the synaptic transistor is analyzed using a semiconductor test analyzer, and the simulation of biological synaptic plasticity is achieved by adjusting the input pulse signal.
[0059] Figure 1 The schematic diagram of the structure of the graphene nanoribbon-based synaptic transistor with adjustable plasticity of the present invention is shown. The tungsten probe is used as the gate to simulate the presynaptic membrane, the anions and cations in the ion-glued gate dielectric layer simulate the neurotransmitters stored in the synaptic vesicles, and the graphene nanoribbon simulates the postsynaptic membrane. The electrical performance of the synaptic transistor device was tested using a Keithley 4200A semiconductor analyzer. Figure 2 is the SVDP of the graphene nanoribbon-based synaptic transistor obtained in Example 1. The reading voltage is 0.2 V, and the gate voltage scanning range is -5 to 5 V. When the gate voltage reaches a certain positive or negative amplitude, the synaptic transistor can be induced to generate an excitatory postsynaptic current, and as the amplitude increases, the EPSC gradually increases. Figure 3 The EPSC of the graphene nanoribbon-based synaptic transistor obtained in Example 1 under the conditions of a pulse amplitude of 4 V and a reading voltage of 0.2 V. By calculation, the postsynaptic current gain (ΔEPSC) is 65 μA, and the current value is still higher than the initial value after the pulse stimulation is removed for 10 seconds, indicating that the device has a certain memory ability and realizes the simulation of synaptic learning and memory ability. Figure 4 The SNDP of the graphene nanoribbon-based synaptic transistor obtained in Example 1 when the amplitude of multiple consecutive pulses is 4V and the reading voltage is 0.2V, the number of pulses is 5, 10, 20, 30, and 50 respectively. As the number of pulses increases, the EPSC of the device gradually increases. Figure 5 The synaptic plasticity comparison of the graphene nanoribbon-based synaptic transistor prepared by adjusting the etching time in Example 2. Figure 5 Samples 1, 2, and 3 are graphene nanoribbons of different widths prepared under the conditions of etching time of 10s, 20s, and 30s, respectively. Under the condition of a reading voltage of 0.2V, a pulse stimulation with an amplitude of 4V is applied to obtain the ΔEPSC of the graphene nanoribbon-based synaptic device. By comparing the ΔEPSC of the device, it can be found that as the etching time increases, the ΔEPSC value of the device increases. As the etching time further increases, the width of the nanoribbon decreases, the ability to capture particles weakens, and the ΔEPSC value decreases, indicating that the width of the graphene nanoribbon has a regulatory effect on the plasticity of the synaptic device. The above data all illustrate that the graphene nanoribbon-based synaptic device prepared by the present invention can simulate the function of biological synapses, and by adjusting the parameters of the pulse stimulation and the width of the graphene nanoribbon, the synaptic plasticity of the synaptic device can be regulated.
[0060] Embodiment 2:
[0061] (1) 2×2cm2 The Si / SiO2 substrate (with an oxide layer thickness of 300 nm) was ultrasonically cleaned with deionized water, acetone, and isopropanol for 30 min, respectively, and then its surface was blown dry with N2;
[0062] (2) Cut the copper foil with graphene film grown on both sides into 1.5×1.5 cm 2 A small piece of copper foil is taken, and the back side thereof is subjected to oxygen plasma etching, wherein the oxygen flow rate is 50 sccm, the radio frequency power is 50 W, and the etching time is 30 s, so as to remove the poor quality graphene film grown on the back side of the copper foil and retain the graphene film on the front side of the copper foil;
[0063] (3) dissolving PMMA in chlorobenzene to prepare a PMMA solution with a mass concentration of 3%;
[0064] (4) spin coating the PMMA solution onto the graphene film surface on the front side of the copper foil (spin coating speed 3000 r / min, time 60 s) to obtain a graphene / PMMA film attached to the surface of the copper foil;
[0065] (5) Dissolve (NH4)2S2O8 powder in deionized water, prepare an etching solution with a concentration of 0.3 mol / L, immerse the copper foil substrate to which the graphene / PMMA film is attached in the solution and etch for 5 h, so that the polymer-supported graphene / PMMA film floats on the surface of the solution, and then transfer it to deionized water for rinsing;
[0066] (6) using a clean Si / SiO2 substrate to fish out and dry the graphene / PMMA film to obtain a graphene / PMMA film attached to the substrate, and then placing it in acetone, acetone:isopropanol = 1:1, and isopropanol solution in turn to remove PMMA to obtain a graphene film attached to the Si / SiO2 substrate;
[0067] (7) dissolving PVK powder in styrene to prepare a PVK precursor solution with a mass concentration of 4%;
[0068] (8) Using an electrofluidic printing device (EHD-Jet electrofluidic printing device), the PVK precursor solution was printed onto the surface of the graphene film to form a PVK nanowire mask; wherein the working voltage was 4500 V and the working distance was 3 mm. The lateral movement distance of the substrate was 180 mm, the lateral movement speed was 500 mm / s, the longitudinal movement distance was 0.3 mm, and the speed was 1 mm / s; the diameter of the obtained nanowires was 400 nm, the lateral length was 2 cm, and the nanowire array spacing was 300 μm;
[0069] (9) Using a mask, evaporating gold electrodes with a thickness of 60 nm and a spacing of 100 μm on the surface of the PVK nanowire array as source and drain electrodes;
[0070] (10) using oxygen plasma etching technology to etch away the graphene not protected by the PVK nanowire mask, the power of oxygen plasma etching was 30 W, the oxygen flow rate was 100 sccm, and the etching time was 10 s, 20 s, and 30 s, respectively, and then the nanowire mask was removed by ultrasound to prepare three graphene nanoribbon arrays with different widths attached to the substrate surface;
[0071] (11) [PVDF-HFP][EMIM-TFSI] ionic liquid and acetone in a mass ratio of 1:4:7 were mixed and stirred on a magnetic stirrer at 50 °C and 600 r / min. After fully dissolved, the mixed solution was drop-coated on a clean glass slide and dried to obtain a 300 μm thick ionic gel film;
[0072] (12) The ion glue gate dielectric layer is attached to the graphene nanoribbon array between the source and drain electrodes to prepare a graphene nanoribbon-based synaptic transistor device.
[0073] (13) The electrical performance of the synaptic transistor was analyzed using a semiconductor test analyzer. By comparing the electrical performance of graphene nanoribbon-based synaptic transistors prepared at different etching times, the regulatory effect of graphene nanoribbon width on device plasticity was explored.
[0074] Matters not covered by the present invention are known technologies.
Claims
1. A graphene nanoribbon-based synaptic transistor with adjustable plasticity, characterized by The structure of the synaptic transistor is, from bottom to top, a substrate, a semiconductor layer, a source-drain electrode, and an ion-glued gate dielectric layer; Wherein, the substrate is a silicon wafer (Si / SiO2) substrate with an oxide layer grown thereon; The semiconductor is a graphene nanoribbon array with adjustable width; the graphene nanoribbon width ranges from 100 to 800 nm, the thickness ranges from 0.7 to 2.5 nm, the length ranges from 10 to 15 mm, and the spacing between the nanoribbons ranges from 100 to 2000 μm; The source and drain electrodes are evaporated gold electrodes with a thickness of 40 to 80 nm; The material of the ion glue grid dielectric layer is [PVDF-HFP] [EMIM-TFSI], and the thickness is 100-500 μm.
2. The method for preparing a graphene nanoribbon-based synaptic transistor with adjustable plasticity according to claim 1, characterized in that The following steps are involved: (1) etching the back side of the copper foil with graphene films grown on both sides with oxygen plasma to remove the poor quality graphene on the back side of the copper foil and retain the graphene film on the front side of the copper foil; Among them, the oxygen flow rate is 50-80sccm, the RF power is 30-60W, and the etching time is 10-60s; (2) spin coating a polymethyl methacrylate (PMMA) solution onto the front surface of the copper foil on which the graphene film is grown, to obtain a graphene / PMMA film attached to the surface of the copper foil; The mass solubility of the PMMA solution is 2-10%, the solvent is chlorobenzene, the spin coating speed of the PMMA solution is 3000-5000 r / min, and the spin coating time is 40-60 s; (3) immersing the copper foil substrate with the graphene / PMMA film attached thereto into an ammonium persulfate solution for etching to obtain a polymer-supported graphene / PMMA film; The etching time of the copper foil is 2 to 8 hours, and the etching solution is an ammonium persulfate ((NH4)2S2O8) solution with a solubility of 0.1 to 1 mol / L; (4) using a Si / SiO2 substrate to fish out and dry the graphene / PMMA film obtained in step (4) to obtain a graphene / PMMA film attached to the substrate; then placing it in acetone, a mixed organic solvent, and an isopropanol solution in turn to remove PMMA, thereby obtaining a single-layer graphene film attached to the Si / SiO2 substrate; The mixed organic solvent is acetone and isopropanol, and the volume ratio of the two is 1:1; (5) using an electrofluidic printing device to print a polyvinyl carbazole (PVK) precursor solution onto the surface of the graphene film obtained in step (4) to form a PVK nanowire mask; The mass solubility of the PVK precursor solution is 2% to 10%, and the solvent is styrene; the working voltage is 4000 to 5000 V, and the working distance is 2 to 3 mm. The lateral movement distance of the substrate is set to 160 to 200 mm, the lateral movement speed is 200 to 600 mm / s, the longitudinal movement distance is 0.1 to 0.5 mm, and the speed is 0.6 to 2 mm / s; (6) using a mask, evaporating metal electrodes with a thickness of 40 to 80 nm and a spacing of 100 to 200 μm on the surface of the PVK nanowire array obtained in step (5) as source and drain electrodes; wherein the metal is gold, aluminum or silver; (7) using oxygen plasma etching technology to etch away the graphene not protected by the nanowire mask, and then removing the nanowire mask by ultrasound to prepare a graphene nanoribbon array; (8) The ion glue gate dielectric layer is attached to the graphene nanoribbon array between the source and drain electrodes, and finally a graphene nanoribbon-based synaptic transistor with adjustable plasticity is prepared.
3. The method for preparing a graphene nanoribbon-based synaptic transistor with adjustable plasticity according to claim 2, characterized in that the substrate is subjected to a pretreatment step: Substrate cleaning: The Si / SiO2 substrate was ultrasonically cleaned with deionized water, acetone, and isopropanol for 30 min, respectively, and then its surface was blown dry with nitrogen (N2) for standby use.
4. The method for preparing a graphene nanoribbon-based synaptic transistor with adjustable plasticity as claimed in claim 2, characterized in that The PVK nanowire mask described in step (5) is a PVK nanowire array with controllable diameter (100-800 nm) and adjustable spacing (50-300 μm).
5. The method for preparing a graphene nanoribbon-based synaptic transistor with adjustable plasticity as claimed in claim 2, characterized in that During the oxygen plasma etching process described in step (7), the oxygen flow rate is 30 to 100 sccm, the etching power is 20 to 80 W, and the etching time is 5 to 60 s.
6. The method for preparing a graphene nanoribbon-based synaptic transistor with adjustable plasticity as described in claim 2 is characterized by the preparation method of the ionic glue gate dielectric layer described in step (8): [PVDF-HFP][EMIM-TFSI] ionic liquid and acetone in a mass ratio of 1:3 to 5:7 are mixed and stirred, and after sufficient dissolution, the mixed solution is dripped onto a clean glass slide, and after drying, an ionic glue film with a thickness of 100 to 500 μm is obtained.